A method for preparing anodized aluminum-magnesium alloy strip
Through the preparation method of anodized aluminum-magnesium alloy strip, combined with the characteristics and process optimization of aluminum-magnesium alloy, the problems of 5-Series aluminum alloy in terms of yield strength, yield rate and production cost are solved, and high strength, high toughness and low Cost anodizing effect.
Patent Information
- Application Number
- CN202410962470.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing 5-series aluminum alloys are difficult to ensure high yield strength, high yield and low production costs.
The preparation method of anodized aluminum-magnesium alloy strip is adopted, including melting of raw aluminum and intermediate metals, composition analysis, semi-continuous casting, sawing, milling, homogenizing, hot rolling, cold rolling, intermediate annealing, stabilizing annealing, acid The washing and bending straightening process controls the matching relationship between the contact arc length and the absolute deformation amount of the rolling deformation zone, improves the allowable addition of Fe elements to 0.35%, and reduces the dependence on high-purity aluminum ingots.
The mechanical properties of the anodized aluminum-magnesium alloy strip and the consistency of surface grains are effectively controlled, the anodized effect is improved, the production cost is reduced, and the appearance quality of the anodized is improved while ensuring high strength and high toughness is improved.
Smart Images

Figure CN118497644B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy strip preparation, and in particular to a method for preparing an anodized aluminum-magnesium alloy strip. Background Art
[0002] In the needs of various industries, aesthetics and safety have gradually become the focus of attention, especially for business travel luggage, car decorations, electronic digital products, etc. On the one hand, the products are required to have high strength, and on the other hand, they must be able to meet complex molding and good anode appearance, and the anode appearance is more required to be free of stripe and regional color difference defects. If 6 series aluminum alloy is used as the raw material for manufacturing products, it is difficult to form in the T6 state. And although it is easier to form in the T4 state, aging treatment increases costs and affects the yield. Therefore, 5 series aluminum alloy has become the research focus of large-size anodized materials.
[0003] In the existing production technology of 5 series aluminum alloys, it is difficult to ensure high yield strength while taking into account the problems of high product yield and low production cost. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the problem in the prior art that 5 series aluminum alloys are difficult to simultaneously ensure high yield strength, high yield rate of products made therefrom and low production cost.
[0006] (II) Technical solution
[0007] To this end, the present invention provides a method for preparing an anodized aluminum-magnesium alloy strip, comprising:
[0008] Step 1: melt the raw aluminum and the intermediate metal, analyze the composition of the molten material, treat the melt quality, and then use semi-continuous casting to obtain an ingot;
[0009] Step 2: After sawing and milling the ingot, the ingot is heated evenly, and then the ingot is taken out of the furnace and hot-rolled to obtain a coil;
[0010] Step 3: The obtained coil is subjected to intermediate annealing after 2 to 5 cold rolling passes, and then subjected to stabilization annealing after 1 to 2 cold rolling passes; the contact arc length L of the rolling deformation zone in each pass and the absolute deformation amount △H satisfy L≤12×△H.
[0011] Step 4: Pickling the surface of the coil after stabilization annealing with a pickling solution;
[0012] Step 5: cold rolling the pickled coil to obtain a rolled material with a preset thickness;
[0013] Step 6: The cold-rolled material to a preset thickness is subjected to a stretching, bending and straightening process to obtain a finished product.
[0014] Furthermore, in step 2, the equalization is bipolar heating, and the ingot after sawing and milling is first kept at a metal temperature of 430-480°C for 8-12 hours, and then the temperature is increased to 500-520°C and kept for 10-20 hours.
[0015] Furthermore, in step 2, the final rolling temperature of the hot rolling is 320-360° C., and the thickness of the obtained coil is 3.5-5.0 mm.
[0016] Furthermore, in step 3, the process conditions of the intermediate annealing are to control the temperature to 280-320° C. and the time to 12-24 hours.
[0017] Furthermore, in step 3, in the cold rolling process before the intermediate annealing, the total deformation of the coil is controlled to be above 60%.
[0018] Furthermore, in step 3, in the cold rolling process after the intermediate annealing, the total deformation of the coil is controlled to be 15-40%.
[0019] Furthermore, in step 3, the process conditions of the stabilization annealing are to control the temperature to 120-280° C. and the time to 10-20 hours.
[0020] Furthermore, in step 4, it also includes: mixing sulfuric acid, nitric acid and phosphoric acid in a volume ratio of (1-2): (2-3): (6-7) to obtain a mixed solution, and mixing the mixed solution with ionized water in a volume ratio of 1:5 to obtain a pickling solution.
[0021] (III) Beneficial effects
[0022] The beneficial effects of the present invention are as follows: the present invention mentions a method for preparing an anodized aluminum-magnesium alloy strip, comprising: step 1: melting raw aluminum and intermediate metal, analyzing the composition of the melted material, treating the melt quality, and obtaining an ingot by semi-continuous casting; step 2: sawing and milling the ingot and then hot-rolling the ingot to obtain a coil; step 3: performing intermediate annealing after 2 to 5 cold rolling passes of the obtained coil, and then performing stabilization annealing after 1 to 2 cold rolling passes; the contact arc length L of each rolling deformation zone and the absolute deformation △H satisfy L≤12×△H. Step 4: surface pickling the coil after stabilization annealing with pickling liquid; step 5: cold rolling the pickled coil to obtain a rolled material of a preset thickness; step 6: the rolled material cold rolled to a preset thickness is subjected to a stretching and straightening process to obtain a finished product.
[0023] This application effectively controls the mechanical properties, surface grains and micro-stress consistency of anodized aluminum-magnesium alloy strips by controlling the composition, rolling process, stabilization annealing and pickling process conditions, so that the stress corrosion inhomogeneity of the anodizing process is further controlled, thereby playing a positive role in ultimately ensuring high strength and high toughness to improve the anodizing effect. At the same time, the present invention greatly increases the allowable addition amount of Fe element to 0.35% under the background of ensuring good appearance quality after anodizing, and thus does not need to use high-purity aluminum ingots as raw materials, which greatly saves production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a diagram showing the surface condition of the anodized aluminum-magnesium alloy strip prepared in Example 1 of the present invention after anodization;
[0025] Figure 2 This is a diagram showing the surface condition of the aluminum plate strip prepared in Comparative Example 1 of the present invention after anodizing;
[0026] Figure 3 This is a diagram showing the overall situation of the anodized aluminum-magnesium alloy strip prepared in Example 1 of the present invention after being stamped into a complex structure;
[0027] Figure 4 This is a diagram showing the overall situation of the aluminum plate and strip prepared in Comparative Example 1 of the present invention after being stamped into a complex structure;
[0028] Figure 5 This is a schematic diagram of the rolling of the aluminum plate and strip prepared in Comparative Example 1 of the present invention;
[0029] Figure 6 This is a surface microstructure image of an anodized aluminum-magnesium alloy strip prepared in Example 2 of the present invention;
[0030] Figure 7 This is a surface structure morphology of the aluminum plate and strip prepared in Comparative Example 1 of the present invention;
[0031] Figure 8 The present invention is a process flow chart of a method for preparing an anodized aluminum-magnesium alloy strip. DETAILED DESCRIPTION
[0032] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0033] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range limited by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0034] In these embodiments, unless otherwise specified, the parts and percentages are all by mass. "Parts by mass" refers to the basic unit of measurement representing the mass ratio of multiple components, and 1 part can represent any unit mass, such as 1 g, 3.527 g, etc. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts. "And / or" is used to indicate that one or both of the situations described may occur, for example, A and / or B include (A and B) and (A or B).
[0035] It should be noted that this application takes the 5 series alloy with high strength and high toughness as the starting point, optimizes the alloy composition and the ingredients composition under the condition of studying the fluidity and casting uniformity of the product with Mg content exceeding 5.5%, and obtains the anodized aluminum-magnesium alloy strip by optimizing and controlling the cold rolling roller and the cold rolling deformation, pre-treating the high Mg alloy precipitation phase before anodizing, etc. The anodized aluminum-magnesium alloy strip mentioned in this application is a 5 series aluminum alloy rolled plate with high strength, high toughness and high anodized appearance quality.
[0036] refer to Figure 8 The present invention provides a method for preparing an anodized aluminum-magnesium alloy strip, comprising:
[0037] Step 1: melt the raw aluminum and the intermediate metal, analyze the composition of the molten material, treat the melt quality, and then use semi-continuous casting to obtain an ingot;
[0038] It should be noted that the raw aluminum can be scrap aluminum or aluminum ingots, and the intermediate metal can be one or more of Al-10Si, Al-10Fe, Al-50Cu, Al-10Mn, pure Mg, pure Zn or Al-5Ti.
[0039] The preparation method mentioned in this application is the latest process technology for the current high-strength 5 series aluminum alloy anodized materials. Due to the limited resources and high prices of high-purity aluminum ingots, the production cost of using high-purity aluminum is very high. The present invention selects waste aluminum or aluminum ingots as raw materials to produce low-cost aluminum alloy products without banded color difference after anodizing.
[0040] Step 2: After sawing and milling the ingot, the ingot is heated evenly, and then the ingot is taken out of the furnace and hot-rolled to obtain a coil;
[0041] It should be noted that the soaking process is bipolar heating. First, the sawn and milled ingot is kept at a metal temperature of 430-480°C for 8-12 hours, then heated to 500-520°C and kept for 10-20 hours. The final rolling temperature of hot rolling is 320-360°C, and the thickness of the resulting coil is 3.5-5.0 mm.
[0042] Step 3: The hot rolled coil is subjected to intermediate annealing after 2 to 5 cold rolling passes, and then subjected to stabilization annealing after 1 to 2 cold rolling passes;
[0043] Exemplarily, the present application adopts a box-type furnace for intermediate annealing, which has a lower cost. It should be noted that for high-Mg alloy products, thanks to the rapid heating and cooling characteristics of the air cushion furnace equipment, the excess Mg is dissolved in the lattice, and less Mg-containing compounds are precipitated along the grain boundaries after intermediate annealing, while the box-type furnace has a slow cooling rate, and the excess Mg gradually precipitates along the grain boundaries. That is, during the pickling process, the product heated by the box-type furnace will show worse corrosion uniformity than the product heated by the air cushion furnace. After the pickling operation, small deformation rolling is performed, and the uneven corrosion pits after pickling corrosion are polished and polished, which greatly reduces the dependence on grain size, the number and distribution of precipitated phases, and corrosion uniformity.
[0044] In the technical solution, in step 3, the process conditions of the intermediate annealing are to control the temperature to 280-320°C and the time to 12-24h.
[0045] In the technical solution, in step 3, in the cold rolling process before the intermediate annealing, the total deformation of the coil is controlled to be above 60%.
[0046] In the technical solution, in step 3, the total cold rolling deformation after intermediate annealing is 15-40%.
[0047] In the technical solution, in step 3, the process conditions of the stabilization annealing are to control the temperature to 120-280°C and the time to 10-20h.
[0048] It should be noted that in the control of cold rolling deformation, it is necessary to strictly control the cold rolling process before intermediate annealing, and control the contact arc length L and absolute deformation △H of each rolling deformation zone, both of which need to satisfy L≤12×△H.
[0049] refer to Figure 5 , where L is the contact arc length between the rolling deformation zone and the roller, i.e. the thick line part in the figure, △H=H2-H1, where H2 represents the initial thickness of the coil and H1 represents the thickness of the coil after rolling.
[0050] Specifically, in order to solve the influence of high Fe content on the quality of oxide film during anodizing, the present invention proposes that the contact arc length L and the absolute deformation △H of the cold rolling deformation zone of each pass must satisfy L≤12×△H, that is, the contact arc length is limited during the rolling thinning process with the same deformation, thereby reducing the deformation length of the surface metal during the rolling process, and is conducive to improving the unevenness of the structural deformation in the width direction and the segregation and uneven distribution of the coarse β phase, and finally achieving the anodized appearance without stripe color difference defects under high Fe tolerance, greatly reducing the influence of Fe content on the appearance quality of anodized. After repeated verification and testing, the upper limit of the allowable addition of Fe element can be increased to 0.35%, which greatly saves production costs.
[0051] In order to minimize the tensile deformation of surface grains under the same rolling deformation △H, the present invention adopts the method of adjusting the use of small diameter rollers for rolling. Generally, rollers with a diameter of 160-250mm are selected to replace conventional rollers with a roller diameter of 380-460mm for rolling.
[0052] Based on this variable control, the resistance to surface deformation can be reduced, the uniformity of surface deformation can be ensured, and the uniformity of grains can be improved. At the same time, the deformation stress difference in different regions in the width direction is also smaller, which can make the electrochemical performance of the anodizing process closer. This application controls the matching relationship between the contact arc length L and the absolute deformation amount △H in the rolling deformation zone, so that the appearance quality of the product anode is not affected by the surface roughness, further reducing the production cost.
[0053] Furthermore, regarding the deformation amount after stabilization annealing, it is mainly because the rolling deformation closes the corrosion pits in the pickling process. If the deformation amount exceeds 5%, it will affect the strength and elongation, while if the deformation amount is less than 2%, it will be difficult to achieve the sealing effect.
[0054] It should be noted that in terms of the stabilization annealing temperature conditions, in order to improve the high elongation of the finished product, a higher stabilization annealing temperature must be used. When the temperature exceeds 200°C, the product will have good ductility. However, if it is at high temperature, the high Mg alloy will precipitate the AL-Mg phase along the grain boundary, which will significantly affect the electrochemical properties of the product.
[0055] Step 4: Pickling the surface of the coil after stabilization annealing with a pickling solution;
[0056] It should be noted that after the coil is stabilization annealed, it is pickled and rolled with a very small deformation amount, so that the high solid solubility Mg is precipitated to a certain extent during the stabilization annealing process. The tendency of strength reduction during the subsequent service of the product will be lower, and its mechanical properties will be more stable.
[0057] In step 4, it also includes: mixing sulfuric acid, nitric acid and phosphoric acid in a volume ratio of (1-2): (2-3): (6-7) to obtain a mixed solution, and mixing the mixed solution with ionized water in a volume ratio of 1:5 to obtain a pickling solution.
[0058] It should be noted that the surface pickling treatment is to remove the Al-Mg phase precipitated along the grain boundary or subgrain boundary after stabilization annealing, so as to improve the chemical stability of the aluminum sheet and strip during the anodizing process, which is beneficial to improve the appearance quality after anodizing.
[0059] Step 5: cold rolling the pickled coil to obtain a rolled material of a preset thickness; wherein, in the cold rolling process, the cold rolling deformation is 2-5%.
[0060] It should be noted that since the solid solubility of Mg in aluminum is very low at room temperature, when it exceeds 3.5%, the Mg-containing phase will easily precipitate along the grain boundaries during the stabilization heat treatment, affecting the corrosion resistance of the product, that is, affecting the thickness uniformity of the oxide film in the electrochemical process of anodizing. The higher the Mg content, the more Mg-containing precipitated phases, and the easier it is to form banded color differences after anodizing.
[0061] After pickling, rolling with a small deformation amount, i.e., cold rolling with a deformation amount of 2-5%, can be performed to polish the uneven corrosion pits after pickling and corrosion, greatly reducing the dependence on grain size, the number and distribution of precipitated phases, and corrosion uniformity, and accordingly designing a new alloy component composition. The present invention does not need to consider the factor that the number of Mg-containing precipitated phases will increase with the increase of Mg content, thereby affecting the surface quality, and directly ensures strength by increasing the Mg content, thereby being more convenient, lower cost, and better stability.
[0062] The present invention utilizes small deformation rolling after pickling to seal the corrosion pits formed after the precipitated phase is corroded, thereby reducing the influence of the precipitated phase under high Mg content on the subsequent anodizing process. This is the key process of the present invention to determine the chemical composition and reduce the process and cost.
[0063] Step 6: The cold-rolled material to a preset thickness is subjected to a bending and straightening process to obtain a finished product, wherein the elongation parameter of the bending and straightening process is set to 0.3-0.8%.
[0064] The present application pays full attention to controlling the combination of the stabilization annealing process and the pickling process so as to achieve that the anodized aluminum-magnesium alloy strip can still maintain a good anodized appearance effect at a high elongation.
[0065] In summary, the present application effectively controls the mechanical properties, surface grain and micro-stress consistency of anodized aluminum-magnesium alloy strips by controlling the component composition, rolling process, stabilization annealing and pickling process conditions, so that the stress corrosion inhomogeneity of the anodizing process is further controlled, thereby ultimately ensuring high strength and high toughness while improving the anodizing effect. It plays a positive role.
[0066] In order to better understand the technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0067] Example 1
[0068] refer to Figure 1 , Figure 1 This is a surface condition diagram of the anodized aluminum-magnesium alloy strip prepared in Example 1, whose composition and content are Si: 0.06wt%, Fe: 0.35wt%, Cu: 0.1wt%, Mn: 0.50wt%, Mg: 6.5wt%, Cr: 0.04wt%, Ti: 0.02wt%, and the remainder is Al and other impurities generated in the manufacturing process. The content of each impurity is ≤0.03%, and the total amount of impurities does not exceed 0.15%.
[0069] The preparation method comprises the following steps:
[0070] After the raw materials and master alloys are smelted, they are double filtered through a plate filter and a deep bed filter, and then semi-continuously cast to obtain an ingot of 420×1450 mm;
[0071] The obtained ingot is sawed and milled before entering the heating furnace, and is first heated at 480°C / 12h, then heated to 520°C / 10h, and then taken out of the furnace for hot rolling. The hot rolling final rolling temperature is 360°C, and the thickness of the hot rolled coil is 5.0mm.
[0072] The hot-rolled coil is subjected to cold rolling, heat treatment and other related processing. The thickness (mm) of each pass in the cold rolling and thinning process and the production process are as follows:
[0073] The thickness of each pass of the coil during the cold rolling process is 5.0mm-3.0mm-1.6mm-1.0mm. After intermediate annealing, the thickness is 0.84mm. After stabilization annealing and pickling, the thickness is 0.8mm, and then the finished product is obtained by bending and straightening.
[0074] The total cold rolling reduction before intermediate annealing is 80%; the rolling is carried out using a 100mm diameter cold rolling roller, and the rolling arc length L of the three passes is 10.0mm (12.0<12×2.0), 8.4mm (8.4<12×1.4) and 5.7mm (5.7<12×0.6), all of which meet L≤12×△H; then the intermediate annealing is carried out using a box furnace at a process condition of 320℃ / 24h, and then the coil is rolled to 0.84mm using a cold rolling deformation of 16%. Then the coil is annealed at 120℃ / 20h, and pickled after annealing and cooling. In the pickling bath, the ratio of phosphoric acid: nitric acid: phosphoric acid is 2:3:7, which is used for pickling treatment on the surface of the coil after dilution. The pickled coil is cold rolled at 4.8% and then straightened by bending to obtain the finished product.
[0075] The pickling process controls the speed to ensure that the contact reaction time is 20s.
[0076] The thickness of the aluminum sheet strip produced is 0.8 mm, the tensile strength of the product is 370 MPa, the yield strength is 320 MPa, the elongation is 14.6%, and there is no strip defect after anodizing.
[0077] Example 2
[0078] The anodized aluminum-magnesium alloy strip prepared in Example 2 has the following composition and content: Si: 0.02wt%, Fe: 0.13wt%, Cu: 0.03wt%, Mn: 0.10wt%, Mg: 5.5wt%, Cr: 0.02wt%, Ti: 0.012wt%, and the remainder is Al and other impurities generated during the manufacturing process. The content of each impurity is ≤0.03%, and the total amount of impurities does not exceed 0.15%.
[0079] The preparation method comprises the following steps:
[0080] After the raw materials and master alloys are smelted, they are double filtered through a plate filter and a deep bed filter, and then semi-continuously cast to obtain an ingot of 650×1650 mm;
[0081] The obtained ingot is sawed and milled before entering the heating furnace, and is first kept at 430℃ / 8h, then heated to 500℃ / 20h, and then taken out of the furnace for hot rolling. The final hot rolling temperature is 320℃, and the thickness of the hot rolled coil is 3.5mm.
[0082] The hot-rolled coil is subjected to cold rolling, heat treatment and other related processing. The thickness (mm) of each pass in the cold rolling and thinning process and the production process are as follows:
[0083] The thickness of each pass of the cold rolling process is 3.5mm-2.1mm-1.2mm-0.69mm. After intermediate annealing, the thickness is 0.41mm. After stabilization annealing and pickling, the thickness is 0.4mm. Then, the finished product is obtained by bending and straightening.
[0084] The total cold rolling reduction before intermediate annealing is 80%; 100mm diameter cold rolling rollers are used for rolling, and the arc lengths L of the three passes are 9.6mm (9.6<12×1.4), 7.7mm (7.7<12×0.9) and 5.8mm (5.8<12×0.51), respectively, all satisfying L≤12×△H; intermediate annealing is carried out under the process conditions of 280℃ / 12h, and then the coil is rolled to 0.41mm using a 40% cold rolling deformation. Then a box furnace is used to anneal the coil at 280℃ / 10h, and pickling is carried out after annealing and cooling. In the pickling tank, the ratio of phosphoric acid: nitric acid: phosphoric acid is 1:3:6, and after dilution, it is used for pickling treatment on the surface of the coil. The pickled coil is cold rolled by 2% and then straightened by bending to obtain the finished product;
[0085] The pickling process controls the speed to ensure that the contact reaction time is 10s.
[0086] The thickness of the aluminum plate strip produced is 0.4 mm, the tensile strength of the product is 380 MPa, the yield strength is 330 MPa, the elongation is 16.4%, and there is no strip defect after anodizing.
[0087] Comparative Example 1
[0088] A 5A06 aluminum alloy strip, whose alloy composition and content are Si: 0.05wt%, Fe: 0.2wt%, Cu: 0.08wt%, Mn: 0.3wt%, Mg: 6.4wt%, Zn: 0.15wt%, Ti: 0.022wt%, and the balance is Al and other impurities generated in the manufacturing process, the content of each impurity is ≤0.05%, and the total amount of impurities does not exceed 0.15%.
[0089] The preparation method comprises the following steps:
[0090] The pure aluminum ingot is fed into a smelting furnace for melting, and an appropriate amount of master alloy is added, and after the composition is adjusted, semi-continuous casting is performed to obtain an ingot of 520×1250 mm;
[0091] The obtained ingot is sawn and milled, and then put into a heating furnace, kept at 470°C for 8 hours, and then taken out of the furnace for hot rolling. The hot rolling final rolling temperature is 300°C, and the thickness of the hot-rolled coil is 4.0 mm.
[0092] The hot-rolled coil is first cold-rolled for 4 passes, each pass is produced using a cold-rolling roller with a diameter of 400 mm, and the rolling thickness is "4.0 mm-2.3 mm-1.7 mm-1.1 mm-0.7 mm" in sequence, with a total cold-rolling reduction of 82%; then, a box-type furnace is used to perform intermediate annealing at a process condition of 320°C / 20h, and then cold-rolled to 0.6 mm, with a total deformation of 14%;
[0093] 4) The product rolled to the finished thickness is set to an elongation of 0.5% for stretching and straightening, and the finished product is produced by splitting the shaft.
[0094] The thickness of the aluminum alloy strip produced is 0.6 mm, the tensile strength of the product is 370 MPa, the yield strength is 360 MPa, and the elongation is 8.6%. The strip defects of the product are obvious after anode treatment.
[0095] refer to Figure 1 and Figure 2 , Figure 1 and Figure 2 The surface conditions of the anodized aluminum-magnesium alloy strip prepared in Example 1 and the aluminum plate strip prepared in Comparative Example 1 are shown respectively. Figure 1 and Figure 2 By comparison, it can be seen that the anodized aluminum-magnesium alloy strip prepared by the present invention has no stripe defects on its surface after anodizing, while the aluminum strip prepared by the traditional process has obvious stripe defects on its surface after anodizing.
[0096] refer to Figure 3 and Figure 4 , Figure 3 and Figure 4 The anodized aluminum-magnesium alloy strip prepared in Example 1 and the aluminum plate strip prepared in Comparative Example 1 are the overall pictures of the two after being stamped into a complex structure. Figure 3 and Figure 4 By comparison, it can be seen that the anodized aluminum-magnesium alloy strip prepared by the present invention has no cracking after complex forming, while the aluminum plate strip prepared by the traditional process has obvious cracking after complex forming.
[0097] contrast Figure 6 and Figure 7It can be seen that the grain width of the product of the present invention is about 15 μm, while the grain size of the product of the general process reaches 40 μm, and the uniformity is even worse. The influence of the present invention on the uniformity of the organization is very significant.
[0098] Compared with traditional 5 series alloys, the present invention has made improvements in the aluminum ingot composition, ingredient formula, production process, etc., and added surface pickling treatment to remove the precipitated phase during the product production process. The resulting aluminum sheet and strip has good stamping performance, high strength and high anode appearance quality, and is very suitable for the development needs of various industries with complex molding structures and high appearance quality requirements.
[0099] The anodized aluminum-magnesium alloy strip prepared by the present invention has the following components and contents, with the sum of the weight percentages being 100%, Si≤0.06%, Fe≤0.35%, Cu≤0.1%, Cr≤0.05%, Ti≤0.02%, Mn content being 0.10%-0.50%, Mg content being 5.5%-6.5%, and the remainder being Al and a variety of non-negligible impurities.
[0100] In the present technical solution, there are multiple components of the impurities, and taking the sum of the weight percentages as 100%, the content of each impurity is ≤0.03%, and the total weight of the impurities does not exceed 0.15% of the total weight of the anodized aluminum-magnesium alloy strip.
[0101] The following is an explanation of the reasons for limiting the content of each component and the process:
[0102] Mg: Mg in the alloy is an essential additive element to ensure the strength of the alloy plate. If the Mg content exceeds 6.5%, it will accelerate the uneven distribution of Mg8Al5, thereby causing instability in the anodizing process, which is not conducive to obtaining a good appearance effect. In addition, the uneven size of Mg8Al5 is prone to overburning during the ingot heating process, affecting product quality.
[0103] Fe: Fe can provide a partial strengthening effect, but when the Fe content exceeds 0.35%, it will promote the increase of coarse β phase. This type of compound is in the shape of rods or strips, affecting the appearance quality after anodizing.
[0104] It should be noted that, under the background of ensuring good appearance quality after anodizing, the present invention greatly increases the allowable addition amount of Fe element to 0.35%, thereby eliminating the need to use high-purity aluminum ingots as raw materials, greatly saving production costs.
[0105] Ti: Ti can refine the grains and make the structure uniform, but when the content exceeds 0.02%, TiB2 tends to aggregate and form slag inclusions in the melt; if the addition amount is insufficient, the grain refinement effect cannot be achieved.
[0106] Mn: Mn is beneficial to improving the strength of the material, improving the hot cracking stability of high Mg alloys, and promoting the uniform distribution of Mg8Al5. It also has a certain effect on grain refinement. However, when its content exceeds 0.5%, it will significantly increase the recrystallization temperature and affect the uniformity of the grains after recrystallization.
[0107] The yield strength of the anodized aluminum-magnesium alloy strip prepared in this application is ≥300 MPa, and the elongation is ≥14%. The anodized aluminum-magnesium alloy strip of the present invention has a higher elongation, which is beneficial to the weight reduction of the product in application scenarios with high formability requirements. The anodized aluminum-magnesium alloy strip prepared by the present invention has no obvious stripe color difference and patch stripe defects, has the characteristics of high strength, high formability, good anodized appearance quality, etc., and is suitable for the development needs of various industries.
[0108] The above describes the basic principles, main features and advantages of the present invention. However, the above is only a specific embodiment of the present invention, and the technical features of the present invention are not limited thereto. Any other implementation methods derived by any technician in the field without departing from the technical solution of the present invention should be included in the patent scope of the present invention.
[0109] In the description of the present invention, each embodiment focuses on the differences from other embodiments, and the same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.
[0110] In the description of the present invention, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically limited. Moreover, the term "includes", "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes those elements, but also includes other elements not clearly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements limited by the sentence "comprising one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.
[0111] In the present invention, unless otherwise clearly specified and limited, when a first feature is “on” or “below” a second feature, it may be that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, when a first feature is “above”, “above” or “above” a second feature, it may be that the first feature is directly above or obliquely above the second feature, or it may simply mean that the first feature is higher in level than the second feature. When a first feature is “below”, “below” or “below” a second feature, it may be that the first feature is directly below or obliquely below the second feature, or it may simply mean that the first feature is lower in level than the second feature.
[0112] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "embodiment", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0113] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may alter, modify, replace and modify the above embodiments within the scope of the present invention.
Claims
1. A method for preparing an anodized aluminum-magnesium alloy strip, characterized in that: include: Step 1: melt the raw aluminum and the intermediate metal, analyze the composition of the melt, treat the melt quality, and then use semi-continuous casting to obtain an ingot; Step 2: sawing and milling the ingot and then soaking it, and then taking the ingot out of the furnace and hot rolling it to obtain a coil; Step 3: The obtained coil is subjected to intermediate annealing after 2 to 5 cold rolling passes, and then subjected to stabilization annealing after 1 to 2 cold rolling passes; the contact arc length L of the rolling deformation zone in each pass and the absolute deformation amount △H satisfy L≤12×△H, where L is the contact arc length between the rolling deformation zone and the roller, △H=H2-H1, H2 represents the initial thickness of the coil, and H1 represents the thickness of the coil after rolling; Step 4: Pickling the surface of the coil after stabilization annealing with a pickling solution; Step 5: cold rolling the pickled coil to obtain a rolled material of a preset thickness, wherein the cold rolling deformation is 2-5% in the cold rolling process; Step 6: The cold-rolled material to a preset thickness is subjected to a bending and straightening process to obtain a finished product; In step 2, the final rolling temperature of hot rolling is 320-360° C., and the thickness of the obtained coil is 3.5-5.0 mm; In step 3, in the cold rolling process before intermediate annealing, the total deformation of the coil is controlled to be above 60%; In step 3, in the cold rolling process after intermediate annealing, the total deformation of the coil is controlled to be 15-40%; In step 3, the process conditions of stabilization annealing are as follows: the temperature is controlled at 120-280° C. and the time is controlled at 10-20 h; In step 4, the process further comprises: mixing sulfuric acid, nitric acid and phosphoric acid in a volume ratio of (1-2):(2-3):(6-7) to obtain a mixed solution, and mixing the mixed solution with ionized water in a volume ratio of 1:5 to obtain a pickling solution; Taking the sum of weight percentage as 100%, the composition and content of the anodized aluminum-magnesium alloy strip are: Si≤0.06%, Fe≤0.35%, Cu≤0.1%, Cr≤0.05%, Ti≤0.02%, Mn content is 0.10%~0.50%, Mg content is 5.5%~6.5%, and the balance is Al and non-negligible impurities.
2. The method for preparing an anodized aluminum-magnesium alloy strip according to claim 1, characterized in that: In step 2, the uniform heating is bipolar heating. First, the ingot after sawing and milling is kept at a metal temperature of 430-480°C for 8-12 hours, and then the temperature is increased to 500-520°C and kept for 10-20 hours.
3. The method for preparing an anodized aluminum-magnesium alloy strip according to claim 1, characterized in that: In step 3, the process conditions of intermediate annealing are to control the temperature to 280-320° C. and the time to 12-24 hours.