Low-refractive-index resin composition, application thereof and optical fiber coating

By using a two-component resin composition of oligomer A and oligomer B, combined with monomer C, a low refractive index, high mechanical strength optical fiber inner layer coating is formed, which solves the problem of optical fiber coating between mechanical properties and light energy transmission efficiency. Taking into account the problem of space, it achieves the effects of high numerical aperture, low loss and high mechanical strength.

CN118852971APending Publication Date: 2024-10-29WUHAN SUNSHINE OPTOELECTRONICS TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410854614.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing optical fiber coatings are easy to break, scratch, absorb moisture and oxidize during the high-temperature melting process, which affects the quality of optical signal transmission. Low-refractive index optical fiber coatings are difficult to balance between mechanical properties and light energy transmission efficiency.

Method used

A two-component resin composition of oligomer A and oligomer B is used to adjust the refractive index, elongation at break and tensile strength through the formation of hydrogen bonds, and the viscosity of the composition is adjusted through monomer C to form a low refractive index, High mechanical strength optical fiber inner coating.

Benefits of technology

It achieves low refractive index, high elongation at break and good tensile strength, meets the requirements of high numerical aperture, low loss and high mechanical strength of optical fiber, forms a uniform, soft and well-wrapped coating, and improves the resistance of optical fiber. Micro-bending performance and light energy transmission efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917750530000031
    Figure BDA0004917750530000031
  • Figure BDA0004917750530000032
    Figure BDA0004917750530000032
  • Figure BDA0004917750530000041
    Figure BDA0004917750530000041
Patent Text Reader

Abstract

The invention belongs to the technical field of resin materials, and particularly relates to a low-refractive-index resin composition, application thereof and an optical fiber coating. The low-refractive-index resin composition comprises an oligomer A, an oligomer B, a polymerization initiator and an auxiliary agent, the oligomer A is a fluorinated polyurethane acrylate oligomer of which the middle chain segment is a straight chain, and the end groups on the two sides of the oligomer A respectively have one or more CH2 = C (R1) COOL1OOCCH-terminated groups; the oligomer B is a fluorinated polyurethane acrylate oligomer of which the middle chain segment is a straight chain, and the end groups on the two sides of the oligomer B are respectively provided with one or more CH2 = C (R1) COOL2NHCOO-end-capping groups. The coating obtained by curing the low-refractive-index resin composition provided by the invention has low refractive index, high elongation at break and good tensile strength, and meets the requirements of high numerical aperture, low loss and high mechanical strength of optical fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resin materials, and in particular relates to a low-refractive-index resin composition and an application thereof and an optical fiber coating. Background Art

[0002] The optical fiber for communication is made of prefabricated quartz rods that are melted and drawn at a high temperature of more than 2000℃ in a high-temperature graphite furnace. The bare fiber is thin, brittle and easy to break. Under the influence of the external environment, it is easy to be scratched, dust adhered, absorbed moisture, and oxidized, which directly affects the transmission quality of the optical signal. Therefore, the bare fiber must be coated and protected. Optical fiber coating is an indispensable key protective material in the production and application of optical fiber. It provides strength protection, waterproofing and stress buffering for optical fiber, thereby maintaining the excellent mechanical and optical properties of optical fiber. At present, optical fiber production adopts a double-layer coating process for optical fiber coating. The double-layer coating includes an inner layer coating and an outer layer coating. The inner layer coating has a low glass transition temperature (Tg) and strong flexibility. It uses the principle of total reflection of light to complete the transmission of light energy together with the quartz fiber core and transmit optical signals.

[0003] Low refractive index optical fiber coating is a special coating for the inner layer of optical fiber. The cured film has a low refractive index, which can increase the numerical aperture of the optical fiber. Under the premise of ensuring good mechanical properties, it can effectively improve the long-distance transmission efficiency of light energy and reduce light loss. Generally speaking, the refractive index of the inner layer of optical fiber coating after curing is required to be ≤1.380. Due to the excellent properties of "three highs" and "two hates" of fluorinated polymers, fluorinated coatings with fluorinated polymers as the main raw materials have high practical value in the inner layer coating. Summary of the invention

[0004] In order to solve the deficiencies of the prior art, the present invention provides a low refractive index resin composition and its application and optical fiber coating. The coating obtained by curing the low refractive index resin composition provided by the present invention has a low refractive index, a high elongation at break and good tensile strength, and meets the requirements of high numerical aperture, low loss and high mechanical strength of optical fiber.

[0005] The technical solution provided by the present invention is as follows:

[0006] A low-refractive index resin composition comprises the following components: oligomer A, oligomer B, a polymerization initiator and an auxiliary agent;

[0007] The oligomer A is a fluorinated polyurethane acrylate oligomer with a straight chain in the middle segment, and the end groups on both sides thereof respectively have one or more CH2=C(R1)COOL1OOCNH-capping groups;

[0008] The oligomer B is a fluorinated polyurethane acrylate oligomer with a straight chain in the middle segment, and the end groups on both sides thereof respectively have one or more CH2=C(R1)COOL2NHCOO-capping groups;

[0009] L1 and L2 are different or the same and are selected from C 1-20 Alkyl, C 3-30 Cycloalkyl, C 6-30 Any of the aromatic groups.

[0010] The polymerization initiator is a photopolymerization initiator.

[0011] In the above technical solution:

[0012] By using the two components of oligomer A and oligomer B, the refractive index, elongation at break and tensile strength can be effectively adjusted based on the formed hydrogen bonds.

[0013] Specifically, the preparation method of the oligomer A comprises the following steps:

[0014] 1) reacting a fluorinated polyol with a diisocyanate to obtain a fluorinated polyurethane isocyanate having isocyanate-terminated terminal groups on both sides;

[0015] 2) reacting the fluorinated polyurethane isocyanate with a hydroxyl-containing (meth)acrylate to obtain the oligomer A.

[0016] Specifically, the preparation method of the oligomer B comprises the following steps: reacting a fluorine-containing polyol with isocyanate (meth)acrylate to obtain oligomer B.

[0017] Specific:

[0018] The hydroxyl-containing (meth)acrylate is a monohydroxyl (meth)acrylate;

[0019] The oligomer A has a structural formula shown in Formula 1:

[0020]

[0021] wherein n is an integer of 1-3, R1 is a linear fluorinated polyether unit or a branched fluorinated polyester unit, and R2 and R3 are independently selected from C 1-20 Alkyl, C 3-30 Cycloalkyl, C 6-30 Any of aryl, wherein the alkyl, cycloalkyl or aryl groups may be substituted by one or more R' groups in each case, R' being identical or different in each case and being respectively hydroxyl, a straight-chain alkyl group having 1 to 6 carbon atoms or a cycloalkyl group having 3 to 12 carbon atoms, and R4 being H or methyl.

[0022] Further, the C3-30 cycloalkyl group includes unsubstituted or C 1-5 Alkyl, C 1-5 Alkoxy, hydroxyl, cyano, nitro substituted monocyclic alkyl, two monocyclic alkyl groups are connected by a single bond or C 1-5 The alkyl groups of the monocyclic alkyl group and the polycyclic alkyl group are bridged to form a polycyclic alkyl group, wherein 1 to 3 hydrogen atoms in the monocyclic alkyl group and the polycyclic alkyl group can be further replaced by C 1-5 The C6-30 aryl group includes phenyl, naphthalene, biphenyl, and polycyclic aromatic groups containing 2-3 benzene rings, wherein the benzene rings are fused, bonded or C 1-5 The alkyl bridge of phenyl and polycyclic aromatic groups can be further bridged by C 1-5 of alkyl substitution.

[0023] Specifically, the isocyanate (meth)acrylate is monoisocyanate (meth)acrylate;

[0024] The oligomer B has the structural formula shown in Formula 2:

[0025]

[0026] wherein m is an integer of 1 to 3, R5 is a linear fluorinated polyether unit or a branched fluorinated polyester unit, and R6 is selected from C 1-20 Alkyl, C 3-30 Cycloalkyl, C 6-30 Any of aryl, wherein the alkyl, cycloalkyl or aryl groups may be substituted by one or more R' groups in each case, R' being the same or different in each case and being respectively hydroxyl, a straight-chain alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, and R7 being H or methyl.

[0027] Furthermore, the C 3-30 The cycloalkyl group includes unsubstituted or C 1-5 Alkyl, C 1-5 Alkoxy, hydroxyl, cyano, nitro substituted monocyclic alkyl, two monocyclic alkyl groups are connected by a single bond or C 1-5 The alkyl groups of the monocyclic alkyl group and the polycyclic alkyl group are bridged to form a polycyclic alkyl group, wherein 1 to 3 hydrogen atoms in the monocyclic alkyl group and the polycyclic alkyl group can be further replaced by C 1-5 Alkyl substituted; said C 6-30 Aryl includes phenyl, polycyclic aromatic groups containing 2-3 benzene rings, the benzene rings are fused, bonded or C 1-5 The alkyl bridge of phenyl and polycyclic aromatic groups can be further bridged by C 1-5 of alkyl substitution.

[0028] Specifically, the structural formula of the fluorinated polyether unit is CH2CF2O(CF2CF2O)y (CF2O) z CF2CH2, (CH2CH2O) x CH2CF2O(CF2CF2O) y (CF2O) Z CF2CH2(OCH2CH2) x , wherein x, y and z are the degree of polymerization, preferably a natural number of 1-20.

[0029] Preferably, the number average molecular weight of the fluorine-containing polyol is between 1500 and 5000.

[0030] Preferably, the fluorinated polyol is preferably a fluorinated polyether diol or a fluorinated polyester diol; the isocyanate is preferably a difunctional isocyanate; the isocyanate (meth)acrylate is preferably a monofunctional isocyanate (meth)acrylate. The number average molecular weight of the fluorinated polyol is between 1500-4500.

[0031] Furthermore, the low refractive index resin composition further comprises a monomer C, wherein the monomer C is selected from a fluorine-containing acrylate having Formula 3:

[0032]

[0033] R8 is a C1-10 perfluoroalkyl group, R9 is a single bond, a hydroxyl substituted or unsubstituted C 1-5 The alkylene group, R 10 It is H or methyl.

[0034] Based on the above technical solution, the addition of monomer C can be used to adjust the viscosity of the composition.

[0035] Specifically, in the present invention, monomer C can be selected from perfluoroalkylethyl (meth) acrylate, perfluorobutylethyl (meth) acrylate, perfluorohexylethyl (meth) acrylate, perfluorohexylpropyl (meth) acrylate, perfluorooctylhexyl (meth) acrylate, perfluorooctylpropyl (meth) acrylate, perfluorodecyl methacrylate, perfluorodecyl ethyl acrylate, perfluorododecylethyl (meth) acrylate, tridecafluorooctyl acrylate, 3-perfluorobutyl-2-hydroxypropyl (meth) acrylate, 3-perfluorohexyl-2-hydroxypropyl (meth) acrylate, 3-(perfluoro-3-methylbutyl) 2-hydroxypropyl methacrylate, 3-(perfluoro-7-methyloctyl)-2-hydroxypropyl methacrylate, etc.

[0036] The polymerization initiator is selected from any one of ketone photoinitiators, benzoin photoinitiators, acylphosphine oxide photoinitiators, and oxime ester photoinitiators, or a combination of at least two thereof.

[0037] Specifically, in the present application, the photoinitiator is preferably 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-2-methyl-1-[4-(tert-butyl)phenyl]-1-propanone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, OXE-01, OXE-02, etc.

[0038] The auxiliary agent includes any one or more of a catalyst, an antioxidant, a dispersant, a solvent, a surfactant, a leveling agent, and a defoaming agent.

[0039] Specifically, the mass ratio of the oligomer A, oligomer B, monomer C and polymerization initiator is (2-4):(4-6):(1-2):(0.1-0.3).

[0040] The oligomer A is prepared according to the following steps: adding an auxiliary agent to the fluorinated diol, dripping isocyanate at room temperature, controlling the reaction temperature below 30°C, and after the dripping is completed, the reaction temperature rises to 60-70°C and reacts for 1-3h, then dripping hydroxy acrylate into the reaction bottle, controlling the temperature at 60-70°C, and after the dripping is completed, reacting for 0.5-3h.

[0041] The oligomer B is prepared according to the following steps: adding an auxiliary agent to the fluorinated diol, adding isocyanate dropwise at room temperature, controlling the reaction temperature at 40-70° C., and reacting for 1-3 hours.

[0042] In a second aspect, the present invention also provides the use of the low-refractive index resin composition as a coating for optical fiber.

[0043] In a third aspect, the present invention also provides an optical fiber coating, which is obtained by coating and photocuring the above-mentioned low-refractive index resin composition.

[0044] Beneficial effects of the present invention:

[0045] The present invention provides a resin composition that can be used for nanoimprinting. By adjusting the ratio of two components, an oligomer A with long-chain molecules and an oligomer B with short-chain molecules, more hydrogen bonds are formed between the two components A and B, and the refractive index and mechanical properties of the coating can be controlled within a certain range.

[0046] The present invention further adjusts the viscosity of the composition through monomer C, which is beneficial to the coating of the optical fiber coating and forms a uniform, soft, and well-wrapped coating;

[0047] The invention has simple components and the prepared coating has lower refractive index and higher strength. DETAILED DESCRIPTION

[0048] The principles and features of the present invention are described below. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0049] In the present invention, a fluorinated polyester diol with a molecular weight of 1500 and a structural formula of Obtained from commercial sources; fluorinated polyether diol with a molecular weight of 4000, purchased from Solvay Company's E10-H.

[0050] Embodiment 1:

[0051] Preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyester diol, and 3 mol of isophorone diisocyanate was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was carried out for two hours. Second step reaction: 3 mol of hydroxyethyl acrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and after the addition was completed, the reaction was carried out for 1 hour. The number average molecular weight of the product was 4704Mn as measured by GPC.

[0052] Preparation of oligomer B: Add catalyst dibutyltin dilaurate and 0.1 mol antioxidant 2,6-di-tert-butyl-p-cresol to 1 mol of fluorinated polyester diol, and add 3 mol of isocyanate ethyl methacrylate dropwise at room temperature. After the addition is completed, heat to 50°C and react for 1.5 hours. The molecular weight of the product measured by GPC is 4310Mn;

[0053] Preparation of the composition: 3 parts of oligomer A, 5 parts of oligomer B and 2 parts of perfluorohexylethyl methacrylate were mixed and stirred, and then 0.15 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain a final formula.

[0054] Embodiment 2:

[0055] The optical fiber coating composition was prepared in the same manner as in Example 1, except that: Composition preparation: 3 parts of oligomer A and 5 parts of oligomer B were mixed and stirred, and then 0.15 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain the final formula.

[0056] Embodiment 3:

[0057] The optical fiber coating composition was prepared in the same manner as in Example 1, except that: Composition preparation: 3 parts of oligomer A, 5 parts of oligomer B and 2 parts of perfluorohexylethyl methacrylate were mixed and stirred, and then 0.15 parts of diphenylphosphine oxide were added to obtain the final formula.

[0058] Embodiment 4:

[0059] An optical fiber coating composition was prepared in the same manner as in Example 1, except that: preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyether diol, and 3 mol of cyclohexane diisocyanate was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was carried out for two hours; second step reaction: 3 mol of hydroxyethyl acrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and the reaction was carried out for 1 hour.

[0060] Embodiment 5:

[0061] The optical fiber coating composition was prepared in the same manner as in Example 4. The composition was prepared by mixing 3 parts of oligomer A, 5 parts of oligomer B and 2 parts of 3-perfluorohexyl-2-hydroxypropyl isobutylene, and then adding 0.15 parts of diphenylphosphine oxide to obtain the final formula.

[0062] Embodiment 6:

[0063] Preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyether diol, and 3 mol of 4,4-diisocyanate dicyclohexylmethane was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was carried out for two hours. Second step reaction: 3 mol of hydroxyethyl acrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and the reaction was carried out for 1 hour after the addition was completed.

[0064] Preparation of oligomer B: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyester diol, and 3 mol of isocyanate ethyl methacrylate was added dropwise at room temperature. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out for 1.5 hours.

[0065] Preparation of the composition: 2 parts of oligomer A, 5 parts of oligomer B and 1 part of perfluoroalkylethyl methacrylate were mixed and stirred, and then 0.1 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain a final formula.

[0066] Embodiment 7:

[0067] An optical fiber coating composition was prepared in the same manner as in Example 6, except that: Preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyether diol, and 3 mol of 1,8-diisocyanooctane was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was carried out for two hours; Second step reaction: 3 mol of hydroxyethyl acrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and the reaction was carried out for 1 hour.

[0068] Embodiment 8:

[0069] Preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyether diol, and 3 mol of trimethylhexamethylene diisocyanate was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was continued for two hours. Second step reaction: 3 mol of hydroxyethyl acrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and the reaction was continued for 1 hour after the addition was completed.

[0070] Preparation of oligomer B: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyester diol, and 3 mol of isocyanate ethyl methacrylate was added dropwise at room temperature. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out for 1.5 hours.

[0071] Preparation of the composition: 1 part of oligomer A, 6 parts of oligomer B and 2 parts of perfluorohexylethyl methacrylate were mixed and stirred, and then 0.3 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain a final formula.

[0072] Embodiment 9:

[0073] An optical fiber coating composition was prepared in the same manner as in Example 8, except that: Preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyether diol, and 3 mol of p-xylene diisocyanate was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was carried out for two hours; Second step reaction: 3 mol of hydroxyethyl acrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and the reaction was carried out for 1 hour.

[0074] Embodiment 10:

[0075] An optical fiber coating composition was prepared in the same manner as in Example 9, except that 1 part of oligomer A, 6 parts of oligomer B and 2 parts of 3-perfluorohexyl-2-hydroxypropyl isobutylene were mixed and stirred, and then 0.3 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate was added to obtain the final formula.

[0076] Embodiment 11:

[0077] Preparation of oligomer A: add 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol to 1 mol of fluorinated polyester diol, and then add 3 mol of 3,3′-dimethoxy-4,4′-biphenyl diisocyanate at room temperature to control the reaction temperature below 30°C. After the addition is completed, the reaction temperature is raised to 65°C and the reaction is continued for two hours. Second step reaction: add 3 mol of hydroxyethyl acrylate to the reaction bottle, and the temperature is controlled at 65°C. After the addition is completed, the reaction is continued for 1 hour.

[0078] Preparation of oligomer B: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyether diol, and 3 mol of isocyanate ethyl methacrylate was added dropwise at room temperature. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out for 1.5 hours.

[0079] Preparation of the composition: 2 parts of oligomer A, 5 parts of oligomer B and 1 part of perfluorododecyl ethyl acrylate were mixed and stirred, and then 0.1 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain a final formula.

[0080] Embodiment 12:

[0081] An optical fiber coating composition was prepared in the same manner as in Example 1, except that: Preparation of oligomer B: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of fluorinated polyester diol, and 3 mol of 2-[2-(methacryloyloxy)ethoxy]ethyl isocyanate was added dropwise at room temperature. After the addition was completed, the temperature was raised to 50°C and the reaction was allowed to react for 1.5 hours.

[0082] Comparative Example 1:

[0083] An optical fiber coating composition was prepared in the same manner as in Example 1, except that: preparation of oligomer A: 0.1 mol of catalyst dibutyltin dilaurate and 0.1 mol of antioxidant 2,6-di-tert-butyl-p-cresol were added to 1 mol of isophorone diisocyanate, and 3 mol of fluorinated polyester diol was added dropwise at room temperature to control the reaction temperature below 30°C. After the addition was completed, the reaction temperature was raised to 65°C and the reaction was carried out for two hours; second step reaction: 3 mol of isocyanate ethyl methacrylate was added dropwise to the reaction bottle, the temperature was controlled at 65°C, and the reaction was carried out for 1 hour.

[0084] Comparative Example 2:

[0085] The optical fiber coating composition was prepared in the same manner as in Example 1, except that: Composition preparation: 8 parts of oligomer A and 2 parts of perfluorohexylethyl methacrylate were mixed and stirred, and then 0.15 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain the final formula.

[0086] Comparative Example 3:

[0087] The optical fiber coating composition was prepared in the same manner as in Example 1, except that: Composition preparation: 8 parts of oligomer B and 2 parts of perfluorohexylethyl methacrylate were mixed and stirred, and then 0.15 parts of ethyl 2,4,6-trimethylbenzoylphenylphosphonate were added to obtain the final formula.

[0088] Performance testing:

[0089] The viscosity was tested with a viscometer; the coating was evenly coated on quartz glass and cured by ultraviolet light for 20 minutes. The refractive index of the film was tested with an Abbe refractometer; the elongation at break and tensile strength were measured with an electronic universal testing machine; the elastic modulus was tested with a static method. The test results are shown in Table 1 below:

[0090] Table 1

[0091]

[0092]

[0093] It can be seen from the above table that it can be seen from Comparative Examples 2, 3 and Comparative Example 1 that the photocurable resin obtained by oligomer A or oligomer B alone cannot meet the requirements of the inner coating of the optical fiber. The difference between the isocyanate group and the carbamate bond in the oligomer A and oligomer B provided in the present application affects each other during the polymerization process, increases the hydrogen bonding effect, and ultimately makes the composition have a significant improvement in mechanical properties such as elongation at break and good tensile strength.

[0094] The low-refractive-index inner coating for optical fiber provided by the present invention has a refractive index lower than 1.36 to meet the transmission loss requirements of optical fiber energy, has a good viscosity range, is easy to coat and wrap the optical fiber, and is conducive to forming a uniform resin protective layer on the surface of the optical fiber; and the coating has the characteristics of good mechanical properties, has a high elongation at break, good tensile strength, and at the same time has a high elastic modulus, high strength and good flexibility, so that the optical fiber is not easy to break when bent, improves the anti-micro-bending performance of the optical fiber, and meets the requirements of high numerical aperture, low loss, and high mechanical strength of the optical fiber.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A low refractive index resin composition, comprising the following components: oligomer A, oligomer B, a polymerization initiator and an auxiliary agent, characterized in that: The oligomer A is a fluorinated polyurethane acrylate oligomer with a straight chain in the middle segment, and the end groups on both sides thereof respectively have one or more CH2=C(R1)COOL1OOCNH-capping groups; The oligomer B is a fluorinated polyurethane acrylate oligomer with a straight chain in the middle segment, and the end groups on both sides thereof respectively have one or more CH2=C(R1)COOL2NHCOO-capping groups; L1 and L2 are different or the same and are selected from C 1-20 Alkyl, C 3-30 Cycloalkyl, C 6-30 Any of the aromatic groups.

2. The low refractive index resin composition according to claim 1, characterized in that: The preparation method of the oligomer A comprises the following steps: 1) reacting a fluorinated polyol with a diisocyanate to obtain a fluorinated polyurethane isocyanate having isocyanate-terminated terminal groups on both sides; 2) reacting the fluorinated polyurethane isocyanate with a hydroxyl-containing (meth)acrylate to obtain the oligomer A; The preparation method of the oligomer B comprises the following steps: reacting a fluorine-containing polyol with isocyanate (meth)acrylate to obtain the oligomer B.

3. The low refractive index resin composition according to claim 2, characterized in that: The hydroxyl-containing (meth)acrylate is a monohydroxyl (meth)acrylate; the oligomer A has a structural formula shown in Formula 1: wherein n is an integer of 1-3, R1 is a linear fluorinated polyether unit or a linear fluorinated polyester unit, and R2 and R3 are independently selected from C 1-20 Alkyl, C 3-30 Cycloalkyl, C 6-30 any of aryl, wherein the alkyl, cycloalkyl or aryl groups may be substituted in each case by one or more R' groups, R' being the same or different in each case and being respectively hydroxyl, a straight-chain alkyl group having 1 to 6 carbon atoms or a cycloalkyl group having 3 to 12 carbon atoms, and R4 being H or methyl; And / or the isocyanate (meth)acrylate is monoisocyanate (meth)acrylate; the oligomer B has the structural formula shown in Formula 2: wherein m is an integer of 1 to 3, R5 is a linear fluorinated polyether unit or a branched fluorinated polyester unit, and R6 is selected from C 1-20 Alkyl, C 3-30 Cycloalkyl, C 6-30 Any of aryl, wherein the alkyl, cycloalkyl or aryl groups may be substituted by one or more R' groups in each case, R' being the same or different in each case and being respectively hydroxyl, a straight-chain alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, and R7 being H or methyl.

4. The low refractive index resin composition according to claim 3, characterized in that: The structural formula of the fluorinated polyether unit is CH2CF2O(CF2CF2O) y (CF2O) z CF2CH2, (CH2CH2O) x CH2CF2O(CF2CF2O) y (CF2O) Z CF2CH2(OCH2CH2) x , where x, y and z are the degrees of polymerization.

5. The low refractive index resin composition according to claim 4, characterized in that: The number average molecular weight of the fluorine-containing polyol is between 1500 and 5000.

6. The low-refractive index resin composition according to claim 1, characterized in that The monomer C is selected from the fluorinated acrylate shown in Formula 3: R8 is C 1-10 R9 is a single bond, hydroxyl substituted or unsubstituted C 1-5 The alkylene group, R 10 It is H or methyl.

7. The low-refractive index resin composition according to claim 6, characterized in that The mass ratio of the oligomer A, oligomer B, monomer C and polymerization initiator is (2-4):(4-6):(1-2):(0.1-0.3).

8. The low refractive index resin composition according to claim 2, characterized in that: The oligomer A is prepared according to the following steps: adding an auxiliary agent to the fluorinated diol, dropping isocyanate at room temperature, controlling the reaction temperature below 30°C, and after the dropwise addition is completed, the reaction temperature is raised to 60-70°C, and the reaction is carried out for 1-3h, and then dropping hydroxy acrylate into the reaction bottle, and the temperature is controlled at 60-70°C. After the dropwise addition is completed, the reaction is carried out for 0.5-3h; The oligomer B is prepared according to the following steps: adding an auxiliary agent to the fluorinated diol, adding isocyanate dropwise at room temperature, controlling the reaction temperature at 40-70° C., and reacting for 1-3 hours.

9. An application of the low refractive index resin composition according to any one of claims 1 to 8, characterized in that: It is used as a coating for optical fibers.

10. An optical fiber coating, characterized in that: The invention is prepared by photocuring the low-refractive-index resin composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Optical fiber inner coating having function of rapid radiation curing

    CN109929429A

  • Low-refractive-index optical fiber inner-layer coating and preparation method thereof

    CN111187568A

  • Resin composition and cured product

    JP1999349646A