Anti-aging coating with damage early warning and corrosion inhibition functions and preparation method
By combining coating resin, corrosion inhibitor composite nanoclay and crystal violet lactone microcapsules in the organic coating, a coating with damage warning and corrosion inhibition functions is realized, which solves the problems of damage and aging of coatings in the existing technology. It improves the aging resistance and corrosion resistance of the coating.
Patent Information
- Application Number
- CN202410921005.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-01
AI Technical Summary
When existing organic anti-corrosion coatings face mechanical damage, aging degradation and corrosion damage, they lack universal research and development strategies that combine damage warning functions and aging and corrosion resistance, resulting in deficiencies in extending their service life.
Using a combination of coating resin, corrosion inhibitor composite nano-clay and crystal violet lactone microcapsules, the coating resin and corrosion inhibitor composite nano-clay are mixed, and the crystal violet lactone microcapsules are released at the damaged area to achieve early warning of damage, and in the damaged area When reaching the metal substrate, the corrosion inhibitor composite nanoclay releases the corrosion inhibitor to inhibit corrosion.
The coating's damage warning function is timely and corrosion-inhibiting performance is achieved, and it can adapt to different light environments, extend the service life of the coating, and reduce production costs.
Smart Images

Figure CN118725627A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of anti-corrosion coating materials, in particular to an anti-aging coating with damage early warning and corrosion inhibition functions and a preparation method thereof. Background Art
[0002] Organic coatings can effectively isolate metal materials from direct contact with corrosive media by forming a physical barrier to extend the service life of metal substrates. However, they face challenges of various forms of coupled damage, including mechanical damage, aging degradation, and corrosion damage. On the one hand, macroscopic damage caused by mechanical action directly damages the structural integrity of the coating substrate; on the other hand, exposure to aging conditions such as ultraviolet radiation and water / humidity can lead to the rupture of polymer chains, forming various microscopic defects, pores or cracks. Although microscopic defects do not immediately destroy the barrier properties of the coating, their formation promotes the entry of corrosive media, thereby gradually weakening and ultimately greatly damaging the protective effect of the coating on the metal. Therefore, giving the coating the ability to respond intelligently to damage, as well as enhancing the weather resistance and corrosion resistance of polymer coatings, is crucial to extending the service life of organic coatings.
[0003] However, most of the current design and development work on organic anti-corrosion coatings only focuses on one aspect, either the intelligent response function or the aging and corrosion resistance. In addition, the coating resins used and the applicable environment are often single, and there is a lack of universal research and development strategies for coatings that have both damage warning functions and aging and corrosion resistance.
[0004] Therefore, it is urgent to develop an anti-corrosion coating system that has both coating damage warning function and aging and corrosion resistance. Summary of the invention
[0005] In order to solve the above problems, the technical solution of the present invention provides an aging-resistant coating with damage warning and corrosion inhibition functions and a preparation method, which can have both the coating damage warning function and aging and corrosion resistance, thereby improving the functionality of the coating.
[0006] According to the first aspect of the technical solution of the present invention, there is provided an anti-aging coating with damage warning and corrosion inhibition functions, which is applied to a metal substrate and includes a coating resin, a corrosion inhibitor composite nanoclay and a plurality of crystal violet lactone microcapsules, wherein the coating resin and the corrosion inhibitor composite nanoclay are mixed, and the plurality of crystal violet lactone microcapsules are dispersed in the mixture of the coating resin and the corrosion inhibitor composite nanoclay;
[0007] The crystal violet lactone microcapsule comprises a microcapsule wall and crystal violet lactone encapsulated in the microcapsule wall;
[0008] When the damage of the coating does not reach the metal substrate, the crystal violet lactone is released from the microcapsule wall to the damaged area of the coating, making the color of the damaged area different from that of other areas of the coating;
[0009] When the damage of the coating reaches the metal substrate, the corrosion inhibitor composite nanoclay releases the corrosion inhibitor at the damaged location.
[0010] In the above scheme, the coating resin is one or more of epoxy resin, acrylic resin, alkyd resin, polyurethane resin, polyester resin, polyurea resin, fluorocarbon resin, polyolefin resin, phenolic resin, and silicone resin.
[0011] In the above scheme, the corrosion inhibitor in the corrosion inhibitor composite nanoclay includes inorganic salts and / or organic small molecules.
[0012] In the above scheme, the nanoclay in the corrosion inhibitor composite nanoclay includes one or more of halloysite, montmorillonite, diatomaceous earth, kaolin, and bentonite.
[0013] In the above scheme, the microcapsule wall includes one or more of polyurethane, polyurea, phenolic resin, urea-formaldehyde resin, and epoxy resin.
[0014] In the above scheme, the corrosion inhibitor composite nanoclay accounts for 0.3wt.% to 5wt.% of the coating mass fraction, and the crystal violet lactone microcapsules account for 2.5wt.% to 15wt.% of the coating mass fraction.
[0015] In the above solution, the thickness of the coating is 60 μm to 300 μm.
[0016] According to a second aspect of the technical solution of the present invention, there is provided a method for preparing an aging-resistant coating having damage warning and corrosion inhibition functions, comprising:
[0017] S1. Evenly disperse 0.5 g to 5 g of nanoclay and 5 g to 15 g of corrosion inhibitor in a mixed solvent of water and dimethyl sulfoxide in a volume ratio of 1:4, immerse for 24 h to 96 h, and obtain corrosion inhibitor composite nanoclay by centrifugation;
[0018] S2, dissolving 0.5 g to 2 g of crystal violet lactone and 0.5 g to 2 g of resin prepolymer in 5 mL to 25 mL of phenyl acetate or ethyl phenyl acetate as the oil phase, using a polyvinyl alcohol aqueous solution with a mass fraction of 0.5 wt.% to 5 wt.% as the water phase, dispersing the two by ultrasonic to obtain an oil-in-water emulsion, adding a resin curing agent to perform in-situ interfacial polymerization, and obtaining crystal violet lactone microcapsules;
[0019] S3. Evenly mix the corrosion inhibitor composite nanoclay, the crystal violet lactone microcapsules and the coating resin, evenly apply them on the surface of the metal substrate by spin coating or dip coating, and cure for 6h to 48h to obtain an aging-resistant coating with damage warning and corrosion inhibition functions.
[0020] In the above scheme, the loading rate of the corrosion inhibitor is 5wt.% to 30wt.%.
[0021] In the above scheme, the coverage rate of the crystal violet lactone is 15wt.% to 40wt.%.
[0022] Beneficial effects of the present invention:
[0023] The present invention discloses an aging-resistant coating with damage warning and corrosion inhibition functions and a preparation method thereof. Once the surface of the coating is damaged, the microcapsule wall is broken and the crystal violet lactone flows out, which can present local fluorescence enhancement in a dark environment and can be combined with nanoclay to present blue in a bright environment to adapt to different application scenarios with bright or dark light. Moreover, direct and timely warning can be given after the surface is damaged, without the stimulation or reaction of other factors, especially without the addition of corrosive media. When the coating damage reaches the metal substrate, the corrosion inhibitor composite nanoclay releases the corrosion inhibitor at the damaged part to inhibit the corrosion process of the metal substrate. The preparation process of the present invention is simple, the production cost is low, the damage warning performance, corrosion inhibition performance and aging resistance of the coating are good, and the coating has universality and a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0025] Figure 1 This is a transmission electron microscopic image of the corrosion inhibitor composite halloysite prepared in Example 1 of the present invention;
[0026] Figure 2 is a scanning electron microscope image of the crystal violet lactone microcapsules prepared in Example 1 of the present invention;
[0027] Figure 3 This is a schematic diagram of the acrylic resin coating of the corrosion inhibitor composite halloysite and crystal violet lactone microcapsules prepared in Example 1 of the present invention after the surface is damaged under visible light;
[0028] Figure 4It is a schematic diagram of the acrylic resin coating of the corrosion inhibitor composite halloysite and crystal violet lactone microcapsules prepared in Example 1 of the present invention after the surface is damaged under ultraviolet light;
[0029] Figure 5 This is a schematic diagram of the pure acrylic resin coating surface under visible light after being damaged in Comparative Example 1 of the present invention;
[0030] Figure 6 This is a schematic diagram of the pure acrylic resin coating under ultraviolet light after the surface is damaged in Comparative Example 1 of the present invention;
[0031] Figure 7 The curve diagrams are shown for Example 2 of the present invention and Comparative Example 2 when they were immersed for 1 day and 7 days respectively after being scratched.
[0032] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0033] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present disclosure. Instead, they are merely examples of devices and methods consistent with some aspects of the present disclosure as detailed in the appended claims.
[0034] The terms "first", "second", etc. in the specification and claims of the present disclosure are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchanged where appropriate, so that the embodiments of the present disclosure described herein can be implemented in an order other than those illustrated or described herein, for example.
[0035] In addition, the terms "comprises," "comprising," and "having," and any variations thereof, are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or apparatus that includes a series of steps or elements is not necessarily limited to those steps or elements explicitly listed, but may include other steps or elements not explicitly listed or inherent to such process, method, product, or apparatus.
[0036] Multiple includes two or more.
[0037] It should be understood that the term "and / or" used in this disclosure is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone.
[0038] The technical solution of the present invention provides an aging-resistant coating with damage warning and corrosion inhibition functions, which is coated on a metal substrate and includes a coating resin, a corrosion inhibitor composite nanoclay and a plurality of crystal violet lactone microcapsules. The coating resin and the corrosion inhibitor composite nanoclay are mixed, and the plurality of crystal violet lactone microcapsules are dispersed in the mixture of the coating resin and the corrosion inhibitor composite nanoclay; the crystal violet lactone microcapsules include a microcapsule wall and crystal violet lactone encapsulated in the microcapsule wall; when the damage of the coating does not reach the metal substrate, the crystal violet lactone is released from the microcapsule wall to the damaged area of the coating, so that the color of the damaged area is different from that of other areas of the coating; when the damage of the coating reaches the metal substrate, the corrosion inhibitor composite nanoclay releases the corrosion inhibitor at the damaged area.
[0039] Specifically, when the surface of the coating is damaged, the wall of the microcapsule is broken and crystal violet lactone flows out. The crystal violet lactone is released into the damaged area, where it can show local fluorescence enhancement in a dark environment, and can also be combined with the nanoclay of the coating to show blue in a bright environment to adapt to different application scenarios with bright or dark light. The damaged position has an obvious color change, which plays a role in damage warning, and can provide direct and timely warning after the surface is damaged, without the need for stimulation or reaction of other factors, especially the addition of corrosive media. When the coating damage reaches the metal substrate, the corrosion inhibitor composite nanoclay releases the corrosion inhibitor at the damaged area to inhibit the corrosion process of the metal substrate.
[0040] Preferably, the coating resin is one or more of epoxy resin, acrylic resin, alkyd resin, polyurethane resin, polyester resin, polyurea resin, fluorocarbon resin, polyolefin resin, phenolic resin, and silicone resin.
[0041] Preferably, the corrosion inhibitor in the corrosion inhibitor composite nanoclay includes inorganic salts and / or organic small molecules.
[0042] Preferably, the nanoclay in the corrosion inhibitor composite nanoclay includes one or more of halloysite, montmorillonite, diatomaceous earth, kaolin and bentonite.
[0043] Preferably, the microcapsule wall comprises one or more of polyurethane, polyurea, phenolic resin, urea-formaldehyde resin and epoxy resin.
[0044] Preferably, the corrosion inhibitor composite nanoclay accounts for 0.3wt.% to 5wt.% of the coating mass fraction, and the crystal violet lactone microcapsules account for 2.5wt.% to 15wt.% of the coating mass fraction.
[0045] Preferably, the coating has a thickness of 60 μm to 300 μm.
[0046] Preferably, the particle size of the crystal violet lactone microcapsules does not exceed 60 μm.
[0047] The technical solution of the present invention also provides a method for preparing an aging-resistant coating with damage warning and corrosion inhibition functions, comprising:
[0048] S1. Evenly disperse 0.5 g to 5 g of nanoclay and 5 g to 15 g of corrosion inhibitor in a mixed solvent of water and dimethyl sulfoxide in a volume ratio of 1:4, immerse for 24 h to 96 h, and obtain corrosion inhibitor composite nanoclay by centrifugation;
[0049] S2, dissolving 0.5 g to 2 g of crystal violet lactone and 0.5 g to 2 g of resin prepolymer in 5 mL to 25 mL of phenyl acetate or ethyl phenyl acetate as the oil phase, using a polyvinyl alcohol aqueous solution with a mass fraction of 0.5 wt.% to 5 wt.% as the water phase, dispersing the two by ultrasonic to obtain an oil-in-water emulsion, adding a resin curing agent to perform in-situ interfacial polymerization, and obtaining crystal violet lactone microcapsules;
[0050] S3. Evenly mix the corrosion inhibitor composite nanoclay, crystal violet lactone microcapsules and coating resin, evenly apply them on the surface of the metal substrate by spin coating or dip coating, and cure for 6h to 48h to obtain an aging-resistant coating with damage warning and corrosion inhibition functions.
[0051] Preferably, the loading rate of the corrosion inhibitor is 5 wt.% to 30 wt.%.
[0052] Preferably, the coverage rate of crystal violet lactone is 15 wt.% to 40 wt.%.
[0053] Preferably, the nanoclay and the corrosion inhibitor are impregnated at room temperature and pressure or low pressure, specifically 20° C. to 30° C., and the pressure is not higher than one standard atmospheric pressure.
[0054] Preferably, after the coating is applied to the surface of the metal substrate, it is cured at room temperature or under heating conditions, specifically at 20°C to 100°C.
[0055] Preferably, after the metal substrate is coated with the coating, the surface of the metal substrate at the coating location can be completely covered by the crystal violet lactone microcapsules, so that no matter where the coating is damaged, the crystal violet lactone microcapsules can be damaged to provide a color change warning.
[0056] Example 1
[0057] Preparation of acrylic resin coating of corrosion inhibitor composite halloysite and crystal violet lactone microcapsules.
[0058] 0.5 g of halloysite and 5 g of 3-amino-5-mercapto-1,2,4-triazole were uniformly dispersed in a mixed solvent of 10 mL of water and 40 mL of dimethyl sulfoxide, immersed for 24 h at room temperature and low pressure, and centrifuged to obtain a corrosion inhibitor composite halloysite;
[0059] 0.5 g of crystal violet lactone and 0.5 g of polyurethane prepolymer were dissolved in 5 mL of phenyl acetate as the oil phase, and a polyvinyl alcohol aqueous solution with a mass fraction of 0.5 wt.% was used as the water phase, and the two were passed through to obtain crystal violet lactone microcapsules;
[0060] The 2024 aluminum alloy sheet was polished with sandpaper, then ultrasonically cleaned with acetone and alcohol, ultrasonically dispersed to form an oil-in-water emulsion, 0.3 g of polyurethane curing agent was added for in-situ interfacial polymerization, and dried for later use;
[0061] 0.3wt.% of corrosion inhibitor composite halloysite and 2.5wt.% of crystal violet lactone microcapsules were added to acrylic resin, stirred evenly, and then evenly coated on the surface of 2024 aluminum alloy using a spin coater;
[0062] Curing was carried out at room temperature for 24 hours, and the coating thickness after curing was 100 μm.
[0063] Comparative Example 1
[0064] It is a pure acrylic resin coating without added fillers.
[0065] like Figure 1 and 2 As shown, it can be seen that in the acrylic resin coating of the corrosion inhibitor composite halloysite and crystal violet lactone microcapsules prepared in Example 1, the halloysite lumen is filled with corrosion inhibitor. Therefore, if the halloysite is damaged, the corrosion inhibitor will be released to inhibit corrosion of the metal substrate. The crystal violet lactone microcapsules are spherical and have relatively uniform size.
[0066] like Figure 3 to Figure 6 As shown, by comparing Example 1 with Comparative Example 1, it can be seen that, whether under visible light or ultraviolet light, the damaged part of the acrylic resin coating with the addition of corrosion inhibitor composite halloysite and crystal violet lactone microcapsules shows obvious color or fluorescence intensity changes, while the scratched part of the pure acrylic resin coating has no obvious color or fluorescence intensity changes.
[0067] Example 2
[0068] Preparation of silicone resin coating of corrosion inhibitor composite montmorillonite and crystal violet lactone microcapsules.
[0069] 2 g of montmorillonite and 10 g of benzotriazole were uniformly dispersed in a mixed solvent of 20 mL of water and 80 mL of dimethyl sulfoxide, immersed for 48 h at room temperature and low pressure, and the corrosion inhibitor composite montmorillonite was obtained by centrifugation;
[0070] 1.5 g of crystal violet lactone and 1.2 g of polyurea prepolymer were dissolved in 15 mL of phenyl acetate as the oil phase, and a 2.5 wt.% polyvinyl alcohol aqueous solution was used as the water phase. The two were dispersed by ultrasonic to form an oil-in-water emulsion, and 0.9 g of polyurea curing agent was added for in-situ interfacial polymerization to obtain crystal violet lactone microcapsules;
[0071] The Q235 low carbon steel sheet was polished with sandpaper, then ultrasonically cleaned with acetone and alcohol and dried for later use;
[0072] . Take 2.5wt.% of corrosion inhibitor composite halloysite and 10wt.% of crystal violet lactone microcapsules and add them to the silicone resin, stir them evenly and apply them evenly on the surface of Q235 low carbon steel sheet with a rotary coater;
[0073] Curing was carried out at 50°C for 24 hours, and the coating thickness after curing was 60 μm.
[0074] Comparative Example 2
[0075] It is a pure silicone resin coating without adding fillers.
[0076] like Figure 7 As shown, by comparing Example 2 with Comparative Example 2, it can be seen that after immersion for 1 day, the low-frequency impedance modulus of Comparative Example 2 is 3.9×105Ω·cm 2 The low-frequency impedance modulus of Example 2 is 5.2×105Ω·cm 2 , which is higher than the scratch coating of comparative example 1; after immersion for 7 days, the low-frequency impedance modulus of comparative example 2 dropped to 2.4×105Ω·cm 2 , while the low-frequency impedance modulus of Example 2 rises to 2.7×106Ω·cm 2 , showing excellent corrosion inhibition performance.
[0077] Example 3
[0078] Preparation of polyurethane resin coating of corrosion inhibitor composite halloysite and crystal violet lactone microcapsules.
[0079] 5 g of halloysite and 15 g of cerium nitrate were uniformly dispersed in a mixed solvent of 50 mL of water and 200 mL of dimethyl sulfoxide, immersed for 96 h at room temperature and low pressure, and centrifuged to obtain a corrosion inhibitor composite halloysite;
[0080] 2 g of crystal violet lactone and 2 g of epoxy resin monomer were dissolved in 25 mL of phenyl acetate as the oil phase, and a 5 wt.% polyvinyl alcohol aqueous solution was used as the water phase. The two were dispersed by ultrasonic to form an oil-in-water emulsion, and 0.8 g of an amine curing agent was added to perform in-situ interfacial polymerization to obtain crystal violet lactone microcapsules;
[0081] The stainless steel sheet was polished with sandpaper, then ultrasonically cleaned with acetone and alcohol and dried for later use;
[0082] 5 wt.% of corrosion inhibitor composite halloysite and 15 wt.% of crystal violet lactone microcapsules were added to the polyurethane resin, stirred evenly, and then evenly coated on the stainless steel surface with a rotary coater;
[0083] Curing was carried out at room temperature for 24 hours, and the coating thickness after curing was 300 μm.
[0084] Comparative Example 3
[0085] It is a pure polyurethane resin coating without adding fillers.
[0086] Table 1 is a performance comparison of Example 1 and Comparative Example 1 after UV aging test. It can be found that after aging for 288 hours, Example 3 is superior to Comparative Example 3 in color difference value, contact angle, low frequency impedance modulus value, surface roughness and other properties compared with Comparative Example 3, indicating that the addition of nanoclay helps to improve the aging resistance of the coating.
[0087] Table 1
[0088] sample Example 3 Comparative Example 3 Color difference value change 9.7 20.1 Water contact angle (°) 52 34 <![CDATA[Low-frequency impedance modulus (Ωcm 2 )]]> <![CDATA[10 9 ]]> <![CDATA[10 7 ]]> Surface roughness(μm) 0.17 0.43
[0089] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. An anti-aging coating with damage warning and corrosion inhibition functions, applied to a metal substrate, characterized in that: It comprises a coating resin, a corrosion inhibitor composite nanoclay and a plurality of crystal violet lactone microcapsules, wherein the coating resin and the corrosion inhibitor composite nanoclay are mixed, and the plurality of crystal violet lactone microcapsules are dispersed in the mixture of the coating resin and the corrosion inhibitor composite nanoclay; The crystal violet lactone microcapsule comprises a microcapsule wall and crystal violet lactone encapsulated in the microcapsule wall; When the damage of the coating does not reach the metal substrate, the crystal violet lactone is released from the microcapsule wall to the damaged area of the coating, making the color of the damaged area different from that of other areas of the coating; When the damage of the coating reaches the metal substrate, the corrosion inhibitor composite nanoclay releases the corrosion inhibitor at the damaged location.
2. The aging-resistant coating with damage warning and corrosion inhibition functions according to claim 1, characterized in that: The coating resin is one or more of epoxy resin, acrylic resin, alkyd resin, polyurethane resin, polyester resin, polyurea resin, fluorocarbon resin, polyolefin resin, phenolic resin and silicone resin.
3. The aging-resistant coating with damage warning and corrosion inhibition functions according to claim 1, characterized in that: The corrosion inhibitor in the corrosion inhibitor composite nanoclay includes inorganic salts and / or organic small molecules.
4. The aging-resistant coating with damage warning and corrosion inhibition functions according to claim 1, characterized in that: The nanoclay in the corrosion inhibitor composite nanoclay includes one or more of halloysite, montmorillonite, diatomite, kaolin and bentonite.
5. The aging-resistant coating with damage warning and corrosion inhibition functions according to claim 1, characterized in that: The microcapsule wall includes one or more of polyurethane, polyurea, phenolic resin, urea-formaldehyde resin and epoxy resin.
6. The aging-resistant coating with damage warning and corrosion inhibition functions according to claim 1, characterized in that: The corrosion inhibitor composite nano clay accounts for 0.3wt.% to 5wt.% of the coating mass fraction, and the crystal violet lactone microcapsules account for 2.5wt.% to 15wt.% of the coating mass fraction.
7. The aging-resistant coating with damage warning and corrosion inhibition functions according to claim 1, characterized in that: The coating has a thickness of 60 μm to 300 μm.
8. A method for preparing an aging-resistant coating with damage warning and corrosion inhibition functions according to any one of claims 1 to 7, characterized in that: include: S1. Evenly disperse 0.5 g to 5 g of nanoclay and 5 g to 15 g of corrosion inhibitor in a mixed solvent of water and dimethyl sulfoxide in a volume ratio of 1:4, immerse for 24 h to 96 h, and obtain corrosion inhibitor composite nanoclay by centrifugation; S2, dissolving 0.5 g to 2 g of crystal violet lactone and 0.5 g to 2 g of resin prepolymer in 5 mL to 25 mL of phenyl acetate or ethyl phenyl acetate as the oil phase, using a polyvinyl alcohol aqueous solution with a mass fraction of 0.5 wt.% to 5 wt.% as the water phase, dispersing the two by ultrasonic to obtain an oil-in-water emulsion, adding a resin curing agent to perform in-situ interfacial polymerization, and obtaining crystal violet lactone microcapsules; S3. Evenly mix the corrosion inhibitor composite nanoclay, the crystal violet lactone microcapsules and the coating resin, evenly apply them on the surface of the metal substrate by spin coating or dip coating, and cure for 6h to 48h to obtain an aging-resistant coating with damage warning and corrosion inhibition functions.
9. The method for preparing an aging-resistant coating with damage warning and corrosion inhibition functions according to claim 8, characterized in that: The loading rate of the corrosion inhibitor is 5wt.% to 30wt.%.
10. The method for preparing an aging-resistant coating with damage warning and corrosion inhibition functions according to claim 8, characterized in that: The coverage rate of the crystal violet lactone is 15 wt.% to 40 wt.%.
Citation Information
Patent Citations
Application method of low-cost corrosion inhibitor loading structure
CN105802310A
Microcapsule-containing self-detection and self-repair intelligent coating and preparation method thereof
CN112552778A
Microcapsule type two-component waterborne polyurethane self-repairing coating and preparation method thereof
CN113337193A
Grading response self-early warning anticorrosive coating and preparation method thereof
CN115895317A
Reversible self-early-warning and self-repairing coating and preparation method thereof
CN117777820A