Tire body rubber composition capable of reducing use of carbon black, preparation method of tire body rubber composition and tire

By using natural rubber, liquid reclaimed rubber and silica and other combinations in tire manufacturing to replace traditional furnace carbon black and optimizing the carcass rubber formula, the carbon dioxide emission problem caused by the high use of carbon black in tire manufacturing is solved. The effect of reducing carbon emissions and maintaining tire performance is achieved.

CN118725422APending Publication Date: 2024-10-01ZHONGCE RUBBER GRP CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410907104.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The high amount of carbon black used in existing tire manufacturing leads to an increase in carbon dioxide emissions. Especially in the production of economical car tires, it is difficult to effectively reduce the use of carbon black to reduce carbon emissions.

Method used

Reduce the use of furnace carbon black by designing a carcass rubber composition containing natural rubber, styrene-butadiene rubber, liquid reclaimed rubber, white carbon black, ultrafine diatomaceous earth and specific accelerators, combined with an optimized mixing process volume while maintaining tire performance.

Benefits of technology

It has achieved a significant reduction in carbon dioxide emissions while meeting tire performance. By replacing furnace carbon black with liquid reclaimed rubber and white carbon black, the filler formula has been optimized, reducing the use of carbon black and reducing carbon emissions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of tire rubber manufacturing, and discloses a tire body rubber composition capable of reducing use of carbon black, a preparation method of the tire body rubber composition and a tire. Through reinforcement interchange of reclaimed rubber, carbon black, an inorganic material and the like and redesign and optimization of a formula, the use of carbon black is greatly reduced, for example, liquid reclaimed rubber, white carbon black and superfine diatomite are added, and the liquid reclaimed rubber, furnace carbon black, white carbon black and superfine diatomite have a synergistic effect; and the proportions of the natural rubber, the phenolic formaldehyde condensation resin, the methyl donor and the like are adjusted, so that the purposes of meeting the tire performance and reducing the carbon dioxide emission can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tire rubber manufacturing, and in particular to a carcass rubber composition capable of reducing the use of carbon black, a preparation method thereof, and a tire. Background Art

[0002] Carbon black has been used as a reinforcing material for rubber tires for 130 years. In 2022, the world's carbon black production has reached 14 million tons, 75% of which is used in tire manufacturing, indicating that carbon black is an indispensable material for tire production. With the publication of patents related to the use of silica in treads by various companies, the use of silica has also increased rapidly in recent years, but the use of carbon black still occupies the absolute main force in rubber tire reinforcement materials. And more than 80% of them are produced by furnace carbon black, that is, they are produced by the oil furnace method through the incomplete combustion of raw oil and fuel oil. The reinforcing filling material of rubber tires is mainly furnace carbon black, which is due to the good lipophilicity of the furnace carbon black surface and the suitable distribution of aggregate morphology and the reinforcement performance of rubber materials.

[0003] Since Michelin issued the "Green Tire" patent in 1992 for using high-content white carbon black in tire tread rubber, the use of white carbon black in the tire industry has indeed developed significantly, reducing the proportion of carbon black to a certain extent. However, white carbon black is mainly used in high-performance tires such as high-wet-slip HPT tires or low-rolling resistance tire tread formulations. In economical car tire products, long mileage, impact resistance and suitable prices account for a high proportion. Economical tires require a wear mileage index of more than half UTGQ 500, so the "semi-green" formula with pure carbon black or half white carbon black is more appropriate. Components other than tread formulas, such as carcass rubber and base rubber, occasionally use white carbon black to replace part of the carbon black patents: such as the carcass rubber patent CN201410609368.8 using wet mixing, and the all-steel base rubber using white carbon black patents CN201210281772.8 and CN200810155766.1. The airtight layer has a patent CN201310268279.7 that uses diatomite to replace carbon black. It can be seen that the use of white carbon black in the carcass rubber adopts a special mixing method, the use of white carbon black in the base rubber is mainly concentrated in all-steel tires, and the use of diatomite in the inner liner is slightly mature. Statistically speaking, the proportion of carbon black used in the current economical semi-steel radial tire formula accounts for 27% of the tire rubber formula by mass.

[0004] From the perspective of environmental carbon dioxide emissions, it is known that the oil furnace combustion process requires about 1.8 tons of carbon dioxide per ton of carbon black, and the entire process from crude oil production to carbon black packaging to produce 1 ton of carbon black requires 4.5 tons of carbon dioxide, so carbon black is a high carbon dioxide emission product. In response to climate change, China has proposed a plan to reduce greenhouse gas emissions, mainly carbon dioxide. Therefore, reducing the use of furnace carbon black is of great significance to reducing carbon dioxide emissions, so it is necessary to significantly reduce the use of carbon black in the production of economy cars, thereby significantly reducing carbon dioxide emissions. Summary of the invention

[0005] The present invention aims at the deficiencies of the prior art and provides a carcass rubber composition and a preparation method thereof, and a tire that reduces the use of carbon black. The carcass rubber composition provided by the present invention can meet the requirements of tire performance while reducing carbon dioxide emissions.

[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions: A carcass rubber composition for reducing carbon black usage, wherein the rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Natural rubber 60-90 parts Styrene butadiene rubber 10-20 parts Butadiene rubber 10-20 parts Liquid recycled rubber 5-10 parts Furnace carbon black 20-30 parts 10-20 parts of white carbon black 5-10 parts of ultrafine diatomaceous earth 1-2 parts of antioxidant Zinc oxide 1-5 parts 1-2 parts stearic acid 1-4 parts of phenolic formaldehyde condensation resin 1-3 parts of methyl donor 20% insoluble sulfur 2-5 parts oil-filled Accelerator 0.5-1.5 parts.

[0007] Preferably, the rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Natural rubber 75-85 parts Styrene butadiene rubber 10-20 parts 5-10 parts of butadiene rubber Liquid recycled rubber 7-10 parts Furnace carbon black 25-30 parts 10-15 parts of white carbon black 5-8 parts of ultra-fine diatomaceous earth 1-2 parts of antioxidant Zinc oxide 2.5-3.5 parts 1-2 parts stearic acid 1.5-2.5 parts of phenolic formaldehyde condensation resin 1-2 parts of methyl donor 20% insoluble sulfur 3-4 parts oil Accelerator 0.5-1.0 part

[0008] The carcass rubber is a rubber composition of the tire polyester cord skeleton material. The hardness is generally required to be 60-70, preferably 64-66. Too low hardness will lead to poor carcass handling performance, and too high hardness will lead to excessive rigidity of the tire carcass and affect comfort. The adhesion between rubber and polyester is an important performance indicator. In order to achieve a higher adhesion level, it is appropriate to use a higher content of natural rubber. Natural rubber has a large molecular weight, good tear resistance and high modulus. Good tear resistance can improve the peeling performance of the colloid and the cord, and high modulus can improve the H extraction performance. The calendering workability of the all-natural rubber carcass formula is not good, so styrene-butadiene rubber and butadiene rubber should be used together to achieve a balance between adhesion and workability. In order to maintain the modulus in the low-carbon formula, furnace carbon black can choose a grade of carbon black with high reinforcement, such as N220 and N330 series. Adhesion promoters are indispensable. A combination of phenolic formaldehyde condensation resin and methyl donor is used. The ratio of the two is adjusted according to the adhesion performance and rubber modulus. The bonding system can increase the modulus of the rubber composition, thereby improving H extraction.

[0009] Preferably, the BET specific surface area of ​​white carbon black is 150-170 m 2 / g, such as Solvay's 1165MP highly dispersed white carbon black; The furnace carbon black is a fine particle high reinforcement series carbon black, including but not limited to N220, N234, N330, N326, and N375.

[0010] Preferably, the ratio of the phenolic formaldehyde condensation resin to the methyl donor is 3:2-3:1; the phenolic formaldehyde condensation resin includes but is not limited to α-methylphenol formaldehyde condensation resin and its derivatives, resorcinol formaldehyde condensation resin and its derivatives, such as B-20-S, SL3020, etc.; the methyl donor is hexamethylenetetramine, referred to as HMT, which is also a accelerator in the tire industry.

[0011] Preferably, the oil-extended 20% insoluble sulfur is IS7020 or highly dispersed HD-OT20, and the insoluble sulfur content of such sulfur is maintained above 80% at 105° C. for 15 minutes; the accelerator is a sulfonamide accelerator, preferably accelerator NS or accelerator CZ.

[0012] Preferably, the liquid regenerated rubber comprises the following components: Rubber powder 100 parts Modifier 10.0-30.0 parts Activator 1.0-10.0 parts; The rubber powder has a size of 40-60 mesh and is prepared by crushing-grinding-screening-metal separation using all-steel tire tread rubber; The modifier includes a mixture of two or more of 3-hydroxycyclopentene, hexadienoic acid, 1,5-cyclooctadiene, cyclopentadienoic acid, and docosadienoic acid; preferably, the modifier also includes one or more of diphenyl disulfide, cyclopentadiene maleate, and dicyclopentadiene maleate; The activator is selected from one or more of liquid isoprene rubber, aromatic oil, vegetable oil, tall oil and pine tar oil.

[0013] Preferably, the method for preparing the liquid regenerated rubber comprises the following steps: 1) Put rubber powder, modifier and activator into a mixer, mix them thoroughly until the material temperature is higher than 90°C, and then put the materials into a twin-screw extruder; 2) The twin-screw extruder is temperature-controlled in different zones. The temperature in the reaction zone is at 360-380℃ for high-temperature desulfurization. After desulfurization, the material enters the cooling zone for cooling and is then extruded from the die of the twin-screw extruder to obtain liquid reclaimed rubber.

[0014] Preferably, the ultrafine diatomaceous earth is a lamellar structure filler obtained by crushing, washing and grinding, chemical decomposition, activation treatment, impurity removal and drying of natural ore, with an average lamellar diameter of <500nm, thickness <100nm, and median particle size D50≤10μm; the ultrafine diatomaceous earth is obtained by water grinding, and the ultrafine diatomaceous earth obtained by this method can achieve sufficient fineness.

[0015] Furthermore, the present invention also discloses a method for preparing the rubber composition, comprising the following steps: 1) One-stage mixing: Use a tangential internal mixer, add raw rubber and liquid reclaimed rubber and plasticize for 20-50 seconds, then add carbon black, white carbon black, ultrafine diatomaceous earth, antioxidant, stearic acid and phenolic formaldehyde condensation resin, pressurize to 120-130℃, lift the drum to clean, then pressurize to 150-165℃ to discharge the glue, and the obtained masterbatch is left for 4-8 hours; 2) Final mixing: Use a tangential internal mixer to add masterbatch, sulfur, accelerator and methyl donor, mix under pressure for 20-35 seconds, lift the mixer to clean, pressurize to 95-105℃ to discharge the rubber, and obtain a rubber composition.

[0016] Furthermore, the present invention also discloses a tire, the carcass rubber of which is prepared by vulcanizing the rubber composition.

[0017] The beneficial effects of the present invention are as follows: the present invention significantly reduces the use of carbon black by reinforcing and exchanging recycled rubber, carbon black and inorganic materials and redesigning and optimizing the formula, such as adding liquid recycled rubber, white carbon black and ultrafine diatomaceous earth, and adjusting the proportions of natural rubber, phenolic formaldehyde condensation resin, methyl donor and other ingredients, so as to achieve the purpose of meeting tire performance while reducing carbon dioxide emissions. DETAILED DESCRIPTION

[0018] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0019] A carcass rubber composition with reduced carbon black usage is provided, and the formula of the rubber composition is shown in Table 1. The sulfur is insoluble sulfur containing 20% ​​oil, and the furnace carbon black 2 is high-structure and high-wear-resistant carbon black N375.

[0020] The preparation method of the rubber composition is as follows: 1) One-stage mixing: Use a tangential internal mixer, add raw rubber and liquid reclaimed rubber and plasticize for 20-50 seconds, then add carbon black, white carbon black, ultrafine diatomaceous earth, antioxidant, stearic acid and phenolic formaldehyde condensation resin, pressurize to 125℃, lift the drum to clean, then pressurize to 150-165℃ to discharge the glue, and the obtained masterbatch is left for 4-8 hours; 2) Final mixing: Use a tangential internal mixer, add masterbatch, sulfur, accelerator and methyl donor, mix under pressure for 20-35 seconds, lift the drum to clean, pressurize to 95-105℃ to discharge the rubber, and obtain a rubber composition. It can be used after being parked for more than 4 hours.

[0021] Among them, the formula of liquid recycled rubber is: 100 parts of rubber powder, 20.0 parts of modifier, and 5.0 parts of activator.

[0022] The preparation of liquid reclaimed rubber is as follows: 1) Put rubber powder, modifier and activator into a mixer, mix them thoroughly until the material temperature is higher than 90°C, and then put the materials into a twin-screw extruder; 2) The twin-screw extruder is temperature-controlled in different zones. The temperature in the reaction zone is at 360-380℃ for high-temperature desulfurization. After desulfurization, the material enters the cooling zone for cooling and is then extruded from the die of the twin-screw extruder to obtain liquid reclaimed rubber with a rubber hydrocarbon content of 50% and a carbon black content of 30%.

[0023] Comparative Example A carcass rubber composition is provided, and the formula of the rubber composition is shown in Table 1.

[0024] The preparation method of the rubber composition is as shown in Examples.

[0025] The formula and preparation method of the liquid regenerated rubber are the same as those in the embodiment.

[0026] Reference ratio A carcass rubber composition is provided, and the formula of the rubber composition is shown in Table 1. Among them, furnace carbon black 1 is a high wear-resistant carbon black.

[0027] The preparation method of the rubber composition is as shown in Examples.

[0028] Table 1 Reference ratio Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Natural rubber 60 80 65 70 80 80 80 80 80 80 80 80 Styrene Butadiene Rubber 20 10 20 20 10 10 10 10 10 10 10 10 Butadiene rubber 20 10 15 10 10 10 10 10 10 10 10 10 Liquid recycled rubber 10 10 10 10 10 10 10 10 10 10 Furnace Carbon Black 1 56 Furnace Carbon Black 2 30 30 30 30 30 30 30 30 White Carbon Black 12 12 12 12 12 12 12 12 Ultrafine diatomaceous earth 5 5 5 5 5 5 5 diatomite 5 Environmentally friendly oil 10 Antioxidant RD 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5 Stearic acid 1 1 1 1 1 1 1 1 1 1 1 1 Resorcinol resin formaldehyde condensation resin 1.8 2.5 3 1.5 2.5 2.5 2.5 2.5 2.5 2.5 2.5 2.5 Methyl donor 1.2 1.5 1 1 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5 Insoluble sulfur IS7020 3.5 3.5 3.5 3.5 3.5 3.5 3.5 3.5 3.5 3.5 3.5 3.5 Accelerator CZ 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 Total formula phr 175.8 167.8 167.8 166.3 137.8 155.8 162.8 125.8 132.8 150.8 157.8 167.8 Formula furnace carbon black ratio% 31.85 17.88 17.88 18.04 0.00 19.26 18.43 0.00 0.00 19.89 19.01 17.88 Rubber specific gravity 1.142 1.129 1.129 1.132 1.044 1.088 1.110 0.995 1.022 1.068 1.128 1.129 Weight of rubber compound per tire (by specific gravity) 0.610 0.485 0.485 0.486 0.449 0.467 0.477 0.427 0.439 0.459 0.485 0.485 Weight of furnace black used per piece / kg 0.194 0.087 0.087 0.088 0.000 0.090 0.088 0.000 0.000 0.091 0.092 0.087 hardness 66 64 63 60 45 55 59 40 44 56 68 62 Tear resistance 75 82 71 73 43 68 71 40 45 65 75 60 H Extract 165 170 158 164 112 135 158 90 105 130 170 158 Table 1 footnote: 1. Natural rubber, Thailand 20# standard rubber STR20, initial plasticity value P0 ≥ 30, plasticity retention rate (PRI) ≥ 40, Mooney viscosity ML (1+4) 100℃ 83; 2.Styrene butadiene rubber, non-oil-extended latex polystyrene butadiene rubber SBR1500, styrene 23.5%, Jilin Petrochemical Products; 3. Butadiene rubber, nickel-based solution polymerized high-cis butadiene rubber, product model BR9000; 4. Furnace carbon black 1, N330, iodine absorption value 84g / kg, oil absorption value 102×10 5 m 3 / kg, CTAB adsorption specific surface area 79×10 3 m 2 / kg; 5. Furnace carbon black 2, N375, iodine absorption value 93g / kg, oil absorption value 114×10 5 m 3 / kg CTAB adsorption specific surface area 96×10 3 m 2 / kg; 6. White carbon black, 1165MP, BET surface area 150-170m 2 / g, Solvay Chemical Products; 7. Ultrafine diatomite, average flake diameter <500nm, thickness <100nm, water grinding, Qixiang High-tech Materials Co., Ltd.; 8. Toluene diphenol formaldehyde condensation resin, SL3020, Universal softening point 99-109℃, free phenol content ≤5%, Huaqi (China) Chemical Co., Ltd.; 9. Methyl donor, HMT, chemical name hexamethylenetetramine, common name urotropine, also known as accelerator H.

[0029] 10. Insoluble sulfur IS7020, insoluble sulfur content ≥70%, thermal stability at 105℃×15 minutes, ≥75%, Shandong Shangshun Chemical Co., Ltd.; Other raw materials are regular industrial products sold in the market.

[0030] Referring to Table 1, Example 1 is the best example. It can be seen from the examples and reference examples that the synergistic effect of liquid regenerated rubber, furnace carbon black 2, white carbon black and ultrafine diatomaceous earth can replace furnace carbon black 1 and reduce the amount of furnace carbon black added without affecting the performance of the rubber composition. It can be seen from Example 1 and Comparative Examples 1-7 that the absence of liquid regenerated rubber, furnace carbon black 2, white carbon black or ultrafine diatomaceous earth will affect the final replacement effect, among which the effect of liquid regenerated rubber is smaller, but the addition of liquid regenerated rubber is beneficial to reduce the amount of furnace carbon black added. It can be seen from Example 1 and Comparative Example 8 that the size of diatomaceous earth will also affect the performance of the rubber composition. Therefore, by appropriately adding other fillers and adjusting the formula, the amount of furnace carbon black added can be reduced and the emission of carbon dioxide can be reduced.

[0031] The above is a description of the embodiments of the present invention. Through the above description of the disclosed embodiments, professionals and technicians in the field can implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will conform to the widest range consistent with the principles and novelties disclosed herein.

Claims

1. A carcass rubber composition for reducing carbon black usage, characterized in that: The rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Natural rubber 60-90 parts Styrene butadiene rubber 10-20 parts Butadiene rubber 10-20 parts Liquid recycled rubber 5-10 parts Furnace carbon black 20-30 parts 10-20 parts of white carbon black 5-10 parts of ultrafine diatomaceous earth 1-2 parts of antioxidant Zinc oxide 1-5 parts 1-2 parts stearic acid 1-4 parts of phenolic formaldehyde condensation resin 1-3 parts of methyl donor 20% insoluble sulfur 2-5 parts oil-filled Accelerator 0.5-1.5 parts.

2. The rubber composition according to claim 1, characterized in that The rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Natural rubber 75-85 parts Styrene butadiene rubber 10-20 parts 5-10 parts of butadiene rubber Liquid recycled rubber 7-10 parts Furnace carbon black 25-30 parts 10-15 parts of white carbon black 5-8 parts of ultra-fine diatomaceous earth 1-2 parts of antioxidant Zinc oxide 2.5-3.5 parts 1-2 parts stearic acid 1.5-2.5 parts of phenolic formaldehyde condensation resin 1-2 parts of methyl donor 20% insoluble sulfur 3-4 parts oil Accelerator 0.5-1.0 part 3. The rubber composition according to claim 1 or 2, characterized in that: The BET specific surface area of ​​the white carbon black is 150-170 m 2 / g; the furnace carbon black is a fine particle high reinforcement series carbon black, including but not limited to N220, N234, N330, N326, and N375.

4. The rubber composition according to claim 1 or 2, characterized in that: The ratio of the phenolic formaldehyde condensation resin to the methyl donor is 3:2-3:1; the phenolic formaldehyde condensation resin includes but is not limited to α-methylphenol formaldehyde condensation resin and its derivatives, resorcinol formaldehyde condensation resin and its derivatives; the methyl donor is hexamethylenetetramine.

5. The rubber composition according to claim 1 or 2, characterized in that: The oil-extended 20% insoluble sulfur is IS7020 or HD-OT20; the accelerator is a sulfonamide accelerator, preferably accelerator NS or accelerator CZ.

6. The rubber composition according to claim 1 or 2, characterized in that: The liquid regenerated rubber comprises the following components: Rubber powder 100 parts Modifier 10.0-30.0 parts Activator 1.0-10.0 parts; The rubber powder has a size of 40-60 mesh and is prepared by crushing-grinding-screening-metal separation using all-steel tire tread rubber; The modifier includes a mixture of two or more of 3-hydroxycyclopentene, hexadienoic acid, 1,5-cyclooctadiene, cyclopentadienoic acid, and docosadienoic acid; preferably, the modifier also includes one or more of diphenyl disulfide, cyclopentadiene maleate, and dicyclopentadiene maleate; The activator is selected from one or more of liquid isoprene rubber, aromatic oil, vegetable oil, tall oil and pine tar oil.

7. The rubber composition according to claim 6, characterized in that The preparation method of the liquid regenerated rubber comprises the following steps: 1) Put rubber powder, modifier and activator into a mixer, mix them thoroughly until the material temperature is higher than 90°C, and then put the materials into a twin-screw extruder; 2) The twin-screw extruder is temperature-controlled in different zones. The temperature in the reaction zone is at 360-380℃ for high-temperature desulfurization. After desulfurization, the material enters the cooling zone for cooling and is then extruded from the die of the twin-screw extruder to obtain liquid reclaimed rubber.

8. The rubber composition according to claim 1 or 2, characterized in that: The ultrafine diatomite is a filler with a lamellar structure, with an average lamellar diameter of less than 500nm, a thickness of less than 100nm, and a median particle size D50≤10μm; the ultrafine diatomite is obtained by water milling.

9. The method for preparing the rubber composition according to any one of claims 1 to 8, characterized in that: The following steps are involved: 1) One-stage mixing: Use a tangential internal mixer, add raw rubber and liquid reclaimed rubber and plasticize for 20-50 seconds, then add carbon black, white carbon black, ultrafine diatomaceous earth, antioxidant, stearic acid and phenolic formaldehyde condensation resin, pressurize to 120-130℃, lift the drum to clean, then pressurize to 150-165℃ to discharge the glue, and the obtained masterbatch is left for 4-8 hours; 2) Final mixing: Use a tangential internal mixer to add masterbatch, sulfur, accelerator and methyl donor, mix under pressure for 20-35 seconds, lift the mixer to clean, pressurize to 95-105℃ to discharge the rubber, and obtain a rubber composition.

10. A tire, characterized in that: The carcass rubber of the tire is prepared by vulcanizing the rubber composition described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Tire body rubber material utilizing regenerated rubber as well as blending method and application thereof

    CN101628994A

  • Tire tube prepared by reclaimed rubber substituting for carbon black

    CN102453264A

  • Tire body rubber composition for reducing tire rolling resistance, mixing method, application and tire

    CN115160656A

  • Method for producing tire rubber composition

    JP2018199791A