Calcium carbonate powder and solid waste powder composite low-cost powder for polyolefin plastic blow-off pipeline and preparation method of calcium carbonate powder and solid waste powder composite low-cost powder

The composite low-cost powder of calcium carbonate powder and solid waste powder solves the problems of high cost and insufficient performance of polyolefin plastic sewage pipe materials, improves high temperature resistance, corrosion resistance and acid and alkali resistance, and prolongs the service life and improved processability.

CN118725410APending Publication Date: 2024-10-01JIANGSU HENGLINGQI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985746.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing polyolefin plastic sewage pipe materials have high cost and insufficient performance. They cannot meet the requirements of high temperature resistance, corrosion resistance, acid and alkali resistance, short service life, and are prone to breakage and aging.

Method used

A composite low-cost powder of calcium carbonate powder and solid waste powder is used. Through modifier treatment and grinding aid addition, a mixture of 50-80% calcium carbonate powder and 20-50% solid waste powder is formed. Ratio, use ring roller mill and gravity-free mixer for processing to improve the performance and processability of the material.

Benefits of technology

It significantly reduces the cost of raw materials, improves the high temperature resistance, corrosion resistance, acid and alkali resistance of polyolefin plastic sewage pipes, extends the service life, and improves the processability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725410A_ABST
    Figure CN118725410A_ABST
Patent Text Reader

Abstract

The invention discloses a calcium carbonate powder and solid waste powder composite low-cost powder for a polyolefin plastic blow-off pipeline, which comprises the following components in parts by mass: 50-80 parts of calcium carbonate powder and 20-50 parts of solid waste powder, the invention further discloses a method for preparing the composite low-cost powder from the ingredients. In the preparation process of the polyolefin plastic for the blow-off pipeline, the solid waste which is an extremely low-cost raw material is compounded with the calcium carbonate and is modified, so that the cost of the calcium carbonate composite powder obtained by compounding is greatly reduced, and due to the change process experienced in the solid waste generation process, the solid waste can be recycled. And the polyolefin filled with the composite material and the calcium carbonate powder has higher performance and better processability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials for sewage pipes, and in particular to a low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes, and also to a preparation method of the low-cost powder. Background Art

[0002] Due to the complexity of the medium transported by polyolefin plastic sewage pipes and the harshness of their use environment, they are required to have properties such as high temperature resistance, corrosion resistance, corrosion resistance, and acid and alkali resistance. Among them, high temperature resistance mainly refers to the stability of the performance of plastic pipes at high temperatures, corrosion resistance mainly refers to the ability of plastic pipes to resist the erosion of various chemical substances, corrosion resistance mainly refers to the ability of plastic pipes to resist the corrosion of harmful substances such as seawater and acid rain, and acid and alkali resistance mainly refers to the stability of plastic pipes in strong acid and strong alkali environments. In addition, a good polyolefin plastic sewage pipe should have a long service life and will not break or age during use. Based on the above-mentioned use requirements of polyolefin plastic sewage pipes, the materials used in their production are required to be high, resulting in high material costs and prices. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a low-cost powder composited with calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes, which has the advantages of low cost, high performance, and easy processing.

[0004] In order to solve the above technical problems, the technical solution of the present invention is: comprising the following components in proportion by weight: 50 to 80 parts of calcium carbonate powder and 20 to 50 parts of solid waste powder;

[0005] The calcium carbonate powder and the solid waste powder are modified by a modifier respectively, wherein the amount of the modifier used in the modification of the calcium carbonate powder is 0.7-1.2% of its mass; and the amount of the modifier used in the modification of the solid waste powder is 0.7-1.2% of its mass;

[0006] The calcium carbonate powder is obtained by processing calcium carbonate ore. When producing the calcium carbonate powder, a grinding aid needs to be added. The amount of the grinding aid is 1-2‰ of the mass of the calcium carbonate ore.

[0007] The solid waste powder is obtained by processing solid waste. The grinding aid also needs to be added when producing the solid waste powder. The amount of the grinding aid is 1 to 2‰ of the mass of the solid waste.

[0008] As a preferred technical solution, the calcium carbonate ore is formed into calcium carbonate powder by a ring roller mill, and the particle size of the calcium carbonate powder detected by an OMEC particle size tester is 11.600 μm ≤ D 97 ≤20.300μm;

[0009] The solid waste includes one of the solid wastes from calcium oxide production, steelmaking, and fiberglass scrap solid waste;

[0010] The solid waste is ground by a roller mill to obtain solid waste powder, and the particle size of the solid waste powder detected by an OMEC particle size tester is 9.800 μm≤D 97 ≤18.900μm;

[0011] The maximum size of the calcium carbonate ore and the solid waste is ≤35mm.

[0012] As a preferred technical solution, the modifier is a combination of two or more of an aluminum-zirconium organometallic complex, a nitrogen-containing long-chain borate ester, and an amino-masked long-chain siloxane in any ratio.

[0013] As a preferred technical solution, the molecular structure of the aluminum-zirconium organometallic complex is

[0014]

[0015] Where x, y, z = 1 to 100;

[0016] 2a+b+c=4;

[0017] d+e=2;

[0018] -OC(R2)O- ligand is a bridging ligand, and the bridging ligand is one of methacrylic acid, itaconic acid, adipic acid, and N,N′-dihydroxyethylglycine;

[0019] The molecular structure of nitrogen-containing long-chain borate ester is:

[0020]

[0021] The molecular structural formula of the amino concealing long-chain siloxane is:

[0022]

[0023] As a preferred technical solution, the grinding aid is one of triethanolamine and ethylene glycol;

[0024] or,

[0025] The grinding aid is a combination of triethanolamine and / or ethylene glycol with sodium aluminate in any proportion;

[0026] or,

[0027] The grinding aid is a combination of triethanolamine and / or ethylene glycol with water glass in any proportion.

[0028] As a preferred technical solution, the calcium carbonate powder and the solid waste powder are modified by a weightless mixer and mixed by a powerless mixer respectively.

[0029] The present invention also relates to a method for preparing a low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes, comprising the following steps:

[0030] SP A1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times the mass of the triethanolamine or the ethylene glycol to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, and add 15 to 23 times the mass of water to dilute for later use;

[0031] SP A2 , taking a mass fraction of the calcium carbonate ore and conveying it to a roller mill, and metering one of the triethanolamine and the ethylene glycol diluted with 15 to 23 times of water during the conveying process;

[0032] The solid waste powder is transported to a roller mill by mass, and a grinding aid prepared by mixing the triethanolamine, one of the ethylene glycols, and the sodium aluminate and the water glass in a ratio of 1:1 diluted with 15 to 23 times of water is added during the transportation process;

[0033] SP A3 , grinding the calcium carbonate ore with a roller mill to obtain calcium carbonate powder, and sending the calcium carbonate powder with a particle size meeting the requirements to a corresponding storage tank through a classifier;

[0034] Grinding the solid waste with a roller mill to obtain solid waste powder, and sending the solid waste powder with a particle size meeting the requirements to a corresponding storage tank through a classifier;

[0035] SP A4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes;

[0036] SP A5, transferring the calcium carbonate powder in the storage tank to the zero-gravity mixer, starting the zero-gravity mixer for stirring, and raising the temperature of the calcium carbonate powder to at least 90° C. during the stirring process, then uniformly adding a modifier to modify the calcium carbonate powder, the modifier addition time is controlled to be 40 to 60 seconds, and the speed of the zero-gravity mixer is controlled to be 50 to 70 rad / min during the addition of the modifier, and the temperature of the calcium carbonate powder after the addition of the modifier is maintained at not less than 90° C., and stirring is continued for 20 to 25 minutes, and the material is discharged and put into the raw material bin after being classified by a classifier to obtain modified calcium carbonate powder;

[0037] The solid waste powder in the storage tank is transferred to the zero-gravity mixer, the zero-gravity mixer is started for stirring, and the solid waste powder is heated to at least 90° C. during the stirring process, and then a modifier is uniformly added to modify the solid waste powder, the modifier addition time is controlled to be 40 to 60 seconds, and the speed of the zero-gravity mixer is controlled to be 50 to 70 rad / min during the addition of the modifier, and the temperature of the solid waste powder after the addition of the modifier is maintained at not less than 90° C., and stirring is continued for 20 to 25 minutes, and the material is discharged and put into the raw material bin after being classified by a classifier to obtain solid waste modified powder;

[0038] SP A6 , respectively transferring the calcium carbonate modified powder and the solid waste modified powder into the raw material bin of the unpowered mixer, starting the unpowered mixer to mix them evenly, and obtaining a composite low-cost powder.

[0039] The present invention also relates to another method for preparing a low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes, comprising the following steps:

[0040] SP B1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times the mass of the triethanolamine or the ethylene glycol to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, and add 15 to 23 times the mass of water to dilute for later use;

[0041] SP B2 , taking a mass fraction of the calcium carbonate ore and conveying it to a roller mill, and metering one of the triethanolamine and the ethylene glycol diluted with 15 to 23 times water during the conveying process;

[0042] The solid waste powder is transported to a roller mill by mass, and a grinding aid prepared by mixing the triethanolamine, one of the ethylene glycols, and the sodium aluminate and the water glass in a ratio of 1:1 diluted with 15 to 23 times water is added during the transportation process.

[0043] SP B3 , grinding the calcium carbonate ore with a roller mill to obtain calcium carbonate powder, and sending the calcium carbonate powder with a particle size meeting the requirements to a corresponding storage tank through a classifier;

[0044] Grinding the solid waste with a roller mill to obtain solid waste powder, and sending the solid waste powder with a particle size meeting the requirements to a corresponding storage tank through a classifier;

[0045] SP B4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes;

[0046] SP B5 , transferring the calcium carbonate powder and the solid waste powder into a weightless mixer according to the mass ratio, starting the weightless mixer for stirring, and heating the mixture of the calcium carbonate powder and the solid waste powder to at least 90° C. during the stirring process, during which the speed of the weightless mixer is controlled to be maintained at 50 to 70 rad / min;

[0047] SP B6 , adding the modifier in proportion by mass into the zero-gravity mixer, and controlling the adding time of the modifier to be 40 to 60 seconds;

[0048] SP B7 , maintaining the powder temperature in the zero-gravity mixer not lower than 90° C., continuing stirring for 20 to 25 minutes, discharging the powder and classifying it with a classifier to obtain a composite low-cost powder.

[0049] The present invention also relates to another method for preparing low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes, comprising the following steps:

[0050] SP C1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times of water to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, add 15 to 23 times of water to dilute for later use;

[0051] SP C2 , take the calcium carbonate ore and solid waste by mass and transport them to the roller mill, and add SP C1 Step-diluted grinding aid;

[0052] SP C3 , grinding the calcium carbonate ore and the solid waste by a roller mill to obtain a mixed powder, and sending the mixed powder with a particle size meeting the requirements into a storage tank through a classifier;

[0053] SP C4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes;

[0054] SP C5 , transferring the carbon mixed powder into a zero-gravity mixer, starting the zero-gravity mixer for stirring, and heating the mixed powder to at least 90° C. during the stirring process, during which the speed of the zero-gravity mixer is controlled to maintain at 50 to 70 rad / min;

[0055] SP C6 , adding the modifier in proportion by mass into the zero-gravity mixer, and controlling the adding time of the modifier to be 40 to 60 seconds;

[0056] SP C7 , maintaining the powder temperature in the zero-gravity mixer not lower than 90° C., continuing stirring for 20 to 25 minutes, discharging the powder and classifying it with a classifier to obtain a composite low-cost powder.

[0057] Due to the adoption of the above technical scheme, the present invention has the following beneficial effects: in the process of preparing polyolefin plastics for sewage pipes, solid waste, an extremely low-cost raw material, is used to compound and modify it with calcium carbonate, so that the cost of the composite calcium carbonate powder obtained by compounding is greatly reduced, and due to the change process experienced by the solid waste during the production process, the composite polyolefin filled with the solid waste and the calcium carbonate powder has higher performance and better processability. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] The following drawings are only intended to illustrate and explain the present invention, and are not intended to limit the scope of the present invention.

[0059] in:

[0060] Figure 1 is a SEM photo of calcium oxide solid waste produced in an embodiment of the present invention;

[0061] Figure 2 It is a reference diagram of the mechanism of action of the aluminum-zirconium coupling agent according to an embodiment of the present invention;

[0062] Figure 3 This is a schematic diagram of the layout of a powder mixing device according to an embodiment of the present invention;

[0063] Figure 4 It is a linear graph of the rheological properties influence test of test examples 1 to 6 of the embodiment of the present invention and comparative examples 1 to 2;

[0064] In the figure: 1-unpowered mixer; 101-first-stage diversion mixing bin; 102-second-stage diversion mixing bin; 103-third-stage diversion mixing bin; 104-first-stage Huirong mixing bin; 105-second-stage Huirong mixing bin; 106-discharging port; 107-unpowered mixer bin body; 108-feeding port; 109-hollow cone; 110-mixing bin; 2-raw material bin one; 3-raw material bin two; 4-raw material bin three; 5-raw material bin four; 6-loss-in-weight scale one; 7-loss-in-weight scale two; 8-elevator one; 9-elevator two; 10-auger one; 11-auger two; 12-auger three; 13-auger four. DETAILED DESCRIPTION

[0065] The present invention is further described below in conjunction with the accompanying drawings and examples. In the following detailed description, certain exemplary embodiments of the present invention are described only by way of illustration. Needless to say, those of ordinary skill in the art will recognize that the described embodiments may be modified in various ways without departing from the spirit and scope of the present invention. Therefore, the drawings and description are illustrative in nature and are not intended to limit the scope of protection of the claims.

[0066] A low-cost powder composited with calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes, mainly used for processing and producing polyolefin plastics for sewage pipes. Specifically, it includes the following components in proportion by mass: 50-80 parts of calcium carbonate powder and 20-50 parts of solid waste powder; the calcium carbonate powder and the solid waste powder are modified by modifiers respectively, and the amount of the modifier used when the calcium carbonate powder is modified is 0.7-1.2% of its mass; the amount of the modifier used when the solid waste powder is modified is 0.7-1.2% of its mass; the calcium carbonate powder is obtained by processing calcium carbonate ore, and a grinding aid needs to be added when producing the calcium carbonate powder, and the amount of the grinding aid is 1-2‰ of the mass of the calcium carbonate ore; the solid waste powder is obtained by processing solid waste, and the grinding aid also needs to be added when producing the solid waste powder, and the amount of the grinding aid is 1-2‰ of the mass of the solid waste. The calcium carbonate ore is formed into calcium carbonate powder by a ring roller mill, and the particle size of the calcium carbonate powder is 11.600 μm ≤ D according to the particle size tester of OMEC. 97 ≤20.300μm; the solid waste includes one of the solid waste from calcium oxide production, steelmaking solid waste, and glass fiber reinforced plastic scrap solid waste; the solid waste is ground by a roller mill to obtain solid waste powder, and the particle size of the solid waste powder detected by an OMEC particle size tester is 9.800μm≤D 97 ≤18.900μm. The maximum size of the calcium carbonate ore and the solid waste is ≤35mm.

[0067] Solid waste from calcium oxide production and steelmaking has mostly undergone high-temperature processing, while solid waste from fiberglass scrap has undergone a series of changes during processing, such as cross-linking. After a series of processes, the original structure of the solid waste will change to a certain extent. These changes will have an immeasurable impact on its application. For example, the presence of fibers in solid waste from calcium oxide production (such as Figure 1 shown) etc.

[0068] At the same time, since one of the compound raw materials is solid waste, these solid wastes can basically be obtained free of charge. Even the enterprises that generate solid wastes need to give certain economic compensation to the units that use them in order to dispose of them. Therefore, the impact of grinding these solid wastes into solid waste powders and then compounding them with powders ground from calcium carbonate ore on the cost of production raw materials is obvious.

[0069] The modifier is a combination of two or more of an aluminum-zirconium organic metal complex, a nitrogen-containing long-chain borate, and an amino-covered long-chain siloxane in any ratio, and preferably two of the components are selected to form the modifier. The molecular structure of the aluminum-zirconium organic metal complex is Where x, y, z = 1 to 100, 2a + b + c = 4, d + e = 2, It is an organic ligand that affects the hydroxyl stability and hydrolysis stability. The -OC(R2)O- ligand is a bridging ligand that imparts good reactivity. The bridging ligand is one of methacrylic acid, itaconic acid, adipic acid, and N,N′-dihydroxyethylglycine.

[0070] The mechanism of action of the aluminum-zirconium coupling agent is as follows: the aluminum-zirconium organic metal complex is composed of three parts: a zirconium skeleton, an aluminum skeleton and an organic functional group ligand. This structural feature gives it a series of characteristics. ① It can achieve stable chemical bonding with inorganic surfaces or metal surfaces. The active hydroxyl groups bound to the metal center (Zr, Al) can undergo condensation with the hydroxylated inorganic surface; ② The percentage of inorganic properties is high, about 75%, which is much higher than the 40% or less of silane coupling agents and the 15% or less of titanate coupling agents; ③ The organic functional groups form an electrostatic bond with the negative charge on the polymer reaction surface. Due to the dual effects of coupling and bridging with positive charges, a strong bond is formed between materials that originally had no bonding force. The mechanism of action is as follows: Figure 2 shown.

[0071] The molecular structure of nitrogen-containing long-chain borate ester is:

[0072]

[0073] The molecular structural formula of the amino concealing long-chain siloxane is:

[0074]

[0075] The nitrogen-containing long-chain borate contains an isopropyl group (-OCH(CH3)2) and an imide group (-CONH) with certain activity; although there is no obvious amino group (-NH2) in the amino-hidden long-chain siloxane, the imide group (-CONH) generated by the reaction still retains the activity of the amino group (-NH2), although the activity is reduced. At the same time, there are three methoxy (-OCH3) active groups in the structure. The presence of these active groups, especially the isopropyl group (-OCH(CH3)2) and the methoxy group (-OCH3). The presence of these active groups reacts with the hydroxyl group (-OH) on the surface of the powder to produce a strong bond, and the long carbon chain contained provides the possibility of polymer entanglement.

[0076] The grinding aid is one of triethanolamine and ethylene glycol; or, the grinding aid is a combination of triethanolamine or / and ethylene glycol with sodium aluminate in any ratio; or, the grinding aid is a combination of triethanolamine or / and ethylene glycol with water glass in any ratio. Preferably, the grinding aid is a combination of triethanolamine or / and ethylene glycol with water glass or sodium aluminate in a 1:1 ratio, and when used, the grinding aid needs to be diluted with 15 to 23 times the amount of water.

[0077] The mechanism of action of the grinding aid is:

[0078] ① Grinding aid molecules adsorb on the surface of particles to reduce the surface energy of the ore, causing surface point defects or defects, thereby reducing the hardness of the ore. At the same time, they adsorb inside new cracks to compensate for the unsaturated bond energy inside them, saturating their valence bond forces, thereby promoting the dispersion of ore particles, effectively preventing the merging of new cracks, and reducing the energy required for crack expansion, thereby promoting crack expansion; ② Grinding aids can affect the rheological properties of slurry and improve the fluidity of slurry. The dispersion of ore particles and the fluidity of slurry are related to the viscosity of slurry. Grinding aids can reduce the viscosity of slurry, thereby improving the agglomeration of ore particles and their adsorption on the inner surface of the mill; ③ Grinding aids form a molecular-thick lubricating film on the surface of ore particles, significantly reducing the friction resistance between ore particles, and also increasing the double-layer repulsion energy between ore particles, making them repel each other, so that fine particles are not easy to aggregate, thereby improving the grinding effect.

[0079] Studies have shown that the combined use of organic and inorganic grinding aids, especially for solid waste grinding, can make the powder finer and the production efficiency higher due to the unpredictability of solid waste.

[0080] The calcium carbonate powder and the solid waste powder are modified by a weightless mixer and mixed by a powerless mixer. Figure 3As shown, the unpowered mixer 1 includes an unpowered mixer chamber 107, and a plurality of mixing chambers 110 arranged from top to bottom are arranged in the unpowered mixer chamber 107. Specifically, a primary flow-dividing mixing chamber 101 formed by one mixing chamber 110, a secondary flow-dividing mixing chamber 102 composed of two mixing chambers 110, a tertiary flow-dividing mixing chamber 103 composed of four mixing chambers 110, a primary flow-receiving mixing chamber 104 composed of two mixing chambers 110, and a secondary flow-receiving mixing chamber 105 composed of one mixing chamber 110. A feed port 108 is provided at the top of the primary flow-dividing mixing chamber 101, and the feed port 108 is in a "Y" structure. The two feed ports of the two secondary flow-dividing and mixing bins 102 are respectively connected to the discharge port of the primary flow-dividing and mixing bin 101, two of the feed ports of the four tertiary flow-dividing and mixing bins 103 are connected to the discharge port of one of the secondary flow-dividing and mixing bins 102, and the other two feed ports are connected to the discharge port of another secondary flow-dividing and mixing bin 102, each of the primary confluence and mixing bins 104 is respectively connected to the discharge port of the two tertiary flow-dividing and mixing bins 103, and the feed port of the secondary confluence and mixing bin 105 is connected to the two primary confluence and mixing bins 104. A discharge port 106 is provided at the bottom of the secondary confluence and mixing bin 105, and a discharge motor is installed below the discharge port 106, and a hollow cone 109 is installed in each mixing bin 110 just below the feed port.

[0081] The bottom of the raw material bin 1 2 and the raw material bin 2 3 is provided with a discharge port, which is connected to the auger 3 12 and the auger 4 13 through the discharge motor. The auger 3 12 and the auger 4 13 are respectively connected to the motor at one end, and the other end is connected to the feed port of the elevator 1 8 and the elevator 2 9. The discharge ports of the elevator 1 8 and the elevator 2 9 are respectively connected to the raw material bin 3 4 and the raw material bin 4 5. The loss-in-weight scale 1 6 and the loss-in-weight scale 2 7 are respectively provided with a hopper, and a barrel is provided under the hopper. A screw is installed in the barrel. A motor is installed at one end of the two barrels, and the other end is respectively connected to the "Y"-shaped structure of the feed port 108. The auger 10 and the auger 2 11 are respectively connected to the raw material bin 3 4 and the hopper of the loss-in-weight scale 1 6, and the raw material bin 4 5 and the hopper of the loss-in-weight scale 2 7.

[0082] Method 1 for preparing low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes, comprising the following steps:

[0083] SP A1, take the triethanolamine or the ethylene glycol at a mass ratio of one thousandth of the calcium carbonate ore, add 15 to 23 times the mass of the triethanolamine or the ethylene glycol in water to dilute for later use; take the triethanolamine or one of the ethylene glycol at a mass ratio of one thousandth of the solid waste powder and mix with the water glass or the sodium aluminate in a ratio of 1:1, and add 15 to 23 times the mass of water to dilute for later use.

[0084] SP A2 , taking a mass fraction of the calcium carbonate ore and conveying it to a roller mill, and during the conveying process, meteringly adding one of the triethanolamine and the ethylene glycol diluted with 15 to 23 times of water.

[0085] The solid waste powder is transported to a roller mill by mass, and a grinding aid prepared by mixing the triethanolamine, one of the ethylene glycols, and the sodium aluminate and the water glass in a ratio of 1:1 diluted with 15 to 23 times water is metered into the grinding aid during the transportation process.

[0086] SP A3 , grinding the calcium carbonate ore with a ring roller mill to obtain calcium carbonate powder, and sending the calcium carbonate powder with a particle size that meets the requirements to a corresponding storage tank through a classifier; grinding the solid waste with a ring roller mill to obtain solid waste powder, and sending the solid waste powder with a particle size that meets the requirements to a corresponding storage tank through a classifier.

[0087] SP A4 , raise the temperature of the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes.

[0088] SP A5 , transfer the calcium carbonate powder in the storage tank to the zero-gravity mixer, start the zero-gravity mixer for stirring, and raise the temperature of the calcium carbonate powder to at least 90°C during the stirring process, then evenly add a portion of the modifier to modify the calcium carbonate powder, the modifier addition time is controlled to be 40 to 60 seconds, and the speed of the zero-gravity mixer is controlled to be 50 to 70 rad / min during the addition of the modifier, and the temperature of the calcium carbonate powder after the addition of the modifier is maintained at not less than 90°C, and stirring is continued for 20 to 25 minutes, and the material is discharged and classified by a classifier and then placed in a raw material bin 2 to obtain modified calcium carbonate powder.

[0089] The solid waste powder in the storage tank is transferred to the zero-gravity mixer, the zero-gravity mixer is started for stirring, and the solid waste powder is heated to at least 90°C during the stirring process, and then the remaining amount of the modifier is evenly added to modify the solid waste powder. The time for adding the modifier is controlled to be 40 to 60 seconds. During the addition of the modifier, the speed of the zero-gravity mixer is controlled to be 50 to 70 rad / min. The temperature of the solid waste powder after the addition of the modifier is maintained at not less than 90°C, and stirring is continued for 20 to 25 minutes. The material is discharged and classified by a classifier and then placed in a raw material bin 23 to obtain solid waste modified powder.

[0090] SP A6 , transfer the modified calcium carbonate powder and the modified solid waste powder to the raw material bin 3 4 and the raw material bin 4 5 respectively, start the auger 1 10, the weight loss scale 1 6, the auger 2 11, and the weight loss scale 2 7, so that the modified calcium carbonate powder and the solid waste powder are evenly mixed in the unpowered mixer 1 to obtain a composite low-cost powder. The unpowered mixer 1 uses the gravity of the powder and the diversion effect of the hollow cone 109 to complete the automatic mixing of materials, specifically:

[0091] Start the auger three 12 to send the modified calcium carbonate powder from the raw material bin 2 into the elevator 1 8, and the elevator 1 8 sends the modified calcium carbonate powder to the raw material bin three 4; start the auger four 13 to send the solid waste modified powder from the raw material bin two 3 into the elevator two 9, and the elevator two 9 sends the solid waste modified powder to the raw material bin four 5. The modified calcium carbonate powder in the raw material bin three 4 is fed into the loss-in-weight scale one 6 through the auger one 10, and the loss-in-weight scale one 6 sets the flow rate according to the ratio, and feeds the modified calcium carbonate powder into the primary diversion mixing bin 101 through the feed port 108; the modified solid waste powder in the raw material bin four 5 is fed into the loss-in-weight scale two 7 through the auger two 11, and the loss-in-weight scale two 7 sets the flow rate according to the ratio, and feeds the modified solid waste powder into the primary diversion mixing bin 101 through the feed port 108. The hollow cone 109 arranged in the first-level diversion mixing bin 101 allows the calcium carbonate modified powder or the solid waste modified powder flowing in to be diverted and mixed below the hollow cone 109, and then flows from the first-level diversion mixing bin 101 through the second-level diversion mixing bin 102 and the third-level diversion mixing bin 103 in sequence to achieve dispersion, mixing, redispersion and remixing of the powder; then the diversion flows into the two first-level confluence mixing bins 104 for confluence, and finally converges into the second-level confluence mixing bin 105. In this process, the mixed material changes from dispersion to convergence, and at the same time, uniform mixing is achieved under the action of each hollow cone 109; finally, the mixed composite powder is discharged through the discharge port 106 to form a finished product.

[0092] The second method for preparing low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes in this embodiment comprises the following steps:

[0093] SP B1 , take the triethanolamine or the ethylene glycol at a mass ratio of one thousandth of the calcium carbonate ore, add 15 to 23 times the mass of the triethanolamine or the ethylene glycol in water to dilute for later use; take the triethanolamine or one of the ethylene glycol at a mass ratio of one thousandth of the solid waste powder and mix with the water glass or the sodium aluminate in a ratio of 1:1, and add 15 to 23 times the mass of water to dilute for later use.

[0094] SP B2 , taking a mass fraction of the calcium carbonate ore and conveying it to a roller mill, and metering one of the triethanolamine and the ethylene glycol diluted with 15 to 23 times water during the conveying process;

[0095] The solid waste powder is transported to a roller mill by mass, and a grinding aid prepared by mixing the triethanolamine, one of the ethylene glycols, and the sodium aluminate and the water glass in a ratio of 1:1 diluted with 15 to 23 times water is added during the transportation process.

[0096] SP B3 , Grind the calcium carbonate ore with a ring roller mill to obtain calcium carbonate powder, and send the calcium carbonate powder with a particle size that meets the requirements to a corresponding storage tank through a classifier. Grind the solid waste with a ring roller mill to obtain solid waste powder, and send the solid waste powder with a particle size that meets the requirements to a corresponding storage tank through a classifier.

[0097] SP B4 , raise the temperature of the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes.

[0098] SP B5 , respectively transfer the calcium carbonate powder and the solid waste powder into a weightless mixer, start the weightless mixer for stirring, and during the stirring process, heat the calcium carbonate powder and the solid waste powder to at least 90° C., during which the speed of the weightless mixer is controlled to remain at 50-70 rad / min.

[0099] SP B6 , add the modifier in the weightless mixer in the mass proportion, and control the adding time of the modifier to be 40 to 60 seconds. In this step, the modifier is two of the aluminum-zirconium organometallic complex, nitrogen-containing long-chain borate, and amino-hidden long-chain siloxane, which are compounded in a 1:1 ratio and added to the weightless mixer.

[0100] SP B7 , maintaining the powder temperature in the zero-gravity mixer not lower than 90° C., continuing stirring for 20 to 25 minutes, discharging the powder and classifying it with a classifier to obtain a composite low-cost powder.

[0101] The third method for preparing low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes in this embodiment comprises the following steps:

[0102] SP C1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times of water to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, add 15 to 23 times of water to dilute for later use;

[0103] SP C2 , take the calcium carbonate ore and solid waste by mass and transport them to the roller mill, and add SP C1 Step-diluted grinding aid;

[0104] SP C3, grinding the calcium carbonate ore and the solid waste by a roller mill to obtain a mixed powder, and sending the mixed powder with a particle size meeting the requirements into a storage tank through a classifier;

[0105] SP C4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes;

[0106] SP C5 , transferring the carbon mixed powder into a zero-gravity mixer, starting the zero-gravity mixer for stirring, and heating the mixed powder to at least 90° C. during the stirring process, during which the speed of the zero-gravity mixer is controlled to maintain at 50 to 70 rad / min;

[0107] SP C6 , adding the modifier in proportion by mass into the zero-gravity mixer, and controlling the adding time of the modifier to be 40 to 60 seconds;

[0108] SP C7 , maintaining the powder temperature in the zero-gravity mixer not lower than 90° C., continuing stirring for 20 to 25 minutes, discharging the powder and classifying it with a classifier to obtain a composite low-cost powder.

[0109] The third method for preparing the low-cost composite powder of calcium carbonate and solid waste for polyolefin plastic sewage pipes in this embodiment is different from the second method in that the raw materials and additives used in steps one and two of the second method are placed together in a roller mill to grind the raw materials.

[0110] The present invention is further described below with specific examples.

[0111] The mixed powder formed by the calcium carbonate powder and the solid waste powder in each embodiment has a particle size of 11.917 μm ≤ D 97 1000 mesh powder ≤12.381μm.

[0112] Example 1

[0113] Using preparation method 1.

[0114] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the weight of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the weight of the solid waste.

[0115] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0116] In this embodiment:

[0117] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11.

[0118] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12.

[0119] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13.

[0120] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 80:20 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14.

[0121] Example 2

[0122] Using preparation method 2.

[0123] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0124] ① The calcium carbonate powder and the solid waste powder for producing calcium oxide are placed into the weightless mixer in a mass ratio of 50:50. The modifier is a compound of amino-masked long-chain siloxane and aluminum-zirconium organometallic complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder, and the amount of aluminum-zirconium organometallic complex is 1% of the mass of the solid waste powder. The bridging ligand of the aluminum-zirconium organometallic complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC21.

[0125] ② The calcium carbonate powder and the solid waste powder for producing calcium oxide are placed into the weightless mixer in a mass ratio of 60:40. The modifier is a compound of amino-masked long-chain siloxane and aluminum-zirconium organometallic complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder, and the amount of aluminum-zirconium organometallic complex is 1% of the mass of the solid waste powder. The bridging ligand of the aluminum-zirconium organometallic complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC22.

[0126] ③ The calcium carbonate powder and the solid waste powder for producing calcium oxide are placed into the weightless mixer in a mass ratio of 70:30. The modifier is a compound of amino-masked long-chain siloxane and aluminum-zirconium organometallic complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder, and the amount of aluminum-zirconium organometallic complex is 1% of the mass of the solid waste powder. The bridging ligand of the aluminum-zirconium organometallic complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC23.

[0127] ④ The calcium carbonate powder and the solid waste powder for producing calcium oxide are placed into the weightless mixer in a mass ratio of 80:20. The modifier is a compound of amino-masked long-chain siloxane and aluminum-zirconium organometallic complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder, and the amount of aluminum-zirconium organometallic complex is 1% of the mass of the solid waste powder. The bridging ligand of the aluminum-zirconium organometallic complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC24.

[0128] Example 3

[0129] Utilize preparation method three.

[0130] ① The calcium carbonate ore and the solid waste are ground in a ratio of 50:50 by mass, the solid waste is solid waste from the production of calcium oxide, the grinding aid added when grinding the calcium carbonate ore is triethanolamine and is added at 1.5‰ of the mass of the calcium carbonate ore, the grinding aids added when grinding the calcium oxide solid waste are ethylene glycol and water glass, and ethylene glycol is mixed at 0.75‰ of the mass of the calcium oxide solid waste and water glass is mixed at 0.75‰ of the mass of the calcium oxide solid waste. The calcium carbonate ore and the calcium oxide solid waste are ground into powder and then put into the weightless mixer. The modifier is a compound of amino-masked long-chain siloxane and aluminum-zirconium organic metal complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder after grinding. The amount of aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder after grinding. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC31.

[0131] ② The calcium carbonate ore and the calcium oxide solid waste are ground in a mass ratio of 60:40. The grinding aid added when grinding the calcium carbonate ore is triethanolamine and is added at 1.5‰ of the mass of the calcium carbonate ore. The grinding aid added when grinding the calcium oxide solid waste is ethylene glycol and water glass, and ethylene glycol is 0.75‰ of the mass of the calcium oxide solid waste and water glass is 0.75‰ of the mass of the calcium oxide solid waste. The calcium carbonate ore and the calcium oxide solid waste are ground and put into the zero-gravity mixer. The modifier is a combination of amino-masked long-chain siloxane and aluminum-zirconium organic metal complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder after grinding, and the amount of aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder after grinding. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC32.

[0132] ③ The calcium carbonate ore and the calcium oxide solid waste are ground in a mass ratio of 70:30. The grinding aid added when the calcium carbonate ore is ground is triethanolamine and is added at 1.5‰ of the mass of the calcium carbonate ore. The grinding aid added when the calcium oxide solid waste is ground is ethylene glycol and water glass, and ethylene glycol is 0.75‰ of the mass of the calcium oxide solid waste and water glass is 0.75‰ of the mass of the calcium oxide solid waste. The calcium carbonate ore and the calcium oxide solid waste are ground and put into the zero-gravity mixer. The modifier is a combination of amino-masked long-chain siloxane and aluminum-zirconium organic metal complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder after grinding, and the amount of aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder after grinding. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC33.

[0133] ④ The calcium carbonate ore and the calcium oxide solid waste are ground in a mass ratio of 80:20. The grinding aid added when grinding the calcium carbonate ore is triethanolamine and is added at 1.5‰ of the weight of the calcium carbonate ore. The grinding aid added when grinding the calcium oxide solid waste is ethylene glycol and water glass, and ethylene glycol is 0.75‰ of the mass of the calcium oxide solid waste and water glass is 0.75‰ of the mass of the calcium oxide solid waste. The calcium carbonate ore and the calcium oxide solid waste are ground and put into the zero-gravity mixer. The modifier is a combination of amino-masked long-chain siloxane and aluminum-zirconium organic metal complex. The amount of amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder after grinding, and the amount of aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder after grinding. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid. The obtained composite low-cost powder is recorded as CC34.

[0134] Example 4

[0135] Using preparation method 1.

[0136] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0137] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is N,N′-dihydroxyethylglycine.

[0138] In this embodiment:

[0139] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-1.

[0140] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-1.

[0141] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-1.

[0142] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 80:20 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-1.

[0143] Example 5

[0144] Using preparation method 1.

[0145] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1‰ of the mass of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1‰ of the mass of the solid waste.

[0146] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0147] In this embodiment:

[0148] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-2.

[0149] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-2.

[0150] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a weight ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-2.

[0151] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-2.

[0152] Example 6

[0153] Using preparation method 1.

[0154] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 2‰ of the mass of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 2‰ of the mass of the solid waste.

[0155] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0156] In this embodiment:

[0157] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-3.

[0158] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-3.

[0159] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-3.

[0160] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-3.

[0161] Example 7

[0162] Using preparation method 1.

[0163] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0164] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 0.8% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 0.8% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0165] In this embodiment:

[0166] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-4.

[0167] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-4.

[0168] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-4.

[0169] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-4.

[0170] Example 8

[0171] Using preparation method 1.

[0172] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0173] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1.2% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1.2% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0174] In this embodiment:

[0175] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-5.

[0176] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-5.

[0177] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a weight ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-5.

[0178] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-5.

[0179] Example 9

[0180] Using preparation method 1.

[0181] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is solid waste produced from the production of calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and sodium aluminate, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0182] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder for producing calcium oxide is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder for producing calcium oxide. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0183] In this embodiment:

[0184] ① The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a ratio of 50:50 by mass using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-6.

[0185] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-6.

[0186] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a weight ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-6.

[0187] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-6.

[0188] Example 10

[0189] Using preparation method 1.

[0190] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the weight of the calcium carbonate ore; the solid waste is solid waste from producing calcium oxide, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the weight of the solid waste.

[0191] The modifier used in the modification of the calcium carbonate powder is the nitrogen-containing long-chain borate, and the amount of the nitrogen-containing long-chain borate is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the solid waste powder produced by calcium oxide production is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the solid waste powder. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0192] In this embodiment:

[0193] ① The modified calcium carbonate powder and the calcium oxide production solid waste powder are mixed in a mass ratio of 50:50 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC11-7.

[0194] ② The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC12-7.

[0195] ③ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a weight ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC13-7.

[0196] ④ The modified calcium carbonate powder and the solid waste powder from calcium oxide production are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CC14-7.

[0197] Embodiment 11

[0198] Using preparation method 1.

[0199] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is steelmaking solid waste, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0200] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the glass fiber reinforced plastic scrap solid waste powder is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the glass fiber reinforced plastic scrap solid waste powder. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0201] In this embodiment:

[0202] ① The modified calcium carbonate powder and the steelmaking solid waste powder are mixed in a mass ratio of 50:50 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CS11.

[0203] ② The modified calcium carbonate powder and the steelmaking solid waste powder are mixed in a mass ratio of 60:40 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CS12.

[0204] ③ The modified calcium carbonate powder and the steelmaking solid waste powder are mixed in a mass ratio of 70:30 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CS13.

[0205] ④ The modified calcium carbonate powder and the steelmaking solid waste powder are mixed in a mass ratio of 80:20 using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CS14.

[0206] Example 12

[0207] Using preparation method 1.

[0208] The grinding aid used when grinding the calcium carbonate ore is triethanolamine, and the amount used is 1.5‰ of the mass of the calcium carbonate ore; the solid waste is fiberglass scrap solid waste, and the grinding aid used when grinding the solid waste is a compound of ethylene glycol and water glass, the compound ratio of the two is 1:1, and the amount used is 1.5‰ of the mass of the solid waste.

[0209] The modifier used in the modification of the calcium carbonate powder is the amino-masked long-chain siloxane, and the amount of the amino-masked long-chain siloxane is 1% of the mass of the calcium carbonate powder. The modifier used in the modification of the glass fiber reinforced plastic scrap solid waste powder is an aluminum-zirconium organic metal complex, and the amount of the aluminum-zirconium organic metal complex is 1% of the mass of the glass fiber reinforced plastic scrap solid waste powder. The bridging ligand of the aluminum-zirconium organic metal complex is methyl acrylic acid.

[0210] In this embodiment:

[0211] ① The calcium carbonate powder and the FRP scrap solid waste powder are modified in a ratio of 50:50 by mass and mixed using the unpowered mixer to obtain a composite low-cost powder, which is denoted as CG11.

[0212] ② The calcium carbonate powder and the FRP scrap solid waste powder are modified in a mass ratio of 60:40 and mixed using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CG12.

[0213] ③ The calcium carbonate powder and the FRP scrap solid waste powder are modified in a mass ratio of 70:30 and mixed using the unpowered mixer to obtain a composite low-cost powder, which is recorded as CG13.

[0214] ④ The calcium carbonate powder and the FRP scrap solid waste powder are modified in a weight ratio of 80:20 and mixed using the unpowered mixer to obtain a composite low-cost powder, which is denoted as CG14.

[0215] For the use of the composite low-cost powder obtained by the present invention for filling and modifying polyolefins, the overall trend of the performance change of the filled and modified polyolefins is consistent. The following only describes the performance change of the powder-filled polyolefins recorded as CC11, CC12, CC13, CC14, CS12, and CG12 to further test the present invention.

[0216] ① The test uses 30% composite low-cost powder filling;

[0217] ②The performance test adopts the description of powder filling PP;

[0218] ③ Test ratio: PP (045): PP (K8303): POE (8150): composite powder = 57:8:5:30, with appropriate amount of antioxidant.

[0219] Test Example 1

[0220] The composite powder adopts CC11.

[0221] Test Example 2

[0222] The composite powder adopts CC12.

[0223] Test Example 3

[0224] The composite powder adopts CC13.

[0225] Test Example 4

[0226] The composite powder is CC14.

[0227] Test Example 5

[0228] The composite powder adopts CS13.

[0229] Test Example 6

[0230] The composite powder adopts CG13.

[0231] Comparative Example 1

[0232] The powder is modified calcium carbonate powder.

[0233] Comparative Example 2

[0234] The powder is calcium oxide solid waste powder.

[0235] The mechanical properties test results of the test examples and comparative examples are shown in Table 1:

[0236] Table 1

[0237]

[0238]

[0239] The rheological properties of test examples 1 to 6 and comparative examples 1 to 2 are shown in Figure 4 It can be seen that after the mixing ratio of calcium carbonate powder and solid waste powder of calcium oxide production exceeds 80:20, as the mixing ratio of calcium oxide solid waste powder increases, it and calcium carbonate powder have a synergistic effect of improving the mechanical properties of polyolefins. When the calcium carbonate powder tested at the same time is mixed with steelmaking solid waste powder and FRP scrap solid waste powder in a ratio of 70:30 to form a composite powder filling, it also has higher mechanical properties than pure calcium carbonate powder when filled; rheological tests also show that the apparent viscosity of the filled polyolefin decreases when the above solid waste powder is added, indicating that it is easy to process and also has a synergistic effect. For the production of calcium oxide solid waste, steelmaking solid waste and FRP scrap solid waste, these raw materials can be obtained free of charge, and even the provider needs to pay a certain amount of solid waste treatment fees. Therefore, the cost after having solid waste powder is much lower than the cost of using calcium carbonate powder alone. In addition, the sewage pipes are all black products, which are not selective for the color of the powder, so that the composite powder has the advantages of low cost, good filling mechanical properties, and easy processing.

[0240] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.

Claims

1. A low-cost powder composited with calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes, characterized in that: The invention comprises the following components in proportion by weight: 50 to 80 parts of calcium carbonate powder and 20 to 50 parts of solid waste powder; The calcium carbonate powder and the solid waste powder are modified by a modifier respectively, wherein the amount of the modifier used in the modification of the calcium carbonate powder is 0.7-1.2% of its mass; and the amount of the modifier used in the modification of the solid waste powder is 0.7-1.2% of its mass; The calcium carbonate powder is obtained by processing calcium carbonate ore. When producing the calcium carbonate powder, a grinding aid needs to be added. The amount of the grinding aid is 1-2‰ of the mass of the calcium carbonate ore. The solid waste powder is obtained by processing solid waste. The grinding aid also needs to be added when producing the solid waste powder. The amount of the grinding aid is 1 to 2‰ of the mass of the solid waste.

2. The low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipe according to claim 1, characterized in that: The calcium carbonate ore is formed into calcium carbonate powder by a ring roller mill, and the particle size of the calcium carbonate powder is 11.600 μm ≤ D 97 ≤20.300μm; The solid waste includes one of the solid wastes from calcium oxide production, steelmaking, and fiberglass scrap solid waste; The solid waste is ground by a roller mill to obtain solid waste powder, and the particle size of the solid waste powder detected by an OMEC particle size tester is 9.800 μm≤D 97 ≤18.900μm; The maximum size of the calcium carbonate ore and the solid waste is ≤35mm.

3. The low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipe according to claim 1, characterized in that: The modifier is a combination of two or more of an aluminum-zirconium organic metal complex, a nitrogen-containing long-chain borate ester, and an amino-hidden long-chain siloxane in any proportion.

4. The low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipe according to claim 3, characterized in that: The molecular structure of the aluminum-zirconium organometallic complex is Where x, y, z = 1 to 100; 2a+b+c=4; d+e=2; -OC(R2)O- ligand is a bridging ligand, and the bridging ligand is one of methacrylic acid, itaconic acid, adipic acid, and N,N′-dihydroxyethylglycine; The molecular structure of nitrogen-containing long-chain borate ester is: The molecular structural formula of the amino concealing long-chain siloxane is:

5. The low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipe according to claim 1, characterized in that: The grinding aid is one of triethanolamine and ethylene glycol; or, The grinding aid is a combination of triethanolamine and / or ethylene glycol with sodium aluminate in any ratio; or, The grinding aid is a combination of triethanolamine and / or ethylene glycol with water glass in any proportion.

6. The low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipe according to claim 1, characterized in that: The calcium carbonate powder and the solid waste powder are modified by a weightless mixer and mixed by a powerless mixer respectively.

7. The method for preparing a low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes according to claim 5, characterized in that: The following steps are included: SP A1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times the mass of the triethanolamine or the ethylene glycol to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, and add 15 to 23 times the mass of water to dilute for later use; SP A2 , taking a mass fraction of the calcium carbonate ore and conveying it to a roller mill, and metering one of the triethanolamine and the ethylene glycol diluted with 15 to 23 times of water during the conveying process; The solid waste powder is transported to a roller mill by mass, and a grinding aid prepared by mixing the triethanolamine, one of the ethylene glycols, and the sodium aluminate and the water glass in a ratio of 1:1 diluted with 15 to 23 times of water is added during the transportation process; SP A3 , grinding the calcium carbonate ore with a roller mill to obtain calcium carbonate powder, and sending the calcium carbonate powder with a particle size meeting the requirements to a corresponding storage tank through a classifier; Grinding the solid waste with a roller mill to obtain solid waste powder, and sending the solid waste powder with a particle size meeting the requirements to a corresponding storage tank through a classifier; SP A4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes; SP A5 , transferring the calcium carbonate powder in the storage tank to the zero-gravity mixer, starting the zero-gravity mixer for stirring, and raising the temperature of the calcium carbonate powder to at least 90° C. during the stirring process, then uniformly adding a modifier to modify the calcium carbonate powder, the modifier addition time is controlled to be 40 to 60 seconds, and the speed of the zero-gravity mixer is controlled to be 50 to 70 rad / min during the addition of the modifier, and the temperature of the calcium carbonate powder after the addition of the modifier is maintained at not less than 90° C., and stirring is continued for 20 to 25 minutes, and the material is discharged and put into the raw material bin after being classified by a classifier to obtain modified calcium carbonate powder; The solid waste powder in the storage tank is transferred to the zero-gravity mixer, the zero-gravity mixer is started for stirring, and the solid waste powder is heated to at least 90° C. during the stirring process, and then a modifier is uniformly added to modify the solid waste powder, the modifier addition time is controlled to be 40 to 60 seconds, and the speed of the zero-gravity mixer is controlled to be 50 to 70 rad / min during the addition of the modifier, and the temperature of the solid waste powder after the addition of the modifier is maintained at not less than 90° C., and stirring is continued for 20 to 25 minutes, and the material is discharged and put into the raw material bin after being classified by a classifier to obtain solid waste modified powder; SP A6 , respectively transferring the calcium carbonate modified powder and the solid waste modified powder into the raw material bin of the unpowered mixer, starting the unpowered mixer to mix them evenly, and obtaining a composite low-cost powder.

8. The method for preparing a low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes according to claim 5, characterized in that: The following steps are included: SP B1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times the mass of the triethanolamine or the ethylene glycol to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, and add 15 to 23 times the mass of water to dilute for later use; SP B2 , taking a mass fraction of the calcium carbonate ore and conveying it to a roller mill, and metering one of the triethanolamine and the ethylene glycol diluted with 15 to 23 times water during the conveying process; The solid waste powder is transported to a roller mill by mass, and a grinding aid prepared by mixing the triethanolamine, one of the ethylene glycols, and the sodium aluminate and the water glass in a ratio of 1:1 diluted with 15 to 23 times water is added during the transportation process. SP B3 , grinding the calcium carbonate ore with a roller mill to obtain calcium carbonate powder, and sending the calcium carbonate powder with a particle size meeting the requirements to a corresponding storage tank through a classifier; Grinding the solid waste with a roller mill to obtain solid waste powder, and sending the solid waste powder with a particle size meeting the requirements to a corresponding storage tank through a classifier; SP B4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes; SP B5 , transferring the calcium carbonate powder and the solid waste powder into a weightless mixer according to the mass ratio, starting the weightless mixer for stirring, and heating the mixture of the calcium carbonate powder and the solid waste powder to at least 90° C. during the stirring process, during which the speed of the weightless mixer is controlled to be maintained at 50 to 70 rad / min; SP B6 , adding the modifier in proportion by mass into the zero-gravity mixer, and controlling the adding time of the modifier to be 40 to 60 seconds; SP B7 , maintaining the powder temperature in the zero-gravity mixer not lower than 90° C., continuing stirring for 20 to 25 minutes, discharging the powder and classifying it with a classifier to obtain a composite low-cost powder.

9. The method for preparing a low-cost composite powder of calcium carbonate powder and solid waste powder for polyolefin plastic sewage pipes according to claim 5, characterized in that: The following steps are included: SP C1 1. Take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the calcium carbonate ore, add 15 to 23 times of water to dilute for later use; take the triethanolamine or the ethylene glycol at a mass ratio of 1 / 1000 of the solid waste powder and mix with the water glass or the sodium aluminate at a ratio of 1:1, add 15 to 23 times of water to dilute for later use; SP C2 , take the calcium carbonate ore and solid waste by mass and transport them to the roller mill, and add SP C1 Step-diluted grinding aid; SP C3 , grinding the calcium carbonate ore and the solid waste by a roller mill to obtain a mixed powder, and sending the mixed powder with a particle size meeting the requirements into a storage tank through a classifier; SP C4 1. Heat the zero-gravity mixer to 95-110°C and keep it warm for at least 30 minutes; SP C5 , transferring the carbon mixed powder into a zero-gravity mixer, starting the zero-gravity mixer for stirring, and raising the temperature of the mixed powder to at least 90° C. during the stirring process, during which the speed of the zero-gravity mixer is controlled to maintain at 50 to 70 rad / min; SP C6 , adding the modifier in proportion by mass into the zero-gravity mixer, and controlling the adding time of the modifier to be 40 to 60 seconds; SP C7 , maintaining the powder temperature in the zero-gravity mixer not lower than 90° C., continuing stirring for 20 to 25 minutes, discharging the powder and classifying it with a classifier to obtain a composite low-cost powder.