Formula and preparation method of antibacterial modified plastic

By using formulas such as polypropylene resin and silver ion antibacterial agents in antibacterial plastics and high temperature and high pressure twin-screw extrusion technology, the problems of insufficient tensile strength, impact strength, flexural modulus and aging resistance of antibacterial plastics are solved. Efficient antibacterial performance and stability are achieved, making it suitable for large-scale production.

CN118725460APending Publication Date: 2024-10-01NINGBO FUTIAN ENG PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992205.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing antibacterial plastics have deficiencies in tensile strength, impact strength, flexural modulus, aging resistance and chemical stability. Poor antibacterial agent dispersion leads to poor antibacterial performance.

Method used

It adopts a formula of polypropylene resin, silver ion antibacterial agent, compatibilizer, coupling agent, lubricant, dispersant, antioxidant, UV absorber and cross-linking agent, and is evenly dispersed through a twin-screw extruder under high temperature and high pressure. antibacterial agent, and carry out melting, mixing, extrusion, cooling and pelletizing processes in an injection molding machine to prepare antibacterial modified plastics.

Benefits of technology

It improves the antibacterial ability, tensile strength, impact strength and flexural modulus of antibacterial modified plastics, enhances aging resistance and chemical stability, ensures the stability and consistency of the processing process, and facilitates mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725460A_ABST
    Figure CN118725460A_ABST
Patent Text Reader

Abstract

The invention discloses an antibacterial modified plastic formula and a preparation method thereof, and particularly relates to the field of antibacterial plastic preparation, and the antibacterial modified plastic formula comprises the following components in parts by weight: 60-80 parts of polypropylene resin, 5-8 parts of a silver ion antibacterial agent, 3-5 parts of a compatilizer, 1-2 parts of a coupling agent, 0.3-0.6 part of a lubricant, 0.3-0.6 part of a dispersant, 0.4-0.8 part of an antioxidant, 0.3-0.5 part of an ultraviolet light absorber and 0.5-0.7 part of a cross-linking agent. In the formula of the antibacterial modified plastic designed by the invention, the silver ion antibacterial agent is uniformly dispersed in the plastic, so that the plastic has efficient antibacterial ability, the antibacterial modified plastic is ensured to have excellent tensile strength, impact strength and flexural modulus, and the actual application requirements are met; the antioxidant and the ultraviolet light absorber effectively improve the aging resistance and chemical stability of the plastic, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of antibacterial plastic preparation, and more specifically, to an antibacterial modified plastic formula and a preparation method thereof. Background Art

[0002] With the development of modern society, plastic products have been widely used in various fields such as industry, agriculture, construction, transportation, communication, medical treatment and daily life. However, plastic products are easily contaminated and breed various microorganisms during use, including bacteria, mold, yeast and viruses. The presence of these microorganisms not only affects the appearance and performance of the product, but may also pose a threat to people's health. Therefore, it is particularly important to develop modified plastics with antibacterial functions.

[0003] Traditional plastic products do not have antibacterial properties. In order to solve this problem, researchers began to explore ways to add antimicrobial agents to plastics to give them antibacterial properties. Antimicrobial plastics are a type of modified plastic that has an inhibitory or killing effect on microorganisms contaminated on the surface of plastics, and keeps itself clean by inhibiting the reproduction of microorganisms. At present, antimicrobial plastics are mainly obtained by adding a small amount of antimicrobial agents to ordinary plastics, such as silver-based inorganic antimicrobial agents, organic antimicrobial agents, natural antimicrobial agents, etc.

[0004] However, the traditional direct addition method has shortcomings in the dispersibility of antimicrobial agents. The dispersibility of antimicrobial agents in plastic substrates is limited by the raw materials, the compatibility of antimicrobial agents and the manufacturing process. Usually, antimicrobial agents are distributed in the plastic substrate in certain aggregates, resulting in poor antimicrobial performance. In order to improve the dispersibility and antimicrobial effect of antimicrobial agents, researchers have developed a variety of improved preparation methods, such as first extruding the antimicrobial agent and substrate resin or resin with good compatibility through a twin-screw extruder to make antimicrobial masterbatch, and then further processing it into antimicrobial plastic products. This method significantly improves the dispersibility of antimicrobial agents in plastics and improves the antimicrobial effect.

[0005] In addition, with the development of nanotechnology, nano-antibacterial plastics have become a research hotspot. Nano-antibacterial agents, such as nano-silver particles, have excellent antibacterial properties and stability, and can be evenly dispersed in plastic substrates to achieve long-term antibacterial effects. By integrating nano-antibacterial agents into plastics, antibacterial plastic products with strong antibacterial properties, safety and environmental protection can be prepared.

[0006] In the above background, the present invention designs an antibacterial modified plastic formula and a preparation method thereof, which improves the shortcomings of existing antibacterial plastics in terms of tensile strength, impact strength, flexural modulus, aging resistance and chemical stability based on the above plastic antibacterial method. Summary of the invention

[0007] In order to overcome the above-mentioned defects of the prior art, the present invention provides an antibacterial modified plastic formula and a preparation method thereof.

[0008] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: an antibacterial modified plastic formula, comprising the following components and their weight portions: 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of cross-linking agent.

[0009] As a further improvement of the technical solution of the present invention, the compatibilizer is preferably maleic anhydride grafted polypropylene, and the coupling agent is preferably a silane coupling agent.

[0010] As a further improvement of the technical solution of the present invention, the lubricant is preferably stearic acid amide, the dispersant is preferably stearate, and the cross-linking agent is preferably dicumyl peroxide.

[0011] A method for preparing an antibacterial modified plastic, the specific preparation method is as follows:

[0012] Step 1, raw material preparation, prepare 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of cross-linking agent;

[0013] Step 2: prepare antibacterial masterbatch, pre-mix, mix the silver ion antibacterial agent, compatibilizer, coupling agent and a small amount of polypropylene resin evenly to form a mixture, and then use a twin-screw extruder to extrude the mixture into antibacterial masterbatch under high temperature and high pressure. In this process, the shearing and kneading action of the twin screw helps to evenly disperse the antibacterial agent in the resin;

[0014] Step 3, preparing antibacterial plastic, adding the remaining polypropylene resin, antibacterial masterbatch, lubricant, dispersant, antioxidant, ultraviolet absorber and crosslinking agent into a high-speed mixer, mixing them evenly, sending the mixed materials into a single-screw or twin-screw extruder, and undergoing the processes of melting, mixing, extruding, cooling and pelletizing to obtain antibacterial modified plastic particles;

[0015] Step 4: Processing and molding: putting the antibacterial modified plastic particles into an injection molding machine, heating and melting them, injecting them into a mold, and demolding them after cooling and solidification to obtain an antibacterial plastic product;

[0016] Step five: performance testing: conducting performance testing on the prepared antibacterial modified plastic.

[0017] As a further improvement of the technical solution of the present invention, the small amount of polypropylene resin added in step 2 accounts for 10% of the total amount, and the polypropylene resin added in step 3 accounts for 90% of the total amount.

[0018] As a further improvement of the technical solution of the present invention, the twin-screw extruder in the step 2 is composed of a feeding zone, a preheating zone, a melting zone, a mixing zone, a venting zone and a cooling zone. During the process of the twin-screw extruder extruding the mixture under high temperature and high pressure, the temperature of the feeding zone on the twin-screw extruder is 20-50°C, the temperature of the preheating zone is 80-100°C, the temperature of the melting zone is 150-170°C, the temperature of the mixing zone and the venting zone is maintained at 160-170°C, the temperature of the cooling zone is 90-110°C, and at the same time, the extrusion pressure of the twin-screw extruder is 10-70MPa.

[0019] As a further improvement of the technical solution of the present invention, the temperature of the melting stage in step three is 180-230°C, the mixing time is not less than 30 minutes, the extrusion pressure is 10-70MPa, and the cooling method adopted in the cooling stage is preferably air cooling.

[0020] As a further improvement of the technical solution of the present invention, in step 4, the injection temperature of the injection molding machine is 180-230° C., and the injection pressure is 40-200 MPa.

[0021] As a further improvement of the technical solution of the present invention, the performance test in step five includes conducting antibacterial performance test, tensile strength test, impact strength test, bending modulus test and chemical stability test on the prepared antibacterial modified plastic.

[0022] Beneficial effects of the present invention:

[0023] In the antibacterial modified plastic formula designed by the present invention, a silver ion antibacterial agent is uniformly dispersed in the plastic, so that the plastic has a highly efficient antibacterial ability and ensures that the antibacterial modified plastic has excellent tensile strength, impact strength and bending modulus, meeting the actual application requirements; the antioxidant and the ultraviolet absorber effectively improve the aging resistance and chemical stability of the plastic, prolong the service life; and by controlling the melting temperature, mixing time, extrusion pressure, etc., the stability and consistency of the antibacterial modified plastic during the processing are ensured, which is convenient for large-scale production; the coupling agent enhances the bonding force between the antibacterial agent and the plastic substrate; the lubricant reduces friction and wear during the processing; and the cross-linking agent is used to improve the heat resistance and strength of the plastic.

[0024] In summary, the antibacterial modified plastics prepared by the antibacterial modified plastic formula have achieved remarkable technical effects in terms of antibacterial properties, physical and mechanical properties, chemical stability, processing properties and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1It is a preparation flow chart of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] An antibacterial modified plastic formula comprises the following components and their weight parts: 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of crosslinking agent.

[0029] Preferably, the compatibilizer is maleic anhydride grafted polypropylene, and the coupling agent is preferably a silane coupling agent.

[0030] Preferably, the lubricant is stearic acid amide, the dispersant is stearate, and the cross-linking agent is dicumyl peroxide.

[0031] Among them, antioxidants and ultraviolet absorbers can be selected from common types on the market, and the specific ingredients are not specifically limited.

[0032] A method for preparing an antibacterial modified plastic, the specific preparation method is as follows:

[0033] Step 1, raw material preparation, prepare 80 parts of polypropylene resin, 8 parts of silver ion antibacterial agent, 5 parts of compatibilizer, 2 parts of coupling agent, 0.6 parts of lubricant, 0.6 parts of dispersant, 0.8 parts of antioxidant, 0.5 parts of ultraviolet absorber and 0.7 parts of cross-linking agent;

[0034] Step 2: prepare antibacterial masterbatch, pre-mix, mix the silver ion antibacterial agent, compatibilizer, coupling agent and a small amount of polypropylene resin evenly to form a mixture, and then use a twin-screw extruder to extrude the mixture into antibacterial masterbatch under high temperature and high pressure. In this process, the shearing and kneading action of the twin screw helps to evenly disperse the antibacterial agent in the resin;

[0035] Step 3, preparing antibacterial plastic, adding the remaining polypropylene resin, antibacterial masterbatch, lubricant, dispersant, antioxidant, ultraviolet absorber and crosslinking agent into a high-speed mixer, mixing them evenly, sending the mixed materials into a single-screw or twin-screw extruder, and undergoing the processes of melting, mixing, extruding, cooling and pelletizing to obtain antibacterial modified plastic particles;

[0036] Step 4: Processing and molding: putting the antibacterial modified plastic particles into an injection molding machine, heating and melting them, injecting them into a mold, and demolding them after cooling and solidification to obtain an antibacterial plastic product;

[0037] Step five: performance testing: conducting performance testing on the prepared antibacterial modified plastic.

[0038] The small amount of polypropylene resin added in step 2 accounts for 10% of the total amount, and the polypropylene resin added in step 3 accounts for 90% of the total amount.

[0039] Wherein, the twin-screw extruder in step 2 is composed of a feeding zone, a preheating zone, a melting zone, a mixing zone, a venting zone and a cooling zone. During the process of the twin-screw extruder extruding the mixture under high temperature and high pressure, the temperature of the feeding zone on the twin-screw extruder is 20-50°C, the temperature of the preheating zone is 80-100°C, the temperature of the melting zone is 150-170°C, the temperature of the mixing zone and the venting zone is maintained at 160-170°C, the temperature of the cooling zone is 90-110°C, and at the same time, the extrusion pressure of the twin-screw extruder is 10-70MPa.

[0040] Among them, the temperature of the melting stage in step three is 180-230° C., the mixing time is not less than 30 min, the extrusion pressure is 10-70 MPa, and the cooling method adopted in the cooling stage is preferably air cooling.

[0041] Wherein, in step 4, the injection molding temperature of the injection molding machine is 180-230° C., and the injection molding pressure is 40-200 MPa.

[0042] Among them, the performance test in step five includes antibacterial performance test, tensile strength test, impact strength test, bending modulus test and chemical stability test on the prepared antibacterial modified plastic.

[0043] Example 2

[0044] An antibacterial modified plastic formula comprises the following components and their weight parts: 60 parts of polypropylene resin, 5 parts of silver ion antibacterial agent, 3 parts of compatibilizer, 1 part of coupling agent, 0.3 parts of lubricant, 0.3 parts of dispersant, 0.4 parts of antioxidant, 0.3 parts of ultraviolet absorber and 0.5 parts of crosslinking agent.

[0045] Preferably, the compatibilizer is maleic anhydride grafted polypropylene, and the coupling agent is preferably a silane coupling agent.

[0046] Preferably, the lubricant is stearic acid amide, the dispersant is stearate, and the cross-linking agent is dicumyl peroxide.

[0047] A method for preparing an antibacterial modified plastic, the specific preparation method is as follows:

[0048] Step 1, raw material preparation, prepare 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of cross-linking agent;

[0049] Step 2: prepare antibacterial masterbatch, pre-mix, mix the silver ion antibacterial agent, compatibilizer, coupling agent and a small amount of polypropylene resin evenly to form a mixture, and then use a twin-screw extruder to extrude the mixture into antibacterial masterbatch under high temperature and high pressure. In this process, the shearing and kneading action of the twin screw helps to evenly disperse the antibacterial agent in the resin;

[0050] Step 3, preparing antibacterial plastic, adding the remaining polypropylene resin, antibacterial masterbatch, lubricant, dispersant, antioxidant, ultraviolet absorber and crosslinking agent into a high-speed mixer, mixing them evenly, sending the mixed materials into a single-screw or twin-screw extruder, and undergoing the processes of melting, mixing, extruding, cooling and pelletizing to obtain antibacterial modified plastic particles;

[0051] Step 4: Processing and molding: putting the antibacterial modified plastic particles into an injection molding machine, heating and melting them, injecting them into a mold, and demolding them after cooling and solidification to obtain an antibacterial plastic product;

[0052] Step five: performance testing: conducting performance testing on the prepared antibacterial modified plastic.

[0053] The small amount of polypropylene resin added in step 2 accounts for 10% of the total amount, and the polypropylene resin added in step 3 accounts for 90% of the total amount.

[0054] Wherein, the twin-screw extruder in step 2 is composed of a feeding zone, a preheating zone, a melting zone, a mixing zone, a venting zone and a cooling zone. During the process of the twin-screw extruder extruding the mixture under high temperature and high pressure, the temperature of the feeding zone on the twin-screw extruder is 20-50°C, the temperature of the preheating zone is 80-100°C, the temperature of the melting zone is 150-170°C, the temperature of the mixing zone and the venting zone is maintained at 160-170°C, the temperature of the cooling zone is 90-110°C, and at the same time, the extrusion pressure of the twin-screw extruder is 10-70MPa.

[0055] Among them, the temperature of the melting stage in step three is 180-230° C., the mixing time is not less than 30 min, the extrusion pressure is 10-70 MPa, and the cooling method adopted in the cooling stage is preferably air cooling.

[0056] Wherein, in step 4, the injection molding temperature of the injection molding machine is 180-230° C., and the injection molding pressure is 40-200 MPa.

[0057] Among them, the performance test in step five includes antibacterial performance test, tensile strength test, impact strength test, bending modulus test and chemical stability test on the prepared antibacterial modified plastic.

[0058] Example 3

[0059] An antibacterial modified plastic formula comprises the following components and their weight parts: 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of crosslinking agent.

[0060] Preferably, the compatibilizer is maleic anhydride grafted polypropylene, and the coupling agent is preferably a silane coupling agent.

[0061] Preferably, the lubricant is stearic acid amide, the dispersant is stearate, and the cross-linking agent is dicumyl peroxide.

[0062] A method for preparing an antibacterial modified plastic, the specific preparation method is as follows:

[0063] Step 1, raw material preparation, prepare 80 parts of polypropylene resin, 5 parts of silver ion antibacterial agent, 5 parts of compatibilizer, 1 part of coupling agent, 0.5 parts of lubricant, 0.5 parts of dispersant, 0.6 parts of antioxidant, 0.4 parts of ultraviolet absorber and 0.6 parts of cross-linking agent;

[0064] Step 2: prepare antibacterial masterbatch, pre-mix, mix the silver ion antibacterial agent, compatibilizer, coupling agent and a small amount of polypropylene resin evenly to form a mixture, and then use a twin-screw extruder to extrude the mixture into antibacterial masterbatch under high temperature and high pressure. In this process, the shearing and kneading action of the twin screw helps to evenly disperse the antibacterial agent in the resin;

[0065] Step 3, preparing antibacterial plastic, adding the remaining polypropylene resin, antibacterial masterbatch, lubricant, dispersant, antioxidant, ultraviolet absorber and crosslinking agent into a high-speed mixer, mixing them evenly, sending the mixed materials into a single-screw or twin-screw extruder, and undergoing the processes of melting, mixing, extruding, cooling and pelletizing to obtain antibacterial modified plastic particles;

[0066] Step 4: Processing and molding: putting the antibacterial modified plastic particles into an injection molding machine, heating and melting them, injecting them into a mold, and demolding them after cooling and solidification to obtain an antibacterial plastic product;

[0067] Step five: performance testing: conducting performance testing on the prepared antibacterial modified plastic.

[0068] The small amount of polypropylene resin added in step 2 accounts for 10% of the total amount, and the polypropylene resin added in step 3 accounts for 90% of the total amount.

[0069] Wherein, the twin-screw extruder in step 2 is composed of a feeding zone, a preheating zone, a melting zone, a mixing zone, a venting zone and a cooling zone. During the process of the twin-screw extruder extruding the mixture under high temperature and high pressure, the temperature of the feeding zone on the twin-screw extruder is 20-50°C, the temperature of the preheating zone is 80-100°C, the temperature of the melting zone is 150-170°C, the temperature of the mixing zone and the venting zone is maintained at 160-170°C, the temperature of the cooling zone is 90-110°C, and at the same time, the extrusion pressure of the twin-screw extruder is 10-70MPa.

[0070] Among them, the temperature of the melting stage in step three is 180-230° C., the mixing time is not less than 30 min, the extrusion pressure is 10-70 MPa, and the cooling method adopted in the cooling stage is preferably air cooling.

[0071] Wherein, in step 4, the injection molding temperature of the injection molding machine is 180-230° C., and the injection molding pressure is 40-200 MPa.

[0072] Among them, the performance test in step five includes antibacterial performance test, tensile strength test, impact strength test, bending modulus test and chemical stability test on the prepared antibacterial modified plastic.

[0073] The antibacterial modified plastics prepared in the above three embodiments were tested for antibacterial properties, tensile strength, impact strength, bending modulus and chemical stability. The test results are as follows:

[0074]

[0075] It can be seen from the above table that the antibacterial modified plastics prepared in Examples 1-3 of the present invention have achieved significant technical effects in terms of antibacterial properties, physical and mechanical properties, chemical stability, processing properties and application prospects. At the same time, the mixing ratio of each component in the raw material can also be freely adjusted and tested according to actual needs.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An antibacterial modified plastic formula, characterized in that: The invention comprises the following components and their weight proportions: 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of crosslinking agent.

2. The antibacterial modified plastic formulation according to claim 1, characterized in that: The compatibilizer is preferably maleic anhydride grafted polypropylene, and the coupling agent is preferably a silane coupling agent.

3. The antibacterial modified plastic formula and preparation method thereof according to claim 1, characterized in that: The lubricant is preferably stearic acid amide, the dispersant is preferably stearate, and the cross-linking agent is preferably dicumyl peroxide.

4. A preparation method, using an antibacterial modified plastic formula according to any one of claims 1 to 3, characterized in that: The specific preparation method is as follows: Step 1, raw material preparation, prepare 60-80 parts of polypropylene resin, 5-8 parts of silver ion antibacterial agent, 3-5 parts of compatibilizer, 1-2 parts of coupling agent, 0.3-0.6 parts of lubricant, 0.3-0.6 parts of dispersant, 0.4-0.8 parts of antioxidant, 0.3-0.5 parts of ultraviolet absorber and 0.5-0.7 parts of cross-linking agent; Step 2: preparing antibacterial masterbatch, pre-mixing, uniformly mixing the silver ion antibacterial agent, compatibilizer, coupling agent and a small amount of polypropylene resin to form a mixture, and then using a twin-screw extruder to extrude the mixture into antibacterial masterbatch under high temperature and high pressure; Step 3, preparing antibacterial plastic, adding the remaining polypropylene resin, antibacterial masterbatch, lubricant, dispersant, antioxidant, ultraviolet absorber and crosslinking agent into a high-speed mixer, mixing them evenly, sending the mixed materials into a single-screw or twin-screw extruder, and undergoing the processes of melting, mixing, extruding, cooling and pelletizing to obtain antibacterial modified plastic particles; Step 4: Processing and molding: putting the antibacterial modified plastic particles into an injection molding machine, heating and melting them, injecting them into a mold, and demolding them after cooling and solidification to obtain an antibacterial plastic product; Step five: performance testing: conducting performance testing on the prepared antibacterial modified plastic.

5. The method for preparing an antibacterial modified plastic according to claim 4, characterized in that: The small amount of polypropylene resin added in step 2 accounts for 10% of the total amount, and the polypropylene resin added in step 3 accounts for 90% of the total amount.

6. The method for preparing an antibacterial modified plastic according to claim 4, characterized in that: In the step 2, the twin-screw extruder consists of a feeding zone, a preheating zone, a melting zone, a mixing zone, a venting zone and a cooling zone. When the twin-screw extruder extrude the mixture under high temperature and high pressure, the temperature of the feeding zone on the twin-screw extruder is 20-50°C, the temperature of the preheating zone is 80-100°C, the temperature of the melting zone is 150-170°C, the temperature of the mixing zone and the venting zone is maintained at 160-170°C, the temperature of the cooling zone is 90-110°C, and the extrusion pressure of the twin-screw extruder is 10-70MPa.

7. The method for preparing an antibacterial modified plastic according to claim 4, characterized in that: In the step 3, the temperature of the melting stage is 180-230° C., the mixing time is not less than 30 min, the extrusion pressure is 10-70 MPa, and the cooling method adopted in the cooling stage is preferably air cooling.

8. The method for preparing an antibacterial modified plastic according to claim 4, characterized in that: In the step 4, the injection molding temperature of the injection molding machine is 180-230° C., and the injection molding pressure is 40-200 MPa.

9. The method for preparing an antibacterial modified plastic according to claim 4, characterized in that: The performance test in step five includes conducting an antibacterial performance test, a tensile strength test, an impact strength test, a flexural modulus test and a chemical stability test on the prepared antibacterial modified plastic.