Bacteriostatic and antibacterial polymer composite master batch and preparation method thereof

By forming stable click connections and chemical bonds on graphene to bind triclosan, combined with the polar characteristics of nylon 6, the problem of dispersion and stability of graphene-loaded triclosan in textile products is solved, and the antibacterial inhibitory effect is significantly improved. Bacterial performance and durability ensure effective destruction of bacteria.

CN118725552APending Publication Date: 2024-10-01NINGBO GRAPHENE INNOVATION CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410778629.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing graphene-loaded triclosan antibacterial materials have problems such as poor dispersion, unstable antibacterial effect and insufficient durability in textile products, and the commonly used fixation methods have hidden dangers to human safety.

Method used

Nylon 6 is used as the polymer matrix, and photoinitiators and catalysts are used to promote the reaction between pentaerythritol tetrakis-3-mercaptopropionate and graphene oxide to form a stable click connection, combined with triclosan, and silane coupling agent and titanate are used The coupling agent improves the dispersion and stability of the antibacterial filler, and the antibacterial composite masterbatch is prepared through a twin-screw extruder.

Benefits of technology

Improves the dispersion and stability of antibacterial fillers in textile materials, enhances antibacterial and bacteriostatic properties and durability, ensures effective destruction of bacterial cell membranes, and the polar compatibility of the material improves the binding force with fibers .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004896450220000091
    Figure BDA0004896450220000091
  • Figure BDA0004896450220000101
    Figure BDA0004896450220000101
Patent Text Reader

Abstract

The invention discloses a bacteriostatic and antibacterial polymer composite master batch and a preparation method thereof. The master batch is prepared from the following raw materials in parts by weight: 90-99 parts of a polymer matrix, 5-10 parts of antibacterial filler, 1-5 parts of a plasticizer, 1-3 parts of a surface coupling agent and 1-3 parts of a compatilizer. According to the antibacterial filler disclosed by the invention, under the action of a photoinitiator, a click reaction is initiated between sulfydryl of pentaerythritol tetra-3-mercaptopropionate and an available sp2 carbon binding site in a graphene structure in an ultraviolet crosslinking manner to form a saturated structure, the sulfydryl is introduced to the surface of graphene, the pentaerythritol tetra-3-mercaptopropionate is polythiol, and the polythiol is added to the surface of the graphene, so that the antibacterial filler is prepared. According to the present invention, the graphene oxide and the triclosan are modified, such that the reaction with the graphene oxide and the reaction with the triclosan are achieved so as to improve the combination firmness between the triclosan and the graphene, the antibacterial and antibacterial performance of the triclosan chemical level is obtained after the modification, the damage to the bacterial cell membrane can be rapidly completed, and the antibacterial performance of the master batch is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer composite masterbatches, and more specifically to an antibacterial and antimicrobial polymer composite masterbatch and a preparation method thereof. Background Art

[0002] Graphene is a carbon atom in the form of sp 2 The nanomaterial with a two-dimensional sheet structure formed by hybrid bonding into a single-layer hexagonal honeycomb lattice has excellent thermal, mechanical and electrical properties. In recent years, scientists have discovered that graphene can be inserted into the bacterial cell membrane for physical cutting, and can also extract phospholipid molecules on the cell membrane on a large scale, thereby destroying the cell membrane and killing bacteria to achieve antibacterial and antibacterial effects. Textile products are common items in daily life. With the gradual improvement of people's living standards, people have put forward higher performance requirements for them, especially in response to super bacteria and large-scale epidemic bacteria that have appeared in recent years. Therefore, the application of graphene in antibacterial materials is of great significance. However, the easy aggregation of graphene itself makes it difficult to achieve a good dispersion effect in the matrix, and the antibacterial and antibacterial ability of graphene is a physical effect, and the antibacterial and antibacterial ability needs to be improved.

[0003] Triclosan, also known as triclosan (TCS), contains three chlorine atoms and one hydroxyl group on its surface. It is a polar molecule with high-efficiency and broad-spectrum antibacterial properties. Currently, most of the patents on graphene-loaded triclosan are carried out through the π-π conjugation, hydrogen bonding and electrostatic attraction of graphene. These effects are not carried out through chemical bonding and are unstable. In addition, the current patents on graphene-loaded triclosan are usually prepared into antibacterial liquid first, and then the fiber is impregnated, rolled or coated, and finally the antibacterial agent is fixed on the fiber through high-temperature baking or other drying methods. However, there are problems in the antibacterial effect, durability, and safety of the dissolved matter of the fabric obtained by this method to the human body. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present application provides an antibacterial and antimicrobial polymer composite masterbatch with good antibacterial properties and stability.

[0005] In order to solve the above technical problems, the technical solution adopted in the present application is: an antibacterial and antimicrobial polymer composite masterbatch, the raw materials for preparing the masterbatch include: 90-99 parts by weight of polymer matrix, 5-10 parts by weight of antibacterial filler, 1-5 parts by weight of plasticizer, 1-3 parts by weight of surface coupling agent, and 1-3 parts by weight of compatibilizer.

[0006] Furthermore, the polymer matrix material is nylon 6 (PA6), commonly known as nylon, which is the earliest synthetic fiber variety in the world; it has a series of advantages such as high strength, wear resistance, and good resilience, and has been widely used in the field of fiber fabrics for pure spinning and blending into various clothing and knitwear; compared with other nylons, nylon 6 has a lower melting point of about 220°C, and is easier to process in terms of technology.

[0007] Furthermore, the plasticizer is polyethylene wax or PEG (polyethylene glycol).

[0008] Furthermore, the surface coupling agent is one of a silane coupling agent or a titanate coupling agent; specifically, the silane coupling agent may be KH-792, tetraisopropyl di(dioctyl phosphite) titanate, and the like.

[0009] Furthermore, the compatibilizer is stearic acid or ABS-g-MAH (maleic anhydride grafted ABS resin compatibilizer).

[0010] Furthermore, the specific preparation method of the antibacterial filler includes:

[0011] (1) adding graphene oxide to ethanol to prepare a dispersion, mixing and stirring evenly, and then ultrasonically reacting at room temperature to obtain a uniform dispersion a;

[0012] (2) adding a photoinitiator and pentaerythritol tetrakis-3-mercaptopropionate to the dispersion a obtained in step (1) in sequence, stirring and mixing until uniform, and then ultrasonicating at 40-50° C. for 20-40 minutes to obtain a uniform mixture a;

[0013] (3) placing the mixture a under a UV lamp and irradiating the mixture for 3-5 hours at a power of 15-25 mW / cm2. After the reaction is completed, the mixture is centrifuged to remove the unreacted material to obtain a modified solution a;

[0014] (4) adding triclosan and a catalyst to the modified liquid a obtained in step (3), stirring and reacting at 40-60° C., and obtaining a modified liquid b after sufficient reaction;

[0015] (5) spray-drying the modified liquid b obtained in step (4) to obtain an antibacterial filler.

[0016] Furthermore, the concentration of graphene oxide in the dispersion a described in step (1) is 5-10 mg / mL.

[0017] Furthermore, the dosage ratio of the photoinitiator and pentaerythritol tetrakis-3-mercaptopropionate described in step (2) is: 15-25 mg: 1.5-2 ml (pentaerythritol tetrakis-3-mercaptopropionate is added to maintain excess; the above ratio can be proportionally expanded or reduced as needed), and the mass ratio of the photoinitiator to the graphene oxide in the dispersion a is 1:24-80.

[0018] Furthermore, the catalyst described in step (4) can be at least one of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, dialkyltin dimaleate, alkyltin dithiolate, and the like.

[0019] Furthermore, the mass ratio of triclosan in step (4) to graphene oxide in dispersion a is 1-5:5, and the dosage ratio of the catalyst to triclosan is 1:15-25.

[0020] The present application also provides a method for preparing the above-mentioned antibacterial and antimicrobial polymer composite masterbatch, the specific process comprising:

[0021] (1) adding 90-99 parts by weight of a polymer matrix, 1-10 parts by weight of an antibacterial filler, 1-5 parts by weight of a plasticizer, 1-3 parts by weight of a surface coupling agent, and 1-3 parts by weight of a compatibilizer into a high-speed mixer according to a formula ratio, and mixing the mixture for 10-40 minutes to obtain a mixed masterbatch;

[0022] (2) The mixed masterbatch is then extruded using a twin-screw extruder at an extrusion temperature of 210-260° C. to obtain a masterbatch.

[0023] Furthermore, the 90-99 polymer matrix is ​​divided into two parts, and the polymer matrix, surface coupling agent and antibacterial filler of one part are first added to a high-speed mixer and stirred at a speed of 300-600rpm for 10-20min; then the compatibilizer, toughening agent and the second part of the polymer matrix are added and stirred at a speed of 300-600rpm for 10-20min to obtain a mixed masterbatch; the present application can further improve the dispersibility of the antibacterial filler and reduce agglomeration by adding the polymer matrix twice and stirring it in a high-speed mixer.

[0024] Advantages and beneficial effects of this application:

[0025] 1. The preparation process of the antibacterial filler of the present application adopts the method of ultraviolet crosslinking under the action of a photoinitiator to induce a click reaction between the thiol group of pentaerythritol tetrakis-3-mercaptopropionate and the available sp2 carbon binding sites in the graphene structure to form a saturated structure, and the thiol group is introduced into the graphene surface. Pentaerythritol tetrakis-3-mercaptopropionate is a polythiol, so that it can react with graphene oxide on one side and with triclosan on the other side, thereby improving the bonding strength between triclosan and graphene. In this process, if the amount of photoinitiator used is too small, very few free radicals are generated, and the reaction speed is too slow, which affects the efficiency of the reaction. If the amount of initiator used is too large, too many free radicals are generated in a very short time, and the rate at which the free radicals collide with each other and terminate the reaction will be greatly increased, which is also not conducive to the reaction. Therefore, the mass ratio of the photoinitiator to the graphene oxide is 1:24-80.

[0026] 2. The present application uses the action of a catalyst to combine the mercapto group with the highly active hydroxyl group in triclosan to obtain a triclosan-graphene oxide modified material with stable chemical bonds; this is because the Sn in the specific catalyst used in the present application 2+ It has two empty orbitals and is easy to form coordination complex with some substances with lone pair electrons. Through the formation and decomplexation of the complex structure, it can catalyze the hydroxyl group and promote the combination of the highly active hydroxyl group in triclosan with the thiol group on the modified graphene oxide to form a stable covalent bond. The covalent bond force is much higher than the hydrogen bond and electrostatic attraction. Moreover, this stability is reflected by comparing the antibacterial rate of the masterbatch spinning fabric made of the triclosan-graphene oxide modified material with the masterbatch spinning fabric made of the unmodified graphene oxide and triclosan directly after washing, which fully demonstrates that the antibacterial stability and durability of the masterbatch of the present application are stronger.

[0027] 3. The matrix material used for the raw material preparation of the masterbatch of the present application is nylon 6, which has polar nitrogen atoms and carbonyl groups on its molecular chain and is a polar polymer; triclosan contains polar chlorine atoms and hydroxyl groups on its surface and is also a polar compound; because triclosan is combined with the surface of graphene, the modified graphene has a similar polarity to nylon 6 and is therefore easier to combine with nylon 6, so that the antibacterial filler has better dispersibility in nylon, and the masterbatch finally obtained has ideal antibacterial properties; after modification with triclosan, the antibacterial and antimicrobial ability of graphene is further improved, and graphene itself has physical antibacterial and antibacterial capabilities. After modification, the antibacterial and antibacterial properties of triclosan at the chemical level are obtained, which can destroy the bacterial cell membrane more quickly, further improving the antibacterial properties of the composite material. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only preferred embodiments, not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Antibacterial filler Example 1

[0030] 1. Add graphene oxide to ethanol to prepare a dispersion (5 mg / mL), mix and stir evenly, and then ultrasonicate at room temperature for 1 h to obtain a uniform dispersion a;

[0031] 2. Add 15 mg of photoinitiator (2,2-dimethoxy-phenylacetophenone) and 1.5 mL of pentaerythritol tetrakis-3-mercaptopropionate to 120 mL of dispersion a in sequence, stir and mix evenly, and then ultrasonicate at 45° C. for 30 minutes to obtain a uniform mixture a;

[0032] 3. Place mixture a under UV light and react for 180 minutes at a UV light power of 20 mW / cm 2 After the reaction is completed, the unreacted material is removed by centrifugation to obtain a modified liquid a;

[0033] 4. Add 0.1 g of triclosan and 5 mg of dibutyltin dilaurate to 100 mL of modified liquid a, stir and react at 40°C, and after fully reacting for 24 hours, obtain modified liquid b.

[0034] 5. The modified liquid b is spray-dried to obtain an antibacterial filler.

[0035] Antibacterial filler Example 2

[0036] 1. Add graphene oxide to ethanol to prepare a dispersion (10 mg / mL), mix and stir evenly, and then ultrasonicate at room temperature for 1 h to obtain a uniform dispersion a;

[0037] 2. Add 20 mg of photoinitiator (2,2-dimethoxy-phenylacetophenone) and 1.5 mL of pentaerythritol tetrakis-3-mercaptopropionate to 120 mL of dispersion a in sequence, stir and mix evenly, and then ultrasonicate at 45° C. for 30 minutes to obtain a uniform mixture a;

[0038] 3. Place mixture a under UV light and react for 180 minutes at a UV light power of 20 mW / cm 2 After the reaction is completed, the unreacted material is removed by centrifugation to obtain a modified liquid a;

[0039] 4. Add 0.45 g of triclosan and 22.5 mg of dibutyltin dilaurate into 100 mL of modified liquid a, stir and react at 50°C. After fully reacting for 24 hours, modified liquid b is obtained.

[0040] 5. The modified liquid b is spray-dried to obtain an antibacterial filler.

[0041] Antibacterial filler example 3

[0042] 1. Add graphene oxide to ethanol to prepare a dispersion (10 mg / mL), mix and stir evenly, and then ultrasonicate at room temperature for 1 h to obtain a uniform dispersion a;

[0043] 2. Add 25 mg of photoinitiator (2,2-dimethoxy-phenylacetophenone) and 1.5 mL of pentaerythritol tetrakis-3-mercaptopropionate to 120 mL of mixture a in sequence, stir and mix evenly, and then ultrasonicate at 45° C. for 30 minutes to obtain a uniform mixture a;

[0044] 3. Place mixture a under UV light and react for 180 minutes at a UV light power of 20 mW / cm 2 After the reaction is completed, the unreacted material is removed by centrifugation to obtain a modified liquid a;

[0045] 4. Add 1 g of triclosan and 50 mg of dibutyltin dilaurate to 100 mL of modified liquid a, stir and react at 40°C. After fully reacting for 24 hours, modified liquid b is obtained.

[0046] 5. The modified liquid b is spray-dried to obtain an antibacterial filler.

[0047] Antibacterial filler embodiment 4

[0048] 1. Add graphene oxide to ethanol to prepare a dispersion (10 mg / mL), mix and stir evenly, and then ultrasonicate at room temperature for 1 h to obtain a uniform dispersion a;

[0049] 2. Directly dry the dispersion a by spray drying to obtain graphene powder.

[0050] Masterbatch Example 1

[0051] The first step: add 50 parts of a polymer matrix, 2 parts of a surface coupling agent (titanium ester coupling agent (tetraisopropyl di(dioctyl phosphite) titanate)), and 5 parts of an antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 15 minutes, then add 2 parts of stearic acid, 3 parts of polyethylene wax, and 45 parts of a polymer matrix and continue stirring for 15 minutes to obtain a mixed masterbatch; the antibacterial filler is prepared as in Example 1.

[0052] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0053] Masterbatch Example 2

[0054] Step 1: Add 50 parts of polymer matrix, 3 parts of surface coupling agent (titanate coupling agent (tetraisopropyl di (dioctyl phosphite) titanate)), and 10 parts of antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 20 minutes, then add 3 parts of stearic acid, 5 parts of polyethylene wax, and 40 parts of polymer matrix and continue stirring for 20 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared in Example 1.

[0055] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0056] Masterbatch Example 3

[0057] The first step: add 50 parts of a polymer matrix, 1 part of a surface coupling agent (silane coupling agent KH-792), and 1 part of an antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 5 minutes, then add 1 part of stearic acid, 1 part of polyethylene wax, and 49 parts of a polymer matrix and continue stirring for 5 minutes to obtain a mixed masterbatch; the antibacterial filler is prepared as in Example 2.

[0058] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0059] Masterbatch Example 4

[0060] The first step: add 50 parts of a polymer matrix, 1.5 parts of a surface coupling agent (silane coupling agent KH-792), and 3 parts of an antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 5 minutes, then add 1.5 parts of stearic acid, 2 parts of polyethylene wax, and 47 parts of a polymer matrix and continue stirring for 10 minutes to obtain a mixed masterbatch; the antibacterial filler is prepared as in Example 2.

[0061] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0062] Masterbatch Example 5

[0063] The first step: add 50 parts of a polymer matrix, 2 parts of a surface coupling agent (silane coupling agent KH-792), and 5 parts of an antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 10 minutes, then add 2 parts of stearic acid, 3 parts of polyethylene wax, and 45 parts of a polymer matrix and continue stirring for 10 minutes to obtain a mixed masterbatch; the antibacterial filler is prepared in Example 2.

[0064] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0065] Masterbatch Example 6

[0066] The first step: add 50 parts of a polymer matrix, 3 parts of a surface coupling agent (titanium ester coupling agent (tetraisopropyl di(dioctyl phosphite) titanate)), and 10 parts of an antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 15 minutes, then add 3 parts of stearic acid, 5 parts of polyethylene wax, and 40 parts of a polymer matrix and continue stirring for 15 minutes to obtain a mixed masterbatch; the antibacterial filler is prepared as in Example 2.

[0067] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0068] Masterbatch Example 7

[0069] Step 1: Add 50 parts of polymer matrix, 1 part of surface coupling agent (silane coupling agent KH-792), and 1 part of antibacterial filler into a high-speed mixer, stir at 300-600 rpm for 5 minutes, then add 1 part of stearic acid, 1 part of polyethylene wax, and 49 parts of polymer matrix and continue stirring for 5 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared in Example 3.

[0070] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0071] Masterbatch Example 8

[0072] Step 1: Add 50 parts of polymer matrix, 1.5 parts of surface coupling agent (silane coupling agent KH-792), and 3 parts of antibacterial filler into a high-speed mixer, stir at 300-600 rpm for 5 minutes, then add 1.5 parts of stearic acid, 2 parts of polyethylene wax, and 47 parts of polymer matrix and continue stirring for 10 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared in Example 3.

[0073] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0074] Masterbatch Example 9

[0075] Step 1: Add 50 parts of polymer matrix, 2 parts of surface coupling agent (silane coupling agent KH-792), and 6 parts of antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 10 minutes, then add 2 parts of stearic acid, 3 parts of polyethylene wax, and 44 parts of polymer matrix and continue stirring for 15 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared in Example 3.

[0076] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0077] Masterbatch Example 10

[0078] Step 1: Add 50 parts of polymer matrix, 3 parts of surface coupling agent (titanate coupling agent (tetraisopropyl di(dioctyl phosphite) titanate)), and 6 parts of antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 15 minutes, then add 3 parts of stearic acid, 5 parts of polyethylene wax, and 40 parts of polymer matrix and continue stirring for 15 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared in Example 3.

[0079] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0080] Comparative Example 1

[0081] The first step: add 50 parts of a polymer matrix, 2 parts of a surface coupling agent (titanium ester coupling agent (tetraisopropyl di(dioctyl phosphite) titanate)), and 5 parts of an antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 15 minutes, then add 2 parts of stearic acid, 3 parts of polyethylene wax, and 45 parts of a polymer matrix and continue stirring for 15 minutes to obtain a mixed masterbatch; the antibacterial filler is prepared according to Example 4, that is, the antibacterial filler does not contain triclosan.

[0082] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0083] Comparative Example 2

[0084] Step 1: Add 50 parts of polymer matrix, 3 parts of surface coupling agent (titanate coupling agent (tetraisopropyl di(dioctyl phosphite) titanate)), and 10 parts of antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 20 minutes, then add 3 parts of stearic acid, 5 parts of polyethylene wax, and 40 parts of polymer matrix and continue stirring for 20 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared as in Example 4, that is, the antibacterial filler does not contain triclosan.

[0085] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0086] Comparative Example 3

[0087] Step 1: Add 50 parts of polymer matrix, 1 part of surface coupling agent (silane coupling agent KH-792), and 1 part of antibacterial filler into a high-speed mixer, stir at a speed of 300-600 rpm for 5 minutes, then add 1 part of stearic acid, 1 part of polyethylene wax, and 49 parts of polymer matrix and continue stirring for 5 minutes to obtain a mixed masterbatch. The antibacterial filler is prepared in Example 1.

[0088] Step 2: Place the mixed masterbatch into a parallel twin-screw extruder, extrude it at a temperature of 210-260°C, cool it in a water tank, cool it in air, and pelletize it to obtain the antibacterial composite masterbatch.

[0089] Table 1 is a table showing the dosage ratios of the main raw materials in the examples and comparative examples of the present application.

[0090] Example Polymer matrix Antibacterial filler Plasticizers Surface coupling agent Compatibilizer Example 1 95 5 Example 1 3 2 2 Example 2 90 10 Example 1 5 3 3 Example 3 99 1 Example 2 1 1 1 Example 4 97 3 Example 2 2 1.5 1.5 Example 5 95 5 Example 2 3 2 2 Example 6 90 10 Example 2 5 3 3 Example 7 99 1 Embodiment 3 1 1 1 Example 8 97 3 Embodiment 3 2 1.5 1.5 Example 9 94 6 Embodiment 3 3 2 2 Example 10 90 10 Example 3 5 3 3 Comparative Example 1 95 5 Example 4 3 2 2 Comparative Example 2 90 10 Example 4 5 3 3 Comparative Example 3 99 1 Embodiment 1 1 1 1

[0091] Then, the performance of the masterbatch obtained in the above-mentioned embodiments and comparative examples of the present application was tested, mainly for antibacterial and antimicrobial properties: the test was conducted according to the evaluation test method for antibacterial properties of textiles in GB / T 20944.3-2008; the deodorization performance: the test was conducted according to the test method in the test of deodorization properties of textiles in GB T 33610.2-2019; the results are shown in Table 2 below:

[0092] Table 2 Antibacterial and antimicrobial properties of masterbatches prepared in Examples and Comparative Examples

[0093]

[0094]

[0095] The above test results show that the masterbatch prepared by adding the specific antibacterial filler of the present application can have more ideal antibacterial and antibacterial properties. This high antibacterial and antibacterial property is based on the Sn in the catalyst. 2+It has two empty orbitals and is easy to form coordination complexes with some substances with lone pairs of electrons. Through the formation and decomplexation of the complex structure, it can catalyze the hydroxyl group and promote the combination of the highly active hydroxyl group in triclosan with the thiol group on the modified graphene oxide to form a stable covalent bond. The force of the covalent bond is much higher than the hydrogen bond and the electrostatic attraction. The antibacterial rate of the masterbatch spinning fabric made of the triclosan-graphene oxide modified material stabilized by chemical bonds is compared with the antibacterial rate of the masterbatch spinning fabric made by directly mixing graphene oxide and triclosan without modification after washing. It is found that the antibacterial stability and durability of the masterbatch prepared by this scheme of the present application are stronger; in the above table, the masterbatch is spun into fabric, and the antibacterial rate measured after washing the fabric 50 / 100 times shows that the masterbatch prepared by the scheme of the present application has ideal antibacterial durability.

Claims

1. An antibacterial and antimicrobial polymer composite masterbatch, characterized in that: The raw materials for preparing the masterbatch include: 90-99 parts by weight of polymer matrix, 5-10 parts by weight of antibacterial filler, 1-5 parts by weight of plasticizer, 1-3 parts by weight of surface coupling agent, and 1-3 parts by weight of compatibilizer.

2. The antibacterial and antimicrobial polymer composite masterbatch according to claim 1, characterized in that: The polymer matrix material is nylon 6.

3. The antibacterial and antimicrobial polymer composite masterbatch according to claim 1, characterized in that: The plasticizer is polyethylene wax or PEG.

4. The antibacterial and antimicrobial polymer composite masterbatch according to claim 1, characterized in that: The surface coupling agent is a silane coupling agent or a titanate coupling agent.

5. The antibacterial and antimicrobial polymer composite masterbatch according to claim 1, characterized in that: The compatibilizer is stearic acid or ABS-g-MAH.

6. The antibacterial and antimicrobial polymer composite masterbatch according to claim 1, characterized in that: The specific preparation process of the antibacterial filler includes: (1) adding graphene oxide to ethanol to prepare a dispersion, mixing and stirring evenly, and then ultrasonically reacting at room temperature to obtain a uniform dispersion a; (2) adding a photoinitiator and pentaerythritol tetrakis-3-mercaptopropionate to the dispersion a obtained in step (1) in sequence, stirring and mixing until uniform, and then ultrasonicating at 40-50° C. for 20-40 minutes to obtain a uniform mixture a; (3) placing the mixture a under a UV lamp and irradiating the mixture for 3-5 hours at a power of 15-25 mW / cm2. After the reaction is completed, the mixture is centrifuged to remove the unreacted material to obtain a modified solution a; (4) adding triclosan and a catalyst to the modified liquid a obtained in step (3), stirring and reacting at 40-60° C., and obtaining a modified liquid b after sufficient reaction; (5) spray-drying the modified liquid b obtained in step (4) to obtain an antibacterial filler.

7. The antibacterial and antimicrobial polymer composite masterbatch according to claim 6, characterized in that: The concentration of graphene oxide in the dispersion a described in step (1) is 5-10 mg / mL.

8. The antibacterial and antimicrobial polymer composite masterbatch according to claim 6, characterized in that: The dosage ratio of the photoinitiator and pentaerythritol tetrakis-3-mercaptopropionate in step (2) is: 15-25 mg: 1.5-2 ml, and the mass ratio of the photoinitiator to the graphene oxide in the dispersion a is 1:24-80.

9. The antibacterial and antimicrobial polymer composite masterbatch according to claim 6, characterized in that: The catalyst described in step (4) is at least one of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, dialkyltin dimaleate, and alkyltin dithiolate.

10. The antibacterial and antimicrobial polymer composite masterbatch according to claim 6, characterized in that: The mass ratio of triclosan in step (4) to graphene oxide in dispersion a is 1-5:5, and the dosage ratio of the catalyst to triclosan is 1:15-25.

11. A method for preparing the antibacterial and antimicrobial polymer composite masterbatch according to any one of claims 1 to 10, characterized in that: The specific process includes: (1) adding 90-99 parts by weight of a polymer matrix, 1-10 parts by weight of an antibacterial filler, 1-5 parts by weight of a plasticizer, 1-3 parts by weight of a surface coupling agent, and 1-3 parts by weight of a compatibilizer into a high-speed mixer according to a formula ratio, and mixing the mixture for 10-40 minutes to obtain a mixed masterbatch; (2) The mixed masterbatch is then extruded using a twin-screw extruder at an extrusion temperature of 210-260° C. to obtain a masterbatch.

12. The method for preparing the antibacterial and antimicrobial polymer composite masterbatch according to claim 11, characterized in that: The 90-99 polymer matrix is ​​divided into two parts. First, the polymer matrix, surface coupling agent and antibacterial filler of one part are added into a high-speed mixer and stirred at a speed of 300-600 rpm for 10-20 minutes; then the compatibilizer, toughening agent and the second polymer matrix are added and stirred at a speed of 300-600 rpm for 10-20 minutes to obtain a mixed masterbatch.