Organic polymer particle opening master batch as well as preparation method and application thereof

Through premixing of predispersed resin powder and organic microsphere powder and melt blending in a twin-screw extruder, the problems of poor dispersion and agglomeration in the existing technology are solved, and the efficient preparation of polyester functional films is achieved. and performance improvements.

CN118725360AInactive Publication Date: 2024-10-01JIANGSU KANGHUI NEW MATERIALS TECH CO LTD

Patent Information

Application Number
CN202411226880.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When preparing the opening agent masterbatch in the existing technology, the dispersion is poor and the agglomeration phenomenon is serious, which affects the performance and production efficiency of the polyester film, and the cost is high.

Method used

Pre-dispersed resin powder and organic microsphere powder are premixed, and melt-blended through a twin-screw extruder to improve the dispersion effect of organic microsphere powder, reduce agglomeration, and reduce costs.

Benefits of technology

It achieves uniform dispersion of organic polymeric particle open masterbatch, reduces the risk of adhesion of polyester functional films, and improves film performance and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of functional master batches, and relates to an organic polymer particle opening master batch and a preparation method and application thereof.The preparation method of the organic polymer particle opening master batch comprises the steps that pre-dispersed resin powder, organic microsphere powder and auxiliaries are premixed, and premixed powder is obtained; feeding the premixed powder and carrier resin particles into a double-screw extruder from different feeding ports for melt blending to obtain organic polymer particle open master batches; the polyester functional film is prepared from the organic polymer particle open master batch to be prepared and other raw materials through a multi-layer co-extrusion technology. In the preparation process of the organic polymer particle opening master batch, the dispersion effect of the organic microsphere powder is better in the extrusion processing link, a polyester functional film prepared from the organic polymer particle opening master batch can endow better optical performance while efficiently achieving the opening effect, and the organic polymer particle opening master batch is particularly suitable for being used as a high-transmittance and high-gloss BOPET film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional masterbatches and relates to an organic polymer particle open masterbatch and a preparation method and application thereof. Background Art

[0002] During film processing, whether during the winding process or after the film is rolled, the layers of the film are easily stuck due to the pressure, which affects the subsequent use. There are two main reasons for the sticking. First, after the film is rolled, the film layers form a vacuum seal, which is not easy to separate; second, after the film is formed, there are a large number of exposed molecular chains on the surface. After the two films are closed, the macromolecular chains will be entangled with each other, making it impossible to open; in order to make the film production smooth, an opening agent is added during the production of polyester film to prevent the film from sticking.

[0003] Traditional opening agents are non-migrating inorganic minerals, such as diatomaceous earth, talc, kaolin, silicon dioxide, etc. The function of the opening agent is to prevent the adhesion between films, especially for thin films or films with high surface gloss, the opening agent can also play a role in slightly reducing the friction coefficient; its mechanism of action is: the inorganic additives are evenly dispersed in the film, forming many fine and hard protrusions on the surface of the film, affecting the flatness of the film surface, thereby breaking the mirror effect, thereby reducing the contact area between the films, achieving the purpose of reducing the friction coefficient of the film surface, and making the film easy to separate; at the same time, due to the existence of these protrusions, it is easy for external air to enter between the two layers of film, avoiding the formation of a vacuum between the two layers of film bonded together, thereby preventing the film from sticking.

[0004] There are two main methods for preparing antiblocking agent masterbatches in the industry. One is to pre-disperse inorganic silica powder into ethylene glycol solvent during the polymerization of polyester resin, and then add it together with the monomer for polymerization during the polymerization process (the powder does not participate in the polymerization). This preparation method is very helpful for the dispersion of inorganic powders, and has high production capacity for continuous production. However, it is difficult to prepare high concentrations (greater than 3%), and it is easy to produce powder agglomeration during polymerization, which affects subsequent use. This preparation method requires the support of the polymerization production line, with large investment and high cost. Another method is to use physical blending twin-screw extrusion. The processing method is simple and the investment is relatively small. However, if the powder is not handled properly, the poor dispersion of the obtained masterbatch will affect the use of the film end.

[0005] Chinese patent application CN109181242A discloses a masterbatch of opening agent for plastic film and a preparation method thereof. The method is mainly based on the process of physical blending and extrusion. Its core technical innovation lies in modifying inorganic powder (including at least one of silicon dioxide, titanium dioxide, barium sulfate, and calcium carbonate particles) with a compatibilizer to enhance its binding property with the resin matrix. However, although this method performs surface active treatment on the inorganic powder, it does not change the original morphology of the powder. Therefore, during the extrusion process, especially when the amount of powder added is large, the material may not be completely dispersed within a limited time due to the relatively short residence time of the material in the screw, resulting in agglomeration. This means that even for ultra-fine particle size and high concentration powder, the method may still face the problem of uneven dispersion during processing, and then there is a risk of powder agglomeration during use. In addition, the compatibility of inorganic powder with polyester resin will also affect the various properties of the resin body to a certain extent.

[0006] Chinese patent application CN114455597A provides a silicon dioxide opening agent for plastic film and a preparation method thereof, which adopts a reactive preparation method to disperse the powder in a solvent. Although it has certain advantages in terms of dispersibility, its process is complicated and industrial production requires greater investment and manpower.

[0007] Therefore, it is necessary to develop a method for preparing an anti-blocking agent masterbatch to solve the problems existing in the above-mentioned prior art. Summary of the invention

[0008] The purpose of the present invention is to solve the problems existing in the prior art and to provide an organic polymer particle open masterbatch and a preparation method and application thereof.

[0009] To achieve the above object, the scheme adopted by the present invention is as follows:

[0010] A method for preparing an organic polymer particle open masterbatch comprises the following steps: firstly, pre-dispersed resin powder, organic microsphere powder and an auxiliary agent are pre-mixed to obtain a pre-mixed powder, and then the pre-mixed powder and carrier resin particles are fed into a twin-screw extruder from different feeding ports for melt blending to obtain an organic polymer particle open masterbatch; wherein the pre-dispersed resin powder and the carrier resin particles are made of the same material; and the absolute value of the difference in particle size between the pre-dispersed resin powder and the organic microsphere powder does not exceed 500 μm.

[0011] When preparing organic polymer microparticle open masterbatch in the prior art, organic microsphere powder and carrier resin particles are fed into a twin-screw extruder at the same time. The particle size of the organic microsphere powder is micron-level, the powder is very fine, and the resin particles are millimeter-level particles. After the two substances are physically mixed, the bulk density of the carrier resin particles and the organic microsphere powder is significantly different. When falling in the feed scale, affected by the airflow, the carrier resin particles (with larger particle size) will fall first, while the organic microsphere powder is difficult to feed, resulting in abnormal stratification of the two components of the feed, uneven feeding, and difficulty in meeting the requirements of co-blending extrusion.

[0012] The present invention premixes pre-dispersed resin powder, organic microsphere powder and an auxiliary agent to obtain a premixed powder, which can improve the bulk density of the organic microsphere powder on the one hand, and disperse the organic microsphere powder in advance on the other hand. Further mixing by a twin-screw during the extrusion process can make the dispersion effect of the organic microsphere powder better.

[0013] As the preferred technical solution:

[0014] In the method for preparing an organic polymer microparticle open masterbatch as described above, the intrinsic viscosity of the pre-dispersed resin powder and the carrier resin particles are different, and the intrinsic viscosity is greater than 0.6dL / g, and the intrinsic viscosity of the pre-dispersed resin powder is higher than the intrinsic viscosity of the carrier resin particles; because the processing time experienced by the pre-dispersed resin powder is longer than that of the carrier resin particles, the viscosity drop is relatively large, therefore, when adding materials, the present invention controls the intrinsic viscosity of the pre-dispersed resin powder to be higher than the intrinsic viscosity of the carrier resin particles, so that the intrinsic viscosity of the final product can be controlled to reach the designed value.

[0015] The method for preparing an organic polymer microparticle open masterbatch as described above, wherein the organic microsphere powder is a monodisperse polystyrene microsphere (a spherical colloidal particle obtained by polymerizing and cross-linking styrene and a silane derivative), and the bulk density is 0.2-0.4 g / cm 3 , particle size is 2-5μm, refractive index is 1.58-1.60, thermal decomposition temperature is >300℃;

[0016] Pre-dispersed resin powder is a powder obtained by grinding polyethylene terephthalate (PET) particles in a grinding mill. Its intrinsic viscosity is 0.78-0.85dL / g and its bulk density is 0.7-0.9g / cm 3 , particle size is 30-100 mesh, melting point is 252-262℃;

[0017] The carrier resin particles are polyethylene terephthalate particles with an intrinsic viscosity of 0.68-0.80 dL / g and a bulk density of 0.6-0.8 g / cm 3 , particle size is 2-4mm, melting point is 255-265℃.

[0018] The method for preparing the organic polymer microparticle open masterbatch as described above, wherein the premixing temperature is 100-130°C, the time is 5-10 minutes, and the rotation speed is 800-1200 rpm;

[0019] The purpose of high-temperature premixing is to accelerate two powders with similar particle sizes to 1000 rpm through a high-speed mixer, and then add a certain amount of heating to fully mix the pre-dispersed resin powder and the organic microsphere powder, so that the two powders are fully interlocked with each other, so that uniform feeding can be achieved during the feeding process without causing stratification, thereby greatly increasing the content of organic microsphere powder in the final organic polymer microparticle open masterbatch.

[0020] In the method for preparing an organic polymer microparticle open masterbatch as described above, the auxiliary agents are a dispersant and an antioxidant, the dispersant is at least one of ethylene bisstearamide, pentaerythritol stearate, and calcium stearate, and the antioxidant is at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester (commonly known as antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (commonly known as antioxidant 168).

[0021] In the method for preparing an organic polymer microparticle open masterbatch as described above, the added amount of each component is, by weight: 60-80 parts of carrier resin particles, 15-30 parts of pre-dispersed resin powder, 3-15 parts of organic microsphere powder, 0.2-0.5 parts of antioxidant, and 0.2-0.5 parts of dispersant.

[0022] The method for preparing an organic polymer microparticle open masterbatch as described above specifically comprises the following steps: firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder; then, the pre-mixed powder is fed into a twin-screw extruder through a side feed port; and at the same time, carrier resin particles are fed into the twin-screw extruder through a main feed port; and finally, the organic polymer microparticle open masterbatch is obtained through mixing, shearing, dispersing and filtering by twin-screw extrusion.

[0023] The present invention also provides an organic polymer microparticle open masterbatch prepared by the preparation method of an organic polymer microparticle open masterbatch as described in any of the above items, with an FPV value of 0.156-0.305 bar / g. The FPV value of the organic polymer microparticle open masterbatch with the same organic microsphere powder content in the prior art is generally 0.536 bar / g. By comparison, it can be seen that the FPV of the organic polymer microparticle open masterbatch of the present invention is significantly lower than that of the prior art, which indicates that the preparation method of the present invention is more conducive to achieving uniform dispersion of organic microsphere powder.

[0024] The present invention also provides a method for preparing a polyester functional film, which adopts a multi-layer co-extrusion technology, and the raw materials of the surface layer are polyester resin and the organic polymer particle open masterbatch as described above.

[0025] As the preferred technical solution:

[0026] In the method for preparing a polyester functional film as described above, the content of organic microsphere powder in the surface layer is 1000-3000 ppm.

[0027] According to the preparation method of a polyester functional film as described above, under the condition of a production speed of 450-500m / min, the pressure fluctuation of the melt filter does not exceed 1.1, the traction, winding and slitting processes are normal, and no abnormal problems such as film breakage, wrinkles, deviation, die lip line, etc. occur in the production process. Microscopic analysis shows that the organic microsphere powder on the surface of the film is evenly distributed without agglomeration; the physical properties of the film are not significantly different from those of conventional films, and all indicators meet the target values; the thickness of the polyester functional film is 29-31.8μm, the transmittance is 90.1%-90.7%, and the haze is 1.2%. -3.1%, clarity is 98.7%-99.7%, gloss is 128.8-135.2GU, dynamic friction coefficient is 0.328-0.397, static friction coefficient is 0.343-0.382, longitudinal tensile strength at break is 200-235MPa, transverse tensile strength at break is 209-239MPa, longitudinal elongation at break is 102%-187%, transverse elongation at break is 100%-136%, longitudinal elastic modulus is 4857-5653MPa, and transverse elastic modulus is 6215-6656MPa.

[0028] Beneficial effects:

[0029] The present invention provides an organic polymer microparticle opening masterbatch and a preparation method and application thereof. The opening masterbatch is first premixed and then blended to prepare the opening masterbatch, and then the opening masterbatch and the base material resin (carrier resin particles) are fed together to produce a polyester functional film. During or after the polyester functional film is rolled into a roll, adhesion between the films can be effectively prevented, and the film opening effect can be efficiently achieved.

[0030] Compared with the conventional one-step physical blending method, the method for preparing the organic polymer microparticle open masterbatch of the present invention can not only effectively reduce the agglomeration of fine powders, thereby improving the performance of the polyester functional film, but also reduce processing costs and improve production efficiency. DETAILED DESCRIPTION

[0031] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0032] The testing standards of relevant performance indicators in the embodiments and comparative examples are as follows:

[0033]

[0034] Example 1

[0035] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0036] (1) Raw material preparation:

[0037] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.68dL / g, bulk density 0.6g / cm 3 , the average particle size is 2.5 mm, and the melting point is 260°C;

[0038] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed by a mill to form powder with an intrinsic viscosity of 0.78 dL / g and a bulk density of 0.75 g / cm 3 , the average particle size is 50 mesh, and the melting point is 260℃;

[0039] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.2g / cm 3 , average particle size is 3 μm, refractive index is 1.59, thermal decomposition temperature is 305 °C;

[0040] Dispersant: ethylene bisstearamide;

[0041] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionate and pentaerythritol tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1;

[0042] (2) Weighing raw materials:

[0043] By weight, take: 60 parts of carrier resin particles, 30 parts of pre-dispersed resin powder, 10 parts of organic microsphere powder, 0.4 parts of antioxidant, and 0.2 parts of dispersant;

[0044] (3) Preparation of organic polymer microparticle opening masterbatch:

[0045] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 100° C., the time is 8 min, and the speed is 1000 rpm;

[0046] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0047] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0048] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.283 bar / g.

[0049] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 31.6μm.

[0050] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0051] Comparative Example 1

[0052] A method for preparing an organic polymer microparticle open masterbatch is basically the same as the method for preparing an organic polymer microparticle open masterbatch in Example 1, except that: no premixing is performed in step (3), that is, carrier resin particles, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are fed into a twin-screw extruder through a main feed port at the same time, and finally the organic polymer microparticle open masterbatch is obtained by mixing, shearing, dispersing and filtering by twin-screw extrusion.

[0053] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.518 bar / g.

[0054] A method for preparing a polyester functional film is basically the same as the method for preparing a polyester functional film in Example 1, except that the organic polymer microparticle opening masterbatch in the A layer raw material is the organic polymer microparticle opening masterbatch of this comparative example, and the thickness of the final film is 31.6 μm.

[0055] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0056] Example 2

[0057] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0058] (1) Raw material preparation:

[0059] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.8dL / g, bulk density 0.65g / cm 3 , the average particle size is 3mm, the melting point is 258℃;

[0060] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed into powder by a mill, with an intrinsic viscosity of 0.85dL / g and a bulk density of 0.8g / cm 3 , the average particle size is 70 mesh, and the melting point is 255℃;

[0061] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.4g / cm 3 , average particle size is 4 μm, refractive index is 1.59, thermal decomposition temperature is 310 °C;

[0062] Dispersant: pentaerythritol stearate;

[0063] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1;

[0064] (2) Weighing raw materials:

[0065] By weight, take: 65 parts of carrier resin particles, 27 parts of pre-dispersed resin powder, 8 parts of organic microsphere powder, 0.4 parts of antioxidant, and 0.2 parts of dispersant;

[0066] (3) Preparation of organic polymer microparticle opening masterbatch:

[0067] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 110° C., the time is 5 min, and the rotation speed is 800 rpm;

[0068] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0069] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0070] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.249 bar / g.

[0071] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 30.8μm.

[0072] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0073] Example 3

[0074] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0075] (1) Raw material preparation:

[0076] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.7dL / g, bulk density 0.6g / cm 3 , the average particle size is 2.5 mm, and the melting point is 255°C;

[0077] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed into powder by a mill, with an intrinsic viscosity of 0.79dL / g and a bulk density of 0.7g / cm 3 , the average particle size is 80 mesh, and the melting point is 252°C;

[0078] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.3g / cm 3 , average particle size is 2 μm, refractive index is 1.58, thermal decomposition temperature is 315°C;

[0079] Dispersant: ethylene bisstearamide;

[0080] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 3:2;

[0081] (2) Weighing raw materials:

[0082] By weight, take: 70 parts of carrier resin particles, 20 parts of pre-dispersed resin powder, 10 parts of organic microsphere powder, 0.5 parts of antioxidant, and 0.2 parts of dispersant;

[0083] (3) Preparation of organic polymer microparticle opening masterbatch:

[0084] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 120° C., the time is 8 min, and the rotation speed is 1100 rpm;

[0085] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0086] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0087] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.245 bar / g.

[0088] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 29.0μm.

[0089] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0090] Example 4

[0091] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0092] (1) Raw material preparation:

[0093] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.75 dL / g, bulk density 0.8 g / cm 3 , the average particle size is 2.0 mm, and the melting point is 265°C;

[0094] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed by a mill to form powder with an intrinsic viscosity of 0.8 dL / g and a bulk density of 0.9 g / cm 3 , the average particle size is 90 mesh, and the melting point is 262°C;

[0095] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.3g / cm 3 , average particle size is 5 μm, refractive index is 1.6, thermal decomposition temperature is 305 °C;

[0096] Dispersant: pentaerythritol stearate;

[0097] Antioxidant: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate;

[0098] (2) Weighing raw materials:

[0099] By weight, take: 75 parts of carrier resin particles, 22 parts of pre-dispersed resin powder, 3 parts of organic microsphere powder, 0.2 parts of antioxidant, and 0.2 parts of dispersant;

[0100] (3) Preparation of organic polymer microparticle opening masterbatch:

[0101] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 120° C., the time is 6 min, and the speed is 1200 rpm;

[0102] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0103] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0104] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.156 bar / g.

[0105] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 29.8μm.

[0106] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0107] Example 5

[0108] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0109] (1) Raw material preparation:

[0110] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.78 dL / g, bulk density 0.7 g / cm 3 , the average particle size is 4.0 mm, and the melting point is 263°C;

[0111] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed by a mill to form powder with an intrinsic viscosity of 0.82dL / g and a bulk density of 0.85g / cm 3 , the average particle size is 30 mesh, and the melting point is 258°C;

[0112] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.35g / cm 3 , average particle size is 3.5μm, refractive index is 1.58, thermal decomposition temperature is 308℃;

[0113] Dispersant: calcium stearate;

[0114] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1;

[0115] (2) Weighing raw materials:

[0116] By weight, take: 75 parts of carrier resin particles, 20 parts of pre-dispersed resin powder, 5 parts of organic microsphere powder, 0.4 parts of antioxidant, and 0.2 parts of dispersant;

[0117] (3) Preparation of organic polymer microparticle opening masterbatch:

[0118] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 125° C., the time is 7 min, and the speed is 900 rpm;

[0119] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0120] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0121] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.215 bar / g.

[0122] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 31.6μm.

[0123] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0124] Example 6

[0125] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0126] (1) Raw material preparation:

[0127] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.8dL / g, bulk density 0.75g / cm 3 , the average particle size is 4.0 mm, and the melting point is 260°C;

[0128] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed by a mill to form powder with an intrinsic viscosity of 0.83dL / g and a bulk density of 0.8g / cm 3 , the average particle size is 100 mesh, and the melting point is 254°C;

[0129] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.3g / cm 3 , average particle size is 3.5μm, refractive index is 1.6, thermal decomposition temperature is 313℃;

[0130] Dispersant: a mixture of pentaerythritol stearate and calcium stearate in a mass ratio of 1:1;

[0131] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 1:1;

[0132] (2) Weighing raw materials:

[0133] By weight, take: 70 parts of carrier resin particles, 15 parts of pre-dispersed resin powder, 15 parts of organic microsphere powder, 0.4 parts of antioxidant, and 0.5 parts of dispersant;

[0134] (3) Preparation of organic polymer microparticle opening masterbatch:

[0135] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 130° C., the time is 10 min, and the speed is 1000 rpm;

[0136] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0137] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0138] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.297 bar / g.

[0139] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 30.8μm.

[0140] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0141] Example 7

[0142] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0143] (1) Raw material preparation:

[0144] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.68dL / g, bulk density 0.6g / cm 3 , the average particle size is 3.0 mm, and the melting point is 263°C;

[0145] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed into powder by a mill, with an intrinsic viscosity of 0.85dL / g and a bulk density of 0.8g / cm 3 , the average particle size is 50 mesh, and the melting point is 256°C;

[0146] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.25g / cm 3 , average particle size is 3.0 μm, refractive index is 1.6, thermal decomposition temperature is 308 °C;

[0147] Dispersant: pentaerythritol stearate;

[0148] Antioxidant: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate;

[0149] (2) Weighing raw materials:

[0150] By weight, take: 80 parts of carrier resin particles, 15 parts of pre-dispersed resin powder, 5 parts of organic microsphere powder, 0.2 parts of antioxidant, and 0.2 parts of dispersant;

[0151] (3) Preparation of organic polymer microparticle opening masterbatch:

[0152] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 120° C., the time is 6 min, and the speed is 900 rpm;

[0153] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0154] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0155] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.228 bar / g.

[0156] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 29.7μm.

[0157] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0158] Example 8

[0159] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0160] (1) Raw material preparation:

[0161] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.7dL / g, bulk density 0.65g / cm 3 , the average particle size is 3.0 mm, and the melting point is 265°C;

[0162] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed by a mill to form powder with an intrinsic viscosity of 0.83dL / g and a bulk density of 0.8g / cm 3 , the average particle size is 60 mesh, and the melting point is 255℃;

[0163] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.3g / cm 3 , average particle size is 3.0 μm, refractive index is 1.6, thermal decomposition temperature is 310°C;

[0164] Dispersant: pentaerythritol stearate;

[0165] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 3:2;

[0166] (2) Weighing raw materials:

[0167] By weight, take: 75 parts of carrier resin particles, 15 parts of pre-dispersed resin powder, 10 parts of organic microsphere powder, 0.5 parts of antioxidant, and 0.3 parts of dispersant;

[0168] (3) Preparation of organic polymer microparticle opening masterbatch:

[0169] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 120° C., the time is 8 min, and the speed is 1000 rpm;

[0170] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0171] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0172] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.289 bar / g.

[0173] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a casting sheet is prepared by multi-layer co-extrusion technology, and then the casting sheet is double-drawn to finally prepare a polyester functional film with a thickness of 29.8μm.

[0174] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0175] Example 9

[0176] A method for preparing an organic polymer microparticle open masterbatch, the specific steps are as follows:

[0177] (1) Raw material preparation:

[0178] Carrier resin particles: polyethylene terephthalate particles, intrinsic viscosity 0.68 dL / g, bulk density 0.65 g / cm 3 , the average particle size is 3.0 mm, and the melting point is 263°C;

[0179] Pre-dispersed resin powder: Polyethylene terephthalate particles are crushed by a mill to form powder with an intrinsic viscosity of 0.83dL / g and a bulk density of 0.8g / cm 3 , the average particle size is 55 mesh, and the melting point is 255℃;

[0180] Organic microsphere powder: monodisperse polystyrene microspheres, bulk density 0.4g / cm 3 , average particle size is 3.0 μm, refractive index is 1.6, thermal decomposition temperature is 310°C;

[0181] Dispersant: a mixture of pentaerythritol stearate and ethylene bisstearamide in a mass ratio of 1:1;

[0182] Antioxidant: a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite in a mass ratio of 3:2;

[0183] (2) Weighing raw materials:

[0184] By weight, take: 65 parts of carrier resin particles, 20 parts of pre-dispersed resin powder, 15 parts of organic microsphere powder, 0.5 parts of antioxidant, and 0.5 parts of dispersant;

[0185] (3) Preparation of organic polymer microparticle opening masterbatch:

[0186] Firstly, pre-dispersed resin powder, organic microsphere powder, dispersant and antioxidant are pre-mixed to obtain pre-mixed powder, wherein the pre-mixing temperature is 120° C., the time is 10 min, and the speed is 1100 rpm;

[0187] Then the premixed powder is fed into the twin-screw extruder through the side feed port, while the carrier resin particles are fed into the twin-screw extruder through the main feed port;

[0188] Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion and filtration.

[0189] The FPV value of the organic polymer microparticle open masterbatch finally obtained is 0.305 bar / g.

[0190] A method for preparing a polyester functional film, wherein an ABA three-layer structure is adopted during film casting, the interlayer ratio of A:B:A is 1:8:1, the raw materials of the A layer are polyester resin (FG604 of Yizheng Chemical Fiber) and the above-prepared organic polymer microparticle open masterbatch, and the raw materials of the B layer are polyester resin (FG604 of Yizheng Chemical Fiber), wherein the content of organic microsphere powder in the A layer is 1500ppm; a cast sheet is prepared by multi-layer co-extrusion technology, and the cast sheet is then double-drawn to finally prepare a polyester functional film with a thickness of 31.8μm.

[0191] The relevant performance data of the polyester functional film finally obtained are shown in Table 1 and Table 2.

[0192] The relevant performance data of the polyester functional films obtained in various embodiments and comparative examples are shown in Table 1 and Table 2 below:

[0193] Table 1

[0194]

[0195] Table 2

[0196]

[0197] It can be seen from the data in Tables 1 and 2 that the overall data values ​​of the optical and mechanical properties of the polyester functional film prepared by the method of the present invention are significantly better than those shown in Comparative Example 1, especially in terms of the key indicators of transmittance, clarity, haze, and friction coefficient. The use of the masterbatch prepared by the masterbatch preparation method of the present invention to prepare the polyester functional film has a more significant advantage in improving the optical properties and opening of the film, and is more suitable for making high-transmittance and high-brightness BOPET film.

[0198] From the data of Example 1 and Comparative Example 1, it can be found that the performance indicators of the polyester functional film finally obtained in Comparative Example 1 are worse than those in Example 1. The reason is that in the process of preparing the masterbatch in Comparative Example 1, the organic microsphere powder and the carrier resin particles are fed into the twin-screw extruder at the same time. The particle size of the organic microsphere powder is micron-level, the powder is very fine, and the resin particles are millimeter-level particles. After the two substances are physically mixed, the bulk density of the carrier resin particles and the organic microsphere powder is significantly different. When falling in the feed scale, affected by the airflow, the carrier resin particles (with larger particle size) will fall first, while the organic microsphere powder is difficult to feed, resulting in abnormal stratification of the two components of the feeding and uneven feeding, resulting in poor uniformity, dispersibility and stability of the masterbatch obtained by extrusion, which makes the various properties of the polyester functional film finally obtained using the masterbatch of Comparative Example 1 deteriorate.

Claims

1. A method for preparing an organic polymer microparticle open masterbatch, characterized in that: First, pre-dispersed resin powder, organic microsphere powder and additives are pre-mixed to obtain pre-mixed powder, and then the pre-mixed powder and carrier resin particles are fed into a twin-screw extruder from different feeding ports for melt blending to obtain an organic polymer microparticle open masterbatch; wherein the pre-dispersed resin powder and the carrier resin particles are made of the same material; the absolute value of the difference in particle size between the pre-dispersed resin powder and the organic microsphere powder does not exceed 500μm.

2. The method for preparing an organic polymer microparticle open masterbatch according to claim 1, characterized in that: The intrinsic viscosity of the pre-dispersed resin powder and the carrier resin particles is different, and both of the intrinsic viscosities are greater than 0.6 dL / g. The intrinsic viscosity of the pre-dispersed resin powder is higher than the intrinsic viscosity of the carrier resin particles.

3. The method for preparing an organic polymer microparticle open masterbatch according to claim 2, characterized in that: Organic microsphere powder is monodisperse polystyrene microspheres with a bulk density of 0.2-0.4g / cm 3 , particle size is 2-5μm, refractive index is 1.58-1.60, thermal decomposition temperature is >300℃; Pre-dispersed resin powder is a powder made by grinding polyethylene terephthalate particles with an intrinsic viscosity of 0.78-0.85dL / g and a bulk density of 0.7-0.9g / cm 3 , particle size is 30-100 mesh, melting point is 252-262℃; The carrier resin particles are polyethylene terephthalate particles with an intrinsic viscosity of 0.68-0.80 dL / g and a bulk density of 0.6-0.8 g / cm 3 , particle size is 2-4mm, melting point is 255-265℃.

4. The method for preparing an organic polymer microparticle open masterbatch according to claim 3, characterized in that: The premixing temperature is 100-130°C, the time is 5-10 minutes, and the speed is 800-1200 rpm.

5. The method for preparing an organic polymer microparticle open masterbatch according to claim 3, characterized in that: The additives are dispersants and antioxidants.

6. The method for preparing an organic polymer microparticle open masterbatch according to claim 5, characterized in that: In terms of weight, the added amount of each component is: 60-80 parts of carrier resin particles, 15-30 parts of pre-dispersed resin powder, 3-15 parts of organic microsphere powder, 0.2-0.5 parts of antioxidant, and 0.2-0.5 parts of dispersant.

7. The method for preparing an organic polymer microparticle open masterbatch according to claim 5, characterized in that: The specific process is: first, pre-dispersed resin powder, organic microsphere powder, dispersant, and antioxidant are premixed to obtain premixed powder, and then the premixed powder is fed into the twin-screw extruder through the side feeding port, and at the same time, the carrier resin particles are fed into the twin-screw extruder through the main feeding port. Finally, the organic polymer microparticle open masterbatch is obtained through twin-screw extrusion mixing, shearing, dispersion, and filtration.

8. An organic polymer microparticle open masterbatch prepared by the method for preparing an organic polymer microparticle open masterbatch according to any one of claims 3 to 7, characterized in that: The FPV value is 0.156-0.305bar / g.

9. A method for preparing a polyester functional film, using a multi-layer co-extrusion technology, characterized in that: The raw materials of the surface layer are polyester resin and the organic polymer microparticle open masterbatch as claimed in claim 8.

10. The method for preparing a polyester functional film according to claim 9, characterized in that: The content of organic microsphere powder in the surface layer is 1000-3000ppm; the thickness of the polyester functional film is 29-31.8μm, the transmittance is 90.1%-90.7%, the haze is 1.2%-3.1%, the clarity is 98.7%-99.7%, the gloss is 128.8-135.2GU, the dynamic friction coefficient is 0.328-0.397, the static friction coefficient is 0.343-0.382, the longitudinal tensile strength at break is 200-235MPa, the transverse tensile strength at break is 209-239MPa, the longitudinal elongation at break is 102%-187%, the transverse elongation at break is 100%-136%, the longitudinal elastic modulus is 4857-5653MPa, and the transverse elastic modulus is 6215-6656MPa.

Citation Information

Patent Citations

  • Antiblocking agent masterbatch for plastic film and preparation method of antiblocking agent masterbatch

    CN109181242A

  • Silicon dioxide anti-blocking agent for plastic film and preparation method of silicon dioxide anti-blocking agent

    CN114455597A

  • Polymer master batch with good dispersibility and its production method and application

    CN101429686A

  • Anti-blocking agent master batch for photodiffusion polyester based film and preparation method and application thereof

    CN101805497A

  • Light diffusion agent mother material used for light diffusion film, preparation method and application thereof

    CN101812220A

Cited By

  • Open master batch for ultra-smooth optical film and optical film

    CN120025666A