Light-cured polyurethane acrylate ink and application thereof
By using light-curing polyurethane acrylate ink of component A and component B on the optical fiber, combined with the reaction of fluorine-containing branched segments and isocyanate, a low refractive index coating is formed, which solves the problem of moisture penetration of the optical fiber in high temperature and high humidity environments. , achieving both high water resistance and mechanical properties.
Patent Information
- Application Number
- CN202410854616.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
Optical fibers are susceptible to moisture penetration in high-temperature and high-humidity environments, resulting in a decrease in optical performance. It is difficult for existing low-refractive index coatings to balance mechanical strength and water resistance.
Photocurable polyurethane acrylate ink is used, which is composed of component A and component B. Component A and component B form a low refractive index cured resin through chelation of inter-segment groups, and are combined with fluorine-containing branched segments. Isocyanate reacts to form H bonds to reduce microphase separation and improve mechanical properties and water resistance.
The formation of a low refractive index coating is achieved, while improving the mechanical properties and water resistance of the optical fiber, significantly improving the overall performance of the polymer, and adapting to use in various environments.
Smart Images

Figure BDA0004917751040000051 
Figure BDA0004917751040000061 
Figure BDA0004917751040000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a light-curing polyurethane acrylate ink and an application thereof. Background Art
[0002] With the rapid development of science and technology, optical fiber has been increasingly used in the fields of communications, electronics, and electricity, becoming a promising new basic material. The accompanying optical fiber technology has also won people's favor with its novelty and convenience. Due to its many characteristics such as anti-electromagnetic interference, high sensitivity, small size, and easy arraying, optical fiber technology has become the key cornerstone of optical fiber communication, optical sensing, optical fiber laser and other technologies.
[0003] In order to ensure that the optical fiber has sufficient mechanical strength and excellent optical properties, and is protected from the external environment during storage and use, and can stably and effectively transmit lasers, a softer low-refractive index inner coating and a harder outer protective coating with toughness, wear resistance, and chemical resistance should be immediately coated when the optical fiber is drawn and formed. Photocurable polyurethane acrylate ink refers to a coating with a refractive index of ≤1.41 after curing. Since the coating itself participates in the transmission of light, the properties of the coating determine the quality level of the optical fiber to a certain extent. In the optical fiber use environment, the optical fiber coating is easily penetrated by moisture because it is exposed to a high temperature and high humidity environment for a long time. The penetrated moisture accumulates at the interface between the optical fiber core made of glass fiber and the optical fiber coating made of resin composition, and plays a role in separating the core and the coating, thereby hindering the optical performance of the optical fiber and becoming an important factor in reducing the long-term reliability of the optical fiber. In view of this, it is urgent to develop a low-refractive index optical fiber coating resin with good properties such as low refractive index, mechanical strength, and water resistance. Summary of the invention
[0004] In order to solve the deficiencies of the prior art, the present invention provides a light-curable polyurethane acrylate ink, a coating and an optical fiber. The light-curable polyurethane acrylate ink can effectively protect the surface of the material, meet the mechanical properties, adhesion and protection of the material, and achieve low refractive index and high water resistance.
[0005] The technical solution provided by the present invention is as follows:
[0006] A light-curable polyurethane acrylate ink, comprising:
[0007] Component A, wherein component A is a fluorinated polyurethane oligomer terminated by a (meth)acrylate functional group, wherein the main chain of component A contains a plurality of -NH-COO-* segments, and * is directly or through a substituted or unsubstituted C 1-30 The alkyl chain is bonded;
[0008] Component B, the component B is a fluorinated polyurethane oligomer terminated by a (meth)acrylate functional group, wherein the main chain of the component B contains a plurality of -OOC-NH-* segments, and * is directly or through a substituted or unsubstituted C 1-30 The alkyl chain is bonded;
[0009] and component C, which is a photocurable polymerization initiator;
[0010] Wherein: the main chain of component A contains one or more fluorinated functional group side chains; and / or the main chain of component B contains one or more fluorinated functional group side chains.
[0011] Specifically, the fluorinated functional group side chain is selected from any C atom in which 1 to 3 H atoms are replaced by fluorine atoms. 1-10 Alkyl, 1-3 H atoms on any C atom are replaced by fluorine atoms 1-10 Alkoxy, 1-3 H atoms on any C atom are replaced by fluorine atoms 1-10 One or more of the alkyl ester groups, the C 1-10 Alkyl, C 1-10 Alkoxy, C 1-10 The alkyl ester group contains one or more R1 substituents, wherein R1 is independently selected from H, hydroxyl, cyano or amino.
[0012] Preferably, the C 1-10 The alkyl group is selected from unsubstituted perfluoroalkyl groups. 1-10 The alkyl group is selected from unsubstituted perfluoro linear alkyl groups, for example, perfluoromethyl, perfluoroethyl, perfluoropropyl, and perfluorobutyl.
[0013] Specifically, the main chain of component A contains polyester and / or polyether repeating segments. The fluorinated functional group side chains are bonded to the polyester and / or polyether segments to form a main chain with a branched structure.
[0014] Each polyether segment or polyester segment can have any suitable molecular weight. For example, each polyester segment can independently have an Mn of less than 20,000, such as an Mn of 1,500.
[0015] Specifically, the main chain of component B contains polyester and / or polyether repeating segments, respectively. The fluorinated functional group side chains are bonded to the polyester and / or polyether segments to form a main chain with a branched structure.
[0016] Each polyether segment or polyester segment can have any suitable molecular weight. For example, each polyester segment can independently have an Mn greater than 1000, such as an Mn of 1500.
[0017] Preferably, the C 1-15The alkyl chain is selected from unsubstituted C 1-10 More preferably, representative alkyl groups include, but are not limited to, methyl, ethyl, propyl, butyl, and pentyl.
[0018] Specifically, the component A is prepared by reacting diol a, diisocyanate and hydroxyl-containing (meth)acrylate, wherein the diol a is a fluorinated polyester diol or a fluorinated polyether diol. The diol a contains a fluorinated functional group side chain. In this embodiment, component A also contains a carbamate function that is not connected to the acrylate function and is formed by reacting an alcohol hydroxyl group with isocyanic acid.
[0019] Specifically, the component B is prepared by reacting a diol b with a (meth)acrylate containing an isocyanate group, wherein the second diol is a fluorinated polyester diol or a fluorinated polyether diol. The diol b contains a fluorinated functional group side chain.
[0020] Specifically, the weight ratio of the oligomer A to the oligomer B is (1-5):(2-7).
[0021] Preferably, the weight ratio of the oligomer A to the oligomer B is (2-4):(4-7).
[0022] Furthermore, the photocurable polyurethane acrylate ink further comprises a component D, wherein the component D is a fluorinated (meth) acrylate, wherein the fluorinated (meth) acrylate comprises a C substituted by one or more R2 1-30 wherein the alkyl group is an alkyl group, and the R2 is independently selected from H, hydroxyl, ether, nitro, amino or cyano.
[0023] Preferably, the fluorinated (meth)acrylate is selected from perfluoroalkyl acrylates containing at least one R2 selected from hydroxyl groups.
[0024] The polymerization initiator is selected from any one of α-hydroxy ketone initiators, benzoin initiators, acylphosphine oxide initiators, acetophenone initiators, morpholinyl ketone initiators, naphthylimide photoinitiators or oxime ester photoinitiators, or a combination of at least two thereof.
[0025] In addition, in addition to the above components, conventional additives such as leveling agents, slip agents, stabilizers or antioxidants may also be included according to the present invention to improve thermal and oxidative stability, storage stability, surface properties, flow properties and process properties. In this case, the weight of the additive added to the resin composition is in the range of 0.1 to 10 weight ratios of the total weight of the resin composition.
[0026] The invention also provides a coating material, comprising the above-mentioned light-curing polyurethane acrylate ink.
[0027] The coating material can be used to coat the surface of an optical fiber to form a low refractive index coating.
[0028] Compared with the prior art, the present application provides a photocurable polyurethane acrylate ink, which comprises a component A having an -NH-COO-* segment and a component B having an -OOC-NH- segment. Through the chelation of the inter-segment groups, the cured resin has a lower refractive index while maintaining good mechanical properties, thereby meeting the requirements for the inner layer coating of the optical fiber. At the same time, a fluorinated polyether (ester) polyol having a fluorinated branch segment is reacted with an isocyanate, a hydroxy acrylate, or an isocyanate acrylate to synthesize an oligomer. An H bond is easily formed between the fluorinated branch segment in the main chain and the -NH in the urethane bond, thereby reducing the degree of microphase separation of the polyurethane segment. While the fluorine element migrates to the surface, it also drives part of the branch chain to migrate to the surface, thereby achieving low-fluorine and high-performance fluorinated oligomers. As a result, the composition can meet the low refractive index requirements while still having excellent comprehensive properties at a lower fluorine content, thereby significantly improving the mechanical properties, water resistance, and weather resistance of the polymer. DETAILED DESCRIPTION
[0029] The principles and features of the present invention are described below. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.
[0030] The fluorinated polyether diol and fluorinated polyester diol used in this embodiment have a molecular weight of 4000 Mn and are commercially available. The structures are shown in Table 1 below, where m, n, p, and q all represent the degree of polymerization:
[0031] Table 1
[0032]
[0033] Comparative Example 1:
[0034] S1: Synthesis of oligomer A-1: Add 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol to 1 mol of fluorinated diol X1, and then add 2.5 mol of isophorone diisocyanate at room temperature to control the reaction temperature below 30°C. After the addition is completed, the reaction temperature is raised to 65°C and the reaction is continued for two hours. Second step reaction: Add 2.5 mol of hydroxyethyl acrylate to the reaction bottle and control the temperature at 65°C. After the addition is completed, the reaction is continued for 1 hour.
[0035] S2: Synthesis of oligomer B-1: Add 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol to 1 mol of fluorinated diol X2, and then drop 2.5 mol of isocyanate ethyl methacrylate at room temperature. After the addition is completed, heat the mixture to 50°C and react for 1.5 hours.
[0036] S3: oligomer A, oligomer B and perfluorohexylethyl methacrylate are mixed and stirred in a weight ratio of 2.5:5:0.15, and then 0.5 weight parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate are added to obtain a final formula.
[0037] Embodiment 1-8:
[0038] The preparation method is the same as that of Example 1, except that oligomer A and oligomer B are prepared by reacting the compounds shown in Table 2 and Table 3, respectively, and the contents of oligomer A and oligomer B and fluorinated monomer C are selected as shown in Table 4 below:
[0039] Table 2
[0040] Fluorinated diols Diisocyanates Hydroxyacrylate A-2 X3 Isophorone diisocyanate Hydroxyethyl acrylate A-3 X4 Cyclohexane diisocyanate Hydroxyethyl acrylate A-4 X4 Methylene diphenyl diisocyanate Hydroxyethyl acrylate A-5 X5 Hexamethylene diisocyanate Hydroxypropyl acrylate
[0041] Table 3
[0042] Fluorinated diols Isocyanate acrylate B-2 X4 Ethyl Methacrylate Isocyanate B-3 X5 Ethyl Methacrylate Isocyanate
[0043] Table 4
[0044]
[0045] Among them, component C is ethyl 2,4,6-trimethylbenzoylphenylphosphonate; D-1 is perfluorooctylpropyl acrylate, and D-2 is 3-perfluorooctyl-2-hydroxypropyl methacrylate.
[0046] Comparative Example 2:
[0047] S1: Synthesis of oligomer A-6: Add 0.1 mol catalyst dibutyltin dilaurate and 0.1 mol antioxidant 2,6-di-tert-butyl-p-cresol to 1 mol isophorone diisocyanate, and then add 2.5 mol fluorinated diol X3 at room temperature to control the reaction temperature below 30°C. After the addition is complete, the reaction temperature rises to 65°C and the reaction is continued for two hours. Second step reaction: Add 2.5 mol isocyanate ethyl methacrylate to the reaction bottle, and control the temperature at 65°C. After the addition is complete, the reaction is continued for 1 hour.
[0048] S2: Synthesis of oligomer B-4: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated diol X5, and 3 mol of isocyanate ethyl methacrylate was added dropwise at room temperature. After the addition was completed, the temperature was raised to 50°C and the reaction was allowed to proceed for 1.5 hours.
[0049] S3: 30 parts of oligomer A, 50 parts of oligomer B and 1 part of perfluorohexylethyl methacrylate were mixed and stirred, and then 10 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain a final formula.
[0050] Performance testing:
[0051] The coating was evenly coated on the quartz glass and cured by ultraviolet light for 20 seconds. The refractive index of the film was tested by Abbe refractometer. The elongation at break and peel strength were tested by universal testing machine. The water resistance was tested according to YD / T 4079-2022. The test results are shown in Table 5 below:
[0052] Table 5
[0053]
[0054] As can be seen from the above table, compared with fluorine-containing straight chains, fluorine-containing segments distributed in the side chains are easier to migrate and enrich to the surface, and a lower fluorine content can effectively protect the polyurethane surface, and have different mechanical properties, adhesion and protection properties that adapt to various environments, while achieving low refractive index and high water resistance. The optical fiber prepared by the technical solution of the optical fiber coating composition has a red spot rate of less than 10% when conducting a light transmission test.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A light-curable polyurethane acrylate ink, characterized in that: include: Component A, wherein component A is a fluorinated polyurethane oligomer terminated by a (meth)acrylate functional group, wherein the main chain of component A contains a plurality of -NH-COO-* segments, and * is directly or through a substituted or unsubstituted C 1-30 The alkyl chain is bonded; Component B, the component B is a fluorinated polyurethane oligomer terminated by a (meth)acrylate functional group, wherein the main chain of the component B contains a plurality of -OOC-NH-* segments, and * is directly or through a substituted or unsubstituted C 1-15 The alkyl chain is bonded; and component C, which is a photocurable polymerization initiator; Wherein: the main chain of component A contains one or more fluorinated functional group side chains; and / or the main chain of component B contains one or more fluorinated functional group side chains.
2. The light-curable polyurethane acrylate ink according to claim 1, characterized in that: The fluorinated functional group side chain is selected from any C atom in which 1 to 3 H atoms are replaced by fluorine atoms. 1-10 Alkyl, 1-3 H atoms on any C atom are replaced by fluorine atoms 1-10 Alkoxy, C in which 1 to 3 H atoms on any C atom are replaced by fluorine atoms 1-10 One or more of the alkyl ester groups, the C 1-10 Alkyl, C 1-10 Alkoxy, C 1-10 The alkyl ester group contains one or more R1 substituents, wherein R1 is independently selected from H, hydroxyl, cyano or amino.
3. The light-curable polyurethane acrylate ink according to claim 2, characterized in that: The C 1-10 The alkyl group is selected from unsubstituted perfluoroalkyl groups.
4. The light-curable polyurethane acrylate ink according to claim 3, characterized in that: The main chain of component A contains polyester and / or polyether segments; and / or the main chain of component B contains polyester and / or polyether segments, and the fluorinated functional group side chains are bonded to the polyester and / or polyether segments to form a main chain with a branched structure.
5. The photocurable polyurethane acrylate ink according to claim 1, characterized in that: The C 1-15 The alkyl chain is selected from unsubstituted C 1-10 of a straight chain alkyl group.
6. The light-curable polyurethane acrylate ink according to claim 1, characterized in that: The component A is prepared by reacting a diol a with a diisocyanate and then with a hydroxyl-containing (meth)acrylate, wherein the diol a is a fluorine-containing polyester diol or a fluorine-containing polyether diol; The component B is prepared by reacting a diol b with a (meth)acrylate containing an isocyanate group, wherein the second diol is a fluorine-containing polyester diol or a fluorine-containing polyether diol; Wherein: the diol a contains a fluorinated functional group side chain; and / or the diol b contains a fluorinated functional group side chain.
7. The light-curable polyurethane acrylate ink according to any one of claims 1 to 6, characterized in that: The weight ratio of the oligomer A to the oligomer B is (1-5):(2-7).
8. The light-curable polyurethane acrylate ink according to claim 7, characterized in that: The component D is a fluorinated (meth)acrylate, wherein the fluorinated (meth)acrylate comprises C substituted by one or more R2 1-30 wherein the alkyl group is an alkyl group, and the R2 is independently selected from H, hydroxyl, ether, nitro, amino or cyano.
9. The light-curable polyurethane acrylate ink according to claim 7, characterized in that: The polymerization initiator is selected from any one of α-hydroxy ketone initiators, benzoin initiators, acylphosphine oxide initiators, acetophenone initiators, morpholinyl ketone initiators, naphthylimide photoinitiators or oxime ester photoinitiators, or a combination of at least two thereof.
10. A coating material comprising the photocurable polyurethane acrylate ink according to any one of claims 1 to 9.