Titanium silicalite molecular sieve with high energy storage density, polypropylene composite material film and preparation method

By introducing titanium silicon molecular sieve TS-1 nanofiller into the polypropylene film and modifying its surface, the limitation between the dielectric constant and breakdown strength of the polypropylene film was solved, and its energy storage density and breakdown field strength were significantly improved. , achieving better capacitor performance.

CN118725367APending Publication Date: 2024-10-01GLOBAL ENERGY INTERCONNECTION RES INST CO LTD +1

Patent Information

Application Number
CN202410907994.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing polypropylene films have shortcomings in terms of high energy storage density, low dielectric constant and insufficient breakdown strength, making it difficult to be practically used in power grids. When a single nanofiller is introduced, the dielectric constant increases at the expense of a decrease in breakdown strength. This results in limited improvement in energy density.

Method used

The titanium silicon molecular sieve TS-1 nanofiller with pore size structure is introduced into the polypropylene matrix, and modified by surface grafting of maleic anhydride polypropylene to improve the compatibility between TS-1 and the polypropylene matrix to form TS-1/ PP-g-MAH/PP composite film enhances dielectric constant and breakdown field strength.

Benefits of technology

The dielectric constant and breakdown field strength of the polypropylene film are significantly improved, the maximum charging energy density is increased by 105%, and the discharge energy density is increased, providing better energy storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725367A_ABST
    Figure CN118725367A_ABST
Patent Text Reader

Abstract

The invention relates to a high-energy-storage-density titanium silicalite molecular sieve / polypropylene composite material film and a preparation method thereof, silanol hydroxyl is converted into amino to realize TS-1 nanoparticle surface modification, maleic anhydride grafted polypropylene is introduced as an intermediate phase, organic groups are grafted on the surface, and the compatibility of filler-matrix is improved. And meanwhile, the dielectric constant is ensured to be improved, and the material has good energy storage performance. The invention provides a technical basis for improving the energy storage density of the polypropylene film capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of polymer composite dielectric energy storage films, and specifically relates to a titanium silicon molecular sieve (TS-1)-maleic anhydride grafted polypropylene-polypropylene composite film with high energy storage density and a preparation method thereof. Technical Background

[0002] Energy is the driving force of today's social development and an important material basis for human survival and development. With the changes in the international energy landscape, low-carbon multi-energy integrated energy systems have gradually become dominant. New green energy has gradually come into people's view. In order to effectively utilize renewable energy with randomness and volatility, various energy storage devices are indispensable. Polymer film capacitors have self-healing properties, high breakdown field strength, high power density, low dielectric loss, mechanical and chemical stability, good thermoplasticity, strong processability, better voltage resistance and rated voltage, long life, etc. It has great development space and is one of the most commonly used energy storage devices on the market.

[0003] Polypropylene (PP) is one of the most widely used energy storage dielectric polymers, with advantages such as low dielectric loss, high breakdown strength and power density, fast energy storage and release speed, and good processability. However, due to its low dielectric constant, the improvement of energy storage density is greatly limited. At an operating electric field strength of 200kV / mm, its energy storage density is only 0.5J / cm 3 , which is difficult to be applied in the power grid. Therefore, it is urgent to develop a polypropylene film with excellent energy storage performance. For linear dielectrics such as polypropylene, the formula for energy storage density can be simplified to: Where ε0 is the dielectric constant of vacuum, ε r is the relative dielectric constant, and it is clear that the ε of polypropylene material r and the maximum E that can be applied to the material (i.e., E b , breakdown strength) is the key parameter that determines the energy storage density.

[0004] Add high dielectric constant (high ε) to the PP matrix r ) Nanofillers are used to increase the dielectric constant, which is a common method for preparing polypropylene-based nanocomposite films with high energy storage density. Since there is a certain limiting relationship between the dielectric constant and the breakdown strength, it can be summarized as E b ∝ε r 0.5 (E bis the experimental value of Weibull breakdown). The inversion relationship shows that the increase of any parameter will come at the expense of a sharp decrease in another parameter. There are many studies on this aspect: for example, Zhang et al. introduced 20 vol% high dielectric barium titanate (BT) into a polypropylene matrix, and the dielectric constant increased from 2.3 to 6.7, while the breakdown field strength of the PP matrix dropped sharply from 622 MV / m to 162 MV / m. Zhou et al. prepared PP / AlN nanocomposite films using high dielectric ceramic AlN as filler. With the increase of AlN nanofiller content, the dielectric constant increased slightly, and the dielectric loss remained at an extremely low level below 0.003. However, compared with pure PP, the introduction of AlN nanofiller reduced the DC and AC breakdown strength, and the breakdown strength continued to decrease with the increase of AlN nanofiller content. Therefore, when polypropylene is modified by a single filler, the increase in dielectric constant is at the expense of a significant decrease in breakdown strength, resulting in limited improvement in energy density, which is something we do not want to see. Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, the present invention introduces a nanofiller TS-1 with an aperture structure into a polypropylene matrix. Since the intrinsic dielectric constant of the titanium silicon molecular sieve TS-1 is large, the dielectric constant of the composite film is significantly improved after the high dielectric nanofiller TS-1 is doped into the polypropylene matrix. In addition, TS-1 has an aperture structure, and its aperture structure can be regulated to make it comparable to the collapse head diameter of the electron avalanche in the α process of electron impact ionization in the solid dielectric. To a certain extent, the electron avalanche breakdown phenomenon caused by the continuous development of electron impact ionization can be suppressed, so that the maximum external electric field strength that the polypropylene-based composite film can withstand is increased. Thereby, a single filler is introduced into polypropylene, so that the dielectric constant and the breakdown field strength are improved at the same time, and the technical problem of the mutual restriction of dielectric properties and breakdown properties is overcome to a certain extent, and a polypropylene film with better energy storage performance is obtained.

[0006] In the process of preparing TS-1 / PP nanocomposite film, it is found that due to the large difference in polarity and surface energy between TS-1 and PP, the filler is very easy to agglomerate, difficult to be evenly dispersed in the matrix, and unable to form a dense body and a compatible interface with the polypropylene matrix. The compatibility problem between the two phases makes it easy for the polymer-based nanocomposite to form pores, and the dielectric and breakdown properties of the polypropylene film are slightly improved. In order to improve the compatibility problem between TS-1 and PP, the TS-1 nanoparticles are modified in the present invention, organic groups are grafted on the surface, and maleic anhydride grafted polypropylene is introduced as an intermediate phase to improve the compatibility of the two. (Comparative Example 1: When the frequency is 1 MHz, the dielectric constant of the unmodified TS-1 / PP composite film is 2.520 and the breakdown field strength is 294.67 kV / mm when the filler doping amount is 1.0 wt%. Under the same filler content, the dielectric constant and breakdown field strength of the modified TS-1 / PP-g-MAH / PP nanocomposite film are increased to 2.559 and 362.11 kV / mm, respectively).

[0007] Therefore, the present invention introduces nanofiller TS-1 with a pore structure into the polypropylene matrix, and modifies it to improve its compatibility with the polypropylene matrix, and prepares a polypropylene-maleic anhydride grafted polypropylene-titanium silicon molecular sieve TS-1 composite film. The breakdown field strength is significantly improved, and the dielectric constant is guaranteed to be improved at the same time. When the doping concentration of TS-1 in TS-1 / PP-g-MAH / PP is 1wt%, the relevant electrical properties are improved to the maximum, and the dielectric constant and breakdown field strength are increased to 2.559 and 362.11kV / mm, respectively, which are increased by 18.7% and 56.97% respectively compared with pure PP, and the maximum charging energy density is 4.11J / cm 3 Increased by 105%, the discharge energy density increased to 3.35J / cm 3 , and has good energy storage performance. The invention provides a technical basis for improving the energy storage density of polypropylene film capacitors.

[0008] The specific technical solution of the present invention is:

[0009] The method for preparing a high energy storage density titanium silicon molecular sieve and polypropylene composite film is to modify TS-1 nanoparticles, graft organic groups on the surface, and introduce maleic anhydride grafted polypropylene as an intermediate phase to improve the compatibility of the two.

[0010] Preferably, the TS-1 modification comprises the following steps:

[0011] (1) Surface hydroxylation of molecular sieves: The molecular sieves react with hydrogen peroxide to obtain hydroxylated molecular sieves;

[0012] (2) Surface amination of molecular sieves: The hydroxylated molecular sieves were amino-modified in an anhydrous ethanol solution of 3-aminopropyltriethoxysilane, and acetic acid was added as a catalyst to prepare the amination molecular sieves;

[0013] (3) Grafting PP onto the molecular sieve surface: The amino molecular sieve reacts with the purified PP-g-MAH to obtain TS-1 / PP-g-MAH.

[0014] Preferably, the surface of the molecular sieve is hydroxylated: the molecular sieve and hydrogen peroxide are added to a round-bottom bottle, and ultrasonicated at room temperature; then reacted under magnetic stirring, filtered after cooling, and washed with a large amount of water; hydroxylated TS-1-OH is obtained, and more amino reaction sites are introduced.

[0015] Preferably: the surface of the molecular sieve is aminated: the hydroxylated molecular sieve is amino-modified in an anhydrous ethanol solution of 3-aminopropyltriethoxysilane, acetic acid is added as a catalyst, ultrasonically dispersed, and then reacted under magnetic stirring, cooled and filtered, and washed with a large amount of water to obtain the TS-1 molecular sieve with surface amino modification; a small amount of turbid solution is taken out from the mixture, filtered and washed with toluene, and vacuum dried to obtain the aminated molecular sieve.

[0016] The preferred method is: grafting PP on the surface of molecular sieve: commercial PP-g-MAH is dissolved in toluene, heated until completely dissolved, cooled, and a large amount of acetone is slowly poured in while hot to precipitate the product, which is filtered to remove the ungrafted small molecule maleic anhydride; the aminated molecular sieve is added to a round-bottom bottle, and then toluene is added, and the purified PP-g-MAH is added, heated to react, cooled to 50°C, and a large amount of acetone (about 3 times) is slowly poured in while hot, filtered and washed with acetone to remove free maleic anhydride oligomers; finally, the separated precipitate is dried in a vacuum to remove the residual acetone, and TS-1 / PP-g-MAH is finally obtained.

[0017] Preferably, the synthesis of TS-1 comprises the following steps: preparing titanium silicon molecular sieve TS-1 by in-situ hydrothermal synthesis method, using Ti2(SO)4 as titanium source, tetraethyl orthosilicate (TEOS) as silicon source, and tetrapropylammonium hydroxide (TPAOH) as template.

[0018] Preferably, the preparation of the high energy storage TS-1 / PP-g-MAH / PP composite film comprises the following steps: the molar ratio of each material is tetraethyl orthosilicate: titanium dioxide: tetrapropylammonium hydroxide: water: hydrogen peroxide = 1.00:0.05:0.40:20:0.20.

[0019] Preferably, the preparation of high energy storage TS-1 / PP-g-MAH / PP composite film includes the following steps: preheating and heating, first use PP particles to clean the cavity 2-3 times. After the cavity is cleaned, run the machine, first pour the weighed polypropylene particles and TS-1 / PP-g-MAH into the cavity in turn, melt compound, and the blending is completed after the machine stops automatically; use a flat vulcanizer to hot press and form a film.

[0020] The invention also relates to a composite film prepared by the method.

[0021] The invention also relates to the application of the composite film in polymer film capacitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 :SEM images of the cross section of the composite film when the TS-1 content is 1.0wt% (a) Unmodified TS-1 / PP nanocomposite film (b) Modified TS-1 / PP-g-MAH / PP nanocomposite film

[0023] Figure 2 :Dielectric constant curves (a) Unmodified TS-1 / PP nanocomposite film (b) Modified TS-1 / PP-g-MAH / PP nanocomposite film

[0024] Figure 3 :Breakdown field strength data diagram (a) Unmodified TS-1 / PP nanocomposite film (b) Modified TS-1 / PP-g-MAH / PP nanocomposite film

[0025] Figure 4 :(a) DE cycle (b) discharge energy density, (c) maximum energy density and charge-discharge efficiency of modified TS-1 / PP-g-MAH / PP nanocomposite films DETAILED DESCRIPTION

[0026] 1. Synthesis and pore structure control of TS-1

[0027] Titanium silicate molecular sieve TS-1 was prepared by in-situ hydrothermal synthesis, with Ti2(SO)4 as titanium source, tetraethyl orthosilicate (TEOS) as silicon source, and tetrapropylammonium hydroxide (TPAOH) as template. During the experiment, an analytical balance was used to accurately weigh the mass of each raw material required, and the molar ratio of each material in the mixed solution was controlled to be tetraethyl orthosilicate: titanium dioxide: tetrapropylammonium hydroxide: water: hydrogen peroxide = 1.00: 0.05: 0.40: 20: 0.20.

[0028] (1) Accurately weigh ultrapure water (55.0 g) and TPAOH (48.8 g), mix thoroughly and slowly heat to 80° C. Keep mechanical stirring during the process, and add TEOS (16.0 g) dropwise to the above mixture within 1 hour.

[0029] (2) Weigh Ti2(SO)4 (1.8 g), dissolve it in hydrogen peroxide (30 wt.%) and dilute it with a small amount of ultrapure water. Then, add it dropwise to the above reaction system and stir it under air atmosphere.

[0030] (3) Finally, the silica sol was injected into the mixed solution and hydrolyzed at 80°C for 6 hours. Ultrapure water was continuously added to fill the liquid level. After the reaction, the mixed solution was transferred to a reactor and hydrothermally crystallized at 160°C for 12 hours.

[0031] (4) The precipitate was centrifuged at 10,000 rpm and washed 5 times to remove excess alkaline substances. Finally, the separated precipitate was vacuum dried at 80° C. for 24 h to remove residual water and obtain a white powder for standby use.

[0032] (5) Accurately weigh a certain mass of the above powdered sample and press TS-1 a :TPAOH:H2O=1:3:5 mass ratio to prepare a mixed solution. 1g TS-1 molecular sieve, 3g TPAOH, 5g H2O, mix, ultrasonicate for 0.5h, put into autoclave, react at 160℃ for 48h.

[0033] (2) After taking out, centrifuge, wash with water, dry, collect the precipitate, and dry it in a vacuum oven overnight to obtain a white powdery substance.

[0034] (3) The molecular sieve without template removal is placed in a muffle furnace, heated to 800°C, kept at this temperature for 3 hours, and then cooled to room temperature. The template removal agent is calcined at high temperature to obtain a molecular sieve with a hollow structure.

[0035] 2. TS-1 modification

[0036] (1) Surface hydroxylation of molecular sieves:

[0037] 5g molecular sieve and 100ml 30% hydrogen peroxide were added to a 250ml round-bottom bottle, and ultrasonicated for 30min at room temperature; then reacted at 105℃ for 5h under magnetic stirring, filtered after cooling, and washed with a large amount of water to obtain hydroxylated TS-1-OH, introducing more amino reaction sites.

[0038] (2) Surface amination of molecular sieves:

[0039] The hydroxylated molecular sieve was amino-modified in an anhydrous ethanol solution of 3-aminopropyltriethoxysilane, 2-3 drops of acetic acid were added as a catalyst, and then ultrasonically dispersed, and then reacted at 90°C for 5 hours under magnetic stirring, cooled and filtered, and washed with a large amount of water to obtain the surface amino-modified TS-1 molecular sieve. A small amount of turbid solution was taken from the mixture, filtered and washed with toluene, and vacuum dried for 6 hours to obtain the functionalized TS-1-g-APS.

[0040] (3) Molecular sieve surface grafted with PP:

[0041] a: 20g of commercial PP-g-MAH was dissolved in 400ml of toluene and heated at 110°C until completely dissolved. The temperature was lowered to 50°C and a large amount of acetone (about 3 times) was slowly poured in while hot to precipitate the product, which was filtered to remove the ungrafted small molecule maleic anhydride.

[0042] b: Add the aminated molecular sieve to a 500ml round-bottom bottle, add 200ml toluene, add 12g purified PP-g-MAH, heat at 110℃ for 3h, cool to 50℃, slowly pour in a large amount of acetone (about 3 times) while hot, filter and wash with acetone to remove free maleic anhydride oligomers. Finally, dry the separated precipitate at 60℃ in vacuum for 24h to remove residual acetone, and finally obtain TS-1 / PP-g-MAH.

[0043] (4) Extraction to determine the grafting rate:

[0044] Accurately weigh a certain mass of TS-1 / PP-g-MAH with surface grafted polypropylene, record the mass as m, wrap it with filter paper and accurately weigh the total mass of the filter paper and sample M1, extract it using Soxhlet extraction method, heat and reflux at 120 degrees for 5 hours. After the experiment, dry the filter paper wrapped with the sample, weigh the total weight of the two again and record it as M2. Calculate the grafting rate based on the mass difference before and after extraction.

[0045] 3. Preparation of high energy storage TS-1 / PP-g-MAH / PP composites

[0046] (1) Before the experiment, the raw materials were placed in a vacuum drying oven for 24 h to remove excess moisture and avoid the interference of water vapor on the experimental data;

[0047] (2) Turn on the torque rheometer mixing platform and set the torque rheometer parameters to a temperature range of 180-190°C, a rotation speed of 45-60 r / min, and a mixing time of 15-20 min;

[0048] (3) Preheat the temperature first. After the instrument is heated to a temperature range of 180-190°C and remains stable for 1-2 minutes, use PP particles to clean the cavity 2-3 times. After the cavity is cleaned, run the machine, first pour the weighed polypropylene particles and TS-1 / PP-g-MAH into the cavity in turn, melt compound, and wait for the machine to stop automatically before blending. In the mixture, the total mass of polypropylene and TS-1 / PP-g-MAH is 20g, and the mass proportions of nanoparticles TS-1 are 0, 0.5wt.%, 1.0wt.%, 1.5wt.%, and 2.0wt.%, respectively.

[0049] To ensure the same experimental environment, the above steps were repeated to prepare the TS-1 / PP composite material of Comparative Example 1. In the mixture, the total mass of polypropylene and TS-1 was 20 g, and the mass proportions of nanoparticle TS-1 were 0, 0.5 wt.%, 1.0 wt.%, 1.5 wt.%, and 2.0 wt.%, respectively.

[0050] 4. Preparation of high energy storage TS-1 / PP-g-MAH / PP composite film

[0051] (1) A square hole with a side length of 10 cm was cut from a polyimide film with a thickness of about 100 μm as a mold. 0.20 g of the composite material was placed in each square hole of the mold and hot-pressed into a film using a flat vulcanizer.

[0052] (2) Turn on the flat vulcanizer for preheating, which takes about 10-15 minutes. At the same time, cut and wipe the required templates clean;

[0053] (3) After reaching the temperature, the pellets were placed in the No. 1 flat vulcanizer, with the pressure set to 0 MPa, the temperature to 180 °C and the time to 10 min. The main purpose was to melt the TS-1 / PP pellets.

[0054] (4) Take out the mold in the No. 1 plate vulcanizer and put it into the No. 2 plate vulcanizer. Set the pressure to 16 MPa, the temperature to 195 °C, and the time to 15 min. In order to reduce the bubbles in the sample film, it is necessary to deflate during the process (the number of deflation times can be set to 10-15 times, 9-11 seconds each time, or 10 times, 10 seconds each time). In the No. 2 plate vulcanizer, the TS-1 / PP-g-MAH / PP composite material will form the desired composite film;

[0055] (5) Take out the mold from the No. 2 flat vulcanizer and put it into the No. 3 flat vulcanizer. Set the pressure to 16 MPa, the temperature to 180 °C, and the time to 10 min. The No. 3 vulcanizer is mainly used for cold pressing to quickly cool down the composite material so that the composite film can be cooled and formed.

[0056] (6) The mold is removed and the scraps at the edge of the film are removed to obtain the desired composite film with a thickness of 100-130 μm.

[0057] The above steps were repeated to prepare the TS-1 / PP composite film of Comparative Example 1.

[0058] The properties of TS-1 / PP-g-MAH / PP composite film were tested by using TS-1 as filler after hollow structure treatment and surface modification. The mass fraction of TS-1 molecular sieve was found to be 1.0wt.% when the mass fraction of TS-1 molecular sieve introduced was the best.

[0059] Sample performance test:

[0060] The obtained samples were subjected to morphological characterization and performance testing, and the breakdown performance, dielectric properties and energy storage density of the samples were tested respectively.

[0061] Field emission scanning electron microscope (JSM-6700F) was used to characterize the surface morphology of the quenched cross section of the composite film. Before the test, the film sample was cleaned with ethanol and placed in a vacuum drying oven at 60°C for drying. The sample was then rapidly quenched in liquid nitrogen, gold-sprayed, and the cross section of the sample after quenching was observed by SEM.

[0062] The test results are as attached Figure 1 shown.

[0063] The black and gray areas in the figure are PP matrix, and the bright particle area is filler. Before modification, the high polarity filler will preferentially gather together and agglomerate. After modification, the nanoparticles are evenly distributed in the matrix, with a good bonding interface between the two, and no obvious pores and defects.

[0064] from Figure 1 It can be seen that due to the large difference in polarity between TS-1 as a high-polar filler and the non-polar polypropylene matrix, the high-polarity filler particles in the unmodified TS-1 / PP nanocomposite film are very easy to agglomerate and difficult to disperse evenly in the matrix. The compatibility problem between the filler and the matrix leads to certain pores and defects in the nanocomposite film, which will have a negative impact on the energy storage performance of the polypropylene composite film.

[0065] The modified TS-1 / PP-g-MAH / PP ternary composite system particles have good compatibility with the matrix, and no voids are observed on the surface of the composite material, indicating that the TS-1 nanofiller is evenly distributed in the PP matrix after chemical modification, and there is a good bonding interface between the two, without obvious pores and defects.

[0066] The wideband dielectric spectrometer NG-40 from Novocontrol GmbH, Germany, tests the dielectric properties of composite film. Before the test, copper electrodes are deposited on both sides of the film using a high vacuum resistance evaporation coating machine to improve the accuracy and repeatability of the experimental data. During the test, the sample is ensured to be in close contact with the upper and lower electrodes and the test is carried out at room temperature to obtain the dielectric constant and dielectric loss of the sample.

[0067] The present invention tests the composite films of Example TS-1 / PP-g-MAH and Comparative Example TS-1 / PP containing different mass fractions of TS-1.

[0068] The experimental results are as follows Figure 2 shown.

[0069] from Figure 2 It can be seen that when the TS-1 doping amount of the unmodified TS-1 / PP nanocomposite film is 0.0wt.%, 0.5wt.%, 1.0wt.%, 1.5wt.% and 2.0wt.%, the corresponding dielectric constants of the nanocomposite film are 2.152, 2.317, 2.520, 2.430 and 2.278, respectively, and the optimal doping amount is 1.0wt.%. The dielectric constants of the modified TS-1 / PP-g-MAH / PP nanocomposite film are 2.152, 2.409, 2.559, 2.489 and 2.332, respectively.

[0070] The dielectric constants of TS-1 / PP and TS-1 / PP-g-MAH / PP nanocomposite films are higher than those of pure polypropylene matrix. The dielectric constants of the samples are relatively stable within the tested frequency range, and the dielectric constant values ​​do not change significantly. With the increase of TS-1 doping amount, the dielectric constant first increases and then decreases. The dielectric properties of the modified ternary composite system are significantly higher than those of the unmodified TS-1 / PP.

[0071] Chemical modification improves the dispersibility of polar fillers in non-polar matrix, improves the compatibility between TS-1 and polypropylene matrix, and avoids the formation of voids and defects inside the material. The fillers are evenly dispersed in the matrix to form a nanoparticle-polymer matrix interface, which produces interfacial polarization under the action of an external electric field. Under the combined action of the two, the dielectric constant of the modified TS-1 / PP-g-MAH / PP nanocomposite film is higher than that of the unmodified TS-1 / PP binary system.

[0072] TS-1 can improve the dielectric constant of the sample, which is related to the process of TS-1 changing the internal polarization of the PP composite sample. In the composite material, the particles with strong dielectric constant have electronic displacement polarization and steering polarization, and TS-1 dispersed in the PP matrix will form a nanoparticle-polymer matrix interface. Under the influence of several polarization effects, the dielectric constant of the composite material is significantly improved. However, as the filler content continues to increase, the filler particles will hinder the movement of the polymer molecular chain, which is not conducive to the occurrence of polarization and the dielectric constant decreases.

[0073] For the unmodified TS-1 / PP composite film in the comparative example, at the same TS-1 doping amount, the dielectric constants of the corresponding nanocomposites were 2.317, 2.520, 2.430 and 2.278, respectively, which were lower than those of the modified examples.

[0074] The voltage breakdown tester DDJ-100 produced by Beijing Guance Precision Instrument Equipment Co., Ltd. was used for testing. 10-15 points were measured for each sample, and the data were processed using Weibull distribution to obtain the breakdown strength value.

[0075] The present invention tested the composite film of Example TS-1 / PP-g-MAH and Comparative Example TS-1 / PP containing different mass fractions of TS-1. The experimental results are shown in Figure 3 shown.

[0076] The results show that the breakdown field strength increases first and then decreases with the increase of TS-1 doping amount. For the unmodified TS-1 / PP nanocomposite film, when the TS-1 doping amount is 0.0wt.%, 0.5wt.%, 1.0wt.%, 1.5wt.% and 2.0wt.%, the corresponding breakdown field strength of the nanocomposite is 230.69, 254.44, 277.57, 267.69 and 260.33 kV / mm, respectively, and the optimal doping amount is 1.0wt.%. The breakdown field strength of the TS-1 / PP-g-MAH / PP nanocomposite film modified with the same filler doping amount is 230.69, 299.40 / 321.56 / 362.11 / 287.91 kV / mm, respectively. The maximum breakdown field strengths of the two nanocomposite films are E b =277.57kV / mm and 362.11kV / mm, and the breakdown strength of pure polypropylene PP was measured to be 230.69kV / mm under the same experimental conditions, which were increased by 20.36% and 56.97% respectively. The breakdown strength of the modified TS-1 / PP-g-MAH nanocomposite film of Example TS-1 was 36.61% higher than that of the comparative example TS-1 / PP.

[0077] After the introduction of TS-1, the breakdown field strength of TS-1 / PP and TS-1 / PP-g-MAH / PP nanocomposite films was improved to varying degrees, both higher than that of pure polypropylene matrix. This is because the pore structure of TS-1 can hinder the development of electron impact ionization under the action of an external electric field, inhibit electron avalanche breakdown, and thus improve the breakdown field strength of polypropylene composite films.

[0078] Comparing the two figures (a) and (b), it can be seen that the breakdown field strength of the modified TS-1 / PP-g-MAH / PP ternary composite system is significantly better than that of the unmodified TS-1 / PP nanocomposite film. There are many factors that increase the breakdown field strength (Eb) of the ternary modified system. On the one hand, the introduction of maleic anhydride grafted polypropylene (PP-g-MAH) as an intermediate phase can improve the interface between the polar filler TS-1 and the non-polar polypropylene (PP) matrix, reduce the defect density inside the material, and avoid the formation of weak points of breakdown. On the other hand, the dielectric constant of PP-g-MAH itself is slightly higher than that of the polypropylene matrix. After the introduction of maleic anhydride grafted polypropylene into the matrix, the self-agglomeration of TS-1 caused by the large difference in polarity can be reduced to a certain extent, the dispersibility of TS-1 can be improved, the formation of voids and holes inside the material can be reduced, and the maximum applied voltage that the TS-1 / PP-g-MAH / PP three-nanocomposite film can withstand can be increased.

[0079] Combined with the above experimental results, it can be seen that the dielectric and breakdown properties of the modified TS-1 / PP-g-MAH / PP ternary composite material are significantly better than those of the unmodified TS-1 / PP.

[0080] In order to further determine the value of the energy storage density of the TS-1 / PP-g-MAH / PP ternary composite film in Example 1, the DE curve was tested at a monopolar triangle voltage of 500 MV / m and an applied voltage frequency of 10 Hz. e The specific value of ) can be obtained by integrating the potential shift of the DE curve with the area of ​​the discharge curve. The charge and discharge efficiency (η) of the composite membrane is obtained by calculating the ratio of the discharge energy density to the charge energy density.

[0081] The experimental results are as follows Figure 4 shown.

[0082] The results show that the maximum discharge energy density of the modified TS-1 / PP-g-MAH / PP nanocomposite film is 4.11 J / cm2 at an electric field of 500 MV / m when the TS-1 content is 1.0 wt%. 3 , which is 105% higher than that of pure matrix. e Also from the initial 1.63J / cm3 Increased to 3.35 J / cm 3 Moreover, the film still maintains a high charge and discharge efficiency of more than 95% when the filler content is 2.0wt% under an electric field of up to 500MV / m.

Claims

1. A method for preparing a high energy storage density titanium silicon molecular sieve / polypropylene composite film, characterized in that: TS-1 nanoparticles were modified, maleic anhydride grafted polypropylene was introduced as the intermediate phase, and organic groups were grafted on the surface to improve the compatibility between the polar filler and the non-polar matrix.

2. The method according to claim 1, characterized in that: TS-1 modification includes the following steps: (1) Surface hydroxylation of molecular sieves: The molecular sieves react with hydrogen peroxide to obtain hydroxylated molecular sieves; (2) Surface amination of molecular sieves: The hydroxylated molecular sieves were amino-modified in an anhydrous ethanol solution of 3-aminopropyltriethoxysilane, and acetic acid was added as a catalyst to prepare the amination molecular sieves; (3) Grafting PP onto the molecular sieve surface: The amino molecular sieve reacts with the purified PP-g-MAH to obtain TS-1 / PP-g-MAH.

3. The method according to claim 1, characterized in that: Surface hydroxylation of molecular sieves: Molecular sieves and hydrogen peroxide are added to a round-bottom bottle and ultrasonicated at room temperature; the reaction is stirred magnetically, filtered after cooling, and washed with a large amount of distilled water; hydroxylated TS-1-OH is obtained, and more amino reaction sites are introduced.

4. The method according to claim 1, characterized in that: Surface amination of molecular sieves: The hydroxylated molecular sieve is amino-modified in an anhydrous ethanol solution of 3-aminopropyltriethoxysilane, acetic acid is added as a catalyst, and the mixture is subjected to ultrasonic dispersion and reacted under magnetic stirring. The mixture is cooled and filtered, and washed with a large amount of water to obtain the surface amino-modified TS-1-NH3 molecular sieve; a small amount of turbid solution is taken out from the mixture, filtered, washed with toluene, and vacuum dried to obtain the amino-modified molecular sieve.

5. The method according to claim 1, characterized in that: Grafting PP on the surface of molecular sieve: Commercial PP-g-MAH is dissolved in toluene, heated until completely dissolved, cooled, and a large amount of acetone is slowly poured in while hot to precipitate the product, which is filtered to remove the ungrafted small molecule maleic anhydride; the amino molecular sieve is added to a round-bottom bottle, and then toluene is added, and the purified PP-g-MAH is added, heated to react, cooled to 50°C, and a large amount of acetone (about 3 times) is slowly poured in while hot, filtered and washed with acetone to remove free maleic anhydride oligomers; finally, the separated precipitate is dried in a vacuum to remove the residual acetone, and TS-1 / PP-g-MAH is finally obtained.

6. The method according to claim 2, characterized in that: The synthesis of TS-1 includes the following steps: preparing titanium silicon molecular sieve TS-1 by in-situ hydrothermal synthesis method, using Ti2(SO)4 as titanium source, tetraethyl orthosilicate (TEOS) as silicon source, and tetrapropylammonium hydroxide (TPAOH) as template.

7. The method according to claim 6, characterized in that: The preparation of the high energy storage TS-1 / PP-g-MAH / PP composite film includes the following steps: the molar ratio of each material is ethyl orthosilicate: titanium dioxide: tetrapropylammonium hydroxide: water: hydrogen peroxide = 1.00:0.05:0.40:20:0.

20.

8. The method according to any one of claims 1 to 7, characterized in that: The preparation of high energy storage TS-1 / PP-g-MAH / PP composite film includes the following steps: preheating and heating, first use PP particles to clean the cavity 2-3 times. After the cavity is cleaned, run the machine, first pour the weighed polypropylene particles and TS-1 / PP-g-MAH into the cavity in turn, melt compound, and wait for the machine to stop automatically when the blending is completed; use a flat vulcanizer to heat press and form a film.

9. A composite film prepared by the method according to any one of claims 1 to 8.

10. Use of the composite film as claimed in claim 9 in polymer film capacitors.

Citation Information

Patent Citations

  • High-energy storage density polypropylene-maleic anhydride grafted polypropylene-nano-zirconia composite material and preparation method thereof

    CN107987390A

  • Preparation method of core-shell-structured nanometer aluminum oxide@zirconium oxide-polypropylene / maleic anhydride grafted polypropylene composite material

    CN111978629A

  • Core-shell nano silicon oxide@zirconium oxide particle-polypropylene maleic anhydride grafted polypropylene composite material and preparation method thereof

    CN112358674A

  • Film having an oxygen scavenger and a volatile organoleptic compound scavenger

    US20190134958A1

Cited By

  • Titanium silical molecular sieve / mesophase aramid composite thin film dielectric material, preparation method and application thereof

    CN122978488A