Electrosilvering-imitating water-based coating composition as well as preparation method and application thereof

Through the combination of wrapped aluminum silver paste and specific resin, combined with organic bentonite and polypropylene glycol, the problem of poor mirror effect of existing imitation silver plating paint and lack of water-based paint is solved, achieving high adhesion, corrosion resistance and low VOC water-based paint. Coatings, suitable for automotive painting, meet the low-cost and efficient production requirements in the automotive field.

CN118725665APending Publication Date: 2024-10-01NIPPON PAINT CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310331608.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing imitation electroplated silver coatings used in the automotive field have poor mirror effects and lack of water-based coatings, making it difficult to meet the requirements for high adhesion, corrosion resistance and cycle resistance. There are also VOC and emission issues.

Method used

Using a combination of wrapped aluminum silver paste and specific resin, the aluminum silver paste is wrapped with thermosetting acrylic resin containing phosphoric acid groups, combined with organic bentonite and polypropylene glycol to prepare aluminum powder orientation agent, control the solvent amount and viscosity, and screen defoaming agents to reduce VOC and improve the mirror effect and adhesion of the paint.

Benefits of technology

A low-VOC, low-emission water-based coating has been achieved, with high mirror effect, excellent adhesion and corrosion resistance, and can present a metal texture like electroplating, meeting the low-cost and efficient production needs of automotive painting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004155096680000061
    Figure BDA0004155096680000061
  • Figure BDA0004155096680000071
    Figure BDA0004155096680000071
  • Figure BDA0004155096680000081
    Figure BDA0004155096680000081
Patent Text Reader

Abstract

The invention provides an electrosilvering-imitating water-based coating composition as well as a preparation method and application of the electrosilvering-imitating water-based coating composition. The water-based coating composition is prepared from the following components in parts by weight: 5 to 7 parts of acrylic emulsion, 2 to 4 parts of water-based amino resin, 0.5 to 2 parts of water-based polyester resin, 0.5 to 2 parts of water-based polyurethane, 10 to 16 parts of water-based color paste, 4 to 7 parts of coated aluminum paste, 1.5 to 3 parts of organic solvent, 10 to 14 parts of aluminum powder orientation agent and 45 to 60 parts of water, wherein the wrapped aluminum paste is prepared by wrapping aluminum paste with thermosetting acrylic resin containing phosphate groups, and the raw materials of the wrapped aluminum paste comprise aluminum paste, trimethylbenzene, isooctanol, the thermosetting acrylic resin containing phosphate groups and a surfactant. The water-based paint composition has a lower VOC value (less than or equal to 420 g / L) and higher angle-dependent heterochromatism, is excellent in adhesive force, weather resistance, cycle resistance and the like, has a high-glossiness mirror surface effect and metal texture, and is similar to a real electrosilvering appearance effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material preparation, and specifically comprises a water-based coating composition imitating electroplating silver, a preparation method and application thereof. Background Art

[0002] As an important branch of coatings, automotive coatings account for about 20% of the total coatings output in countries with developed automobile industries. At the same time, as a high-tech variety of coatings, it represents the level of a country's coatings industry technology. Therefore, while meeting consumers' high requirements for appearance and quality, it must also meet national standards for low VOC and low emissions.

[0003] At the same time, with the improvement of consumers' living standards, higher requirements are placed on the color and appearance of automobile bodies. The silver coating formed by electroplating silver technology has a certain development in the decoration field due to its strong reflective ability and good thermal conductivity, electrical conductivity and welding properties. However, electroplating can generally only attach the coating to the surface of metal materials, and it is almost impossible to perform electroplating operations on non-metallic materials. In addition, the large area of ​​the automobile body, the easy corrosion of steel materials, the high requirements for the comprehensive performance of the body coating (weather resistance, hiding power, etc.), the automobile is produced on an assembly line, the paint needs to be recycled for a long time, and the low cost and other factors are not conducive to the promotion of electroplating technology in the automotive field.

[0004] In order to meet the appearance requirements of automobile bodies in the automotive field and ensure the protective effect of the coating, imitation electroplating silver paint is currently widely used for spraying to achieve the appearance effect of the car body. However, the mirror effect of the existing imitation electroplating silver paint is poor, and there is no public imitation electroplating silver water-based paint. In view of this, it is necessary to develop a water-based paint that can meet the requirements of national standards and has a high mirror effect like electroplating, excellent adhesion, good corrosion resistance and cycle resistance. Summary of the invention

[0005] In view of the above problems existing in the prior art, the first object of the present invention is to provide an aqueous coating composition imitating electroplated silver. The aqueous coating composition has a lower VOC value (≤420g / L) and a higher angular heterochromaticity, and the formed coating film has good comprehensive performance, excellent adhesion, corrosion resistance, cycle resistance, etc., and the coating can show a metallic texture and a high mirror effect like electroplating, which is similar to the appearance effect of real electroplated silver.

[0006] A second object of the present invention is to provide a water-based coating that imitates electroplating silver.

[0007] The third object of the present invention is to provide a method for preparing the water-based coating as described above.

[0008] A fourth object of the present invention is to provide an application of the above-mentioned water-based coating composition or the above-mentioned water-based coating in automobile painting.

[0009] To achieve the above first object, the technical solution adopted by the present invention includes:

[0010] The present invention discloses a water-based coating composition for imitating electroplating silver, which comprises the following raw materials in parts by weight:

[0011] 5-7 parts of acrylic emulsion, 2-4 parts of water-based amino resin, 0.5-2 parts of water-based polyester resin, 0.5-2 parts of water-based polyurethane, 10-16 parts of water-based color paste, 4-7 parts of encapsulated aluminum silver paste, 1.5-3 parts of organic solvent, 10-14 parts of aluminum powder directing agent and 45-60 parts of water;

[0012] The encapsulated aluminum paste is prepared by encapsulating aluminum paste with a thermosetting acrylic resin containing a phosphoric acid group, and the raw materials of the encapsulated aluminum paste include aluminum paste, trimethylbenzene, isooctyl alcohol, a thermosetting acrylic resin containing a phosphoric acid group, and a surfactant.

[0013] Furthermore, the raw materials of the encapsulated aluminum paste include, by weight, 1-2 parts of aluminum paste, 1-2 parts of trimethylbenzene, 1-2 parts of isooctyl alcohol, 0.7-1.4 parts of thermosetting acrylic resin containing a phosphoric acid group, and 0.5-1 parts of a surfactant;

[0014] Furthermore, the mass ratio of the aluminum paste, trimethylbenzene and isooctyl alcohol is 1:1:1.

[0015] Furthermore, the encapsulated aluminum-silver paste is prepared by the following method:

[0016] Dissolve the aluminum silver paste in a mixed solution of trimethylbenzene and isooctyl alcohol;

[0017] Adding a thermosetting acrylic resin containing a phosphoric acid group under stirring conditions to encapsulate the aluminum paste;

[0018] When the particle size is ≤20μm, add the surfactant and mix well.

[0019] Furthermore, the aluminum-silver paste is a silver dollar type aluminum-silver paste.

[0020] Furthermore, the aluminum-silver paste has a particle size D50 of 8-12 μm measured from small to large.

[0021] Furthermore, the thickness-to-diameter ratio of the aluminum-silver paste is 60:1-80:1.

[0022] Furthermore, the aluminum powder directing agent is composed of 1.5-2.5 parts of organic bentonite, 96-98 parts of water and 0.8-1.2 parts of polypropylene glycol in parts by weight.

[0023] Furthermore, the water-based color paste contains 9-11 parts of black paste.

[0024] Furthermore, the aqueous coating composition further comprises, by weight, 0.4-0.8 parts of a rheological additive, 0.1-0.4 parts of a tackifier, 0.1-0.4 parts of a dispersant, 0-0.2 parts of a defoamer and 0.1-0.4 parts of a pH adjuster.

[0025] To achieve the above second purpose, the technical solution adopted by the present invention includes:

[0026] The invention discloses a water-based paint imitating electroplating silver. The water-based paint is prepared from raw materials comprising the water-based paint composition as described above.

[0027] To achieve the third objective above, the technical solution adopted by the present invention includes:

[0028] The present invention discloses a method for preparing the water-based coating as described above, comprising the following steps:

[0029] Add organic solvent, acrylic emulsion, water-based amino resin, water-based polyester resin, water-based polyurethane, water-based color paste, encapsulated aluminum silver paste, and aluminum powder directing agent into the container in sequence, control the pH to 8.0-8.4, add water and stir until the required viscosity is reached.

[0030] To achieve the fourth objective above, the technical solution adopted by the present invention includes:

[0031] The present invention discloses an aqueous coating composition as described above or application of the aqueous coating as described above in automobile painting.

[0032] Furthermore, the application method comprises the following steps:

[0033] The metal substrate is sprayed with a primer and then sprayed with a water-based paint that simulates electroplating silver as described above.

[0034] Beneficial effects of the present invention:

[0035] The water-based coating composition provided in the present invention has the following advantages:

[0036] 1. Select appropriate water-based resins, pigments, additives, organic solvents and water to prepare water-based paint to meet the Ministry of Industry and Information Technology's water-based automotive paint access requirements.

[0037] 2. The specific aluminum paste is made into an encapsulated aluminum paste by using a specific resin encapsulation method, which avoids chemical reaction caused by direct contact between water and aluminum paste, making it easier to apply it in water-based paint systems. In addition, by controlling the thickness-to-diameter ratio of the aluminum paste, the fineness of the encapsulated aluminum paste, and the raw material composition and proportion of the encapsulated aluminum paste, the solubility, hydrophilicity, dispersibility and stability of the encapsulated aluminum paste in water-based paints can be further improved.

[0038] 3. Through solvent screening, the amount of solvent added is reduced while considering the requirements of aluminum paste solubility, defoaming properties, and VOC content, and the solid content of the coating is controlled to meet the national standard GB / T 38597 Water-based coatings - Original automotive coatings (passenger cars) - Basecoat ≤420g / L.

[0039] 4. By using organic bentonite as the directional aid of the water-based paint and controlling the ratio of organic bentonite to water, an aluminum powder directional agent with good stability and not easy to gel is obtained, which solves the problem of poor directional arrangement of aluminum powder in water-based paint and enables the paint to form a film to achieve high FF properties of color.

[0040] 5. Through the reduction of viscosity and high pigment-to-base ratio, the film thickness of the paint can be reduced to 1-2μm, and the arrangement of the aluminum silver paste is more flat and uniform, showing a good mirror effect.

[0041] 6. Through NV ≥ 11% and defoaming agent screening, poor defoaming, abnormal appearance and excessive VOC can be avoided under low viscosity and low NV conditions.

[0042] 7. The coating prepared by the coating composition of the present invention is helpful to improve the coating process of automobile bodies when used for coating. Due to the low film thickness and better hiding power, the color paint can be sprayed in one coat instead of two coats, and the other coat is sprayed with solid color paint to ensure comprehensive performance, and the middle coating process can be eliminated to achieve low VOC and low CO2 emissions. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1a The front view of the coatings obtained in Example 4 of the present invention and Comparative Example 10 is shown.

[0044] Figure 1b The side physical pictures of the coatings obtained in Example 4 of the present invention and Comparative Example 10 are shown.

[0045] Figure 2 The scanning electron microscope images (500 times) of the coatings obtained in Example 4 of the present invention and Comparative Example 10 are shown.

[0046] Figure 3 The scanning electron microscope images (1000 times) of the coatings obtained in Example 4 of the present invention and Comparative Example 10 are shown. DETAILED DESCRIPTION

[0047] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and drawings. It should be clear that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] The purpose of the present invention is illustrated by the following examples. The components of the composition are illustrated in parts by weight as a general standard. Unless otherwise specified, for the sake of simplicity, the "parts" described in the examples of the present invention have the same meaning as parts by weight.

[0049] The present invention provides an aqueous coating composition for imitating electroplating silver, which comprises the following raw materials in parts by weight:

[0050] 5-7 parts of acrylic emulsion, 2-4 parts of water-based amino resin, 0.5-2 parts of water-based polyester resin, 0.5-2 parts of water-based polyurethane, 10-16 parts of water-based color paste, 4-7 parts of encapsulated aluminum silver paste, 1.5-3 parts of organic solvent, 10-14 parts of aluminum powder directing agent and 45-60 parts of water;

[0051] The encapsulated aluminum paste is prepared by encapsulating aluminum paste with a thermosetting acrylic resin containing a phosphoric acid group, and the raw materials of the encapsulated aluminum paste include aluminum paste, trimethylbenzene, isooctyl alcohol, a thermosetting acrylic resin containing a phosphoric acid group, and a surfactant.

[0052] The first problem that needs to be solved is that the water-based coating composition is a water-based polymer membrane system. If the aluminum-silver paste comes into direct contact with water, not only will aluminum hydroxide be generated, causing the overall color of the coating to darken and become unusable, but more seriously, the generated hydrogen will bring the risk of flammability and explosion. For this reason, the inventors selected a packaging technology to pre-treat the aluminum-silver paste and isolate the aluminum-silver paste from water so that it can be safely put into the production of water-based coatings.

[0053] Although there are many organic solvents on the market that can dissolve aluminum paste, such as ester solvents, aromatic solvents, alcohol solvents, ether solvents, etc., ester solvents have poor hydrophilicity and are not suitable for water-based coatings. Benzene, toluene, xylene, and ethylbenzene in aromatic solvents cannot be used due to national standards. Although alcohol solvents and ether solvents have good hydrophilicity, they have poor solubility in aluminum paste and cannot meet application requirements. For this reason, the inventor weighed various factors and finally determined to use a combination of trimethylbenzene and isooctyl alcohol through a large number of experimental screenings. This combination is not only not restricted by national standards, but also takes into account hydrophilicity and solubility.

[0054] Furthermore, after selecting an organic solvent to dissolve the aluminum paste, the aluminum paste also needs to be coated. Although the traditional silicon-coated aluminum paste can use the coating film formed by SiO2 to protect the aluminum paste, the coating layer formed by SiO2 has poor permeability, which will reduce the brightness of the aluminum paste itself. At the same time, because SiO2 is an inorganic substance and the coating is an organic resin system, the groups on the resin cannot be well anchored on the surface of the aluminum paste, resulting in worse orientation of the aluminum powder and worse mirror effect; another coating method is to introduce organic phosphorus compounds, such as Aika's stapa series and Xingbolian's aquasilbp / an, but because small molecule compounds are added, it is difficult to truly protect the stability of the aluminum powder in water; and the physical protection method usually uses a polystyrene resin layer to coat the aluminum paste, but because the adhesion between the polystyrene resin layer and the aluminum powder is weak, the resin layer can easily fall off the surface of the aluminum powder under high shear, losing its protective effect on the aluminum powder, and is not suitable. In a specific embodiment, a thermosetting acrylic resin containing a phosphoric acid group is finally selected for coating in combination with various factors, and a surfactant is added after uniform coating to further improve the dispersibility and stability of the aluminum paste in the aqueous system, wherein the selected acrylic resin contains a phosphoric acid group, which is anchored by the phosphoric acid group and the surface of the aluminum powder to provide good and lasting protection, and at the same time, the acrylic resin and the aluminum powder orienting agent form a network structure, so that the aluminum powder is well oriented in the coating, and high FF properties of the coating are achieved; in a specific embodiment, the raw materials of the encapsulated aluminum paste include 1-2 parts of aluminum paste, 1-2 parts of trimethylbenzene, 1-2 parts of isooctyl alcohol, 0.7-1.4 parts of a thermosetting acrylic resin containing a phosphoric acid group, and 0.5-1 parts of a surfactant; in order to ensure the hydrophilicity and solubility of the aluminum paste, when the mass ratio of the aluminum paste, trimethylbenzene and isooctyl alcohol is 1:1:1, the best comprehensive effect is presented.

[0055] Furthermore, the encapsulated aluminum-silver paste is prepared by the following method:

[0056] Dissolve the aluminum silver paste in a mixed solution of trimethylbenzene and isooctyl alcohol;

[0057] Adding a thermosetting acrylic resin containing a phosphoric acid group under stirring conditions to encapsulate the aluminum paste;

[0058] When the particle size is ≤20μm, add the surfactant and mix well.

[0059] Furthermore, the aluminum paste is a silver dollar type aluminum paste. The silver dollar type aluminum paste can make the coating have good FF properties and reduce the deformation, breakage, and color and quality abnormalities of the aluminum paste caused by long-term circulation in the production line circulation system. For example, Dongyang FD-5090 and Z0684N can be selected.

[0060] Furthermore, the aluminum paste is measured from small to large particle size D50 between 8-12 μm. When the aluminum paste particle size D50 is less than 8 μm, the hiding power is reduced and the light transmittance resistance is reduced. When it is greater than 12 μm, the particle size is too large and will affect the FF property of the coating.

[0061] Furthermore, the thickness-to-diameter ratio of the aluminum paste is 60:1-80:1, and the state is stable after being wrapped with resin, and water is not easy to penetrate into the surface of the aluminum paste. The thickness-to-diameter ratio here can be understood as the ratio of the length of the aluminum sheet to the cross-sectional diameter of the aluminum sheet. This specific thickness-to-diameter ratio allows the aluminum paste to have a certain shape and particle size ratio, which can ensure that the paint after spraying has good anti-circulation properties. In the present invention, the aluminum paste has good angular heterochromaticity (also known as "FF property"), which is the property that the brightness changes with the angle of viewing the coated object, that is, the contrast between light (bright part) and dark (shaded part). If the thickness-to-diameter ratio is too low (for example, lower than 60:1), the hiding power is too poor. If it is higher than 80:1, the aluminum paste is too thin, and it is easy to deform and break after a long period of circulation in the circulation system, resulting in a contact reaction between the aluminum paste and water.

[0062] Furthermore, the water-based color paste includes 9-11 parts of black paste. Exemplarily, the black paste is a color paste after carbon black is pretreated, accounting for 9-11 parts; the water-based color paste also contains a small amount of other color pastes, and the other color pastes can be white paste, blue paste, purple paste, etc.; the white paste is a color paste after titanium white is pretreated, and the weight of the white paste is 0.1-2 parts; the blue paste is a color paste after phthalocyanine blue is pretreated, and the weight of the blue paste is 1-3 parts; the purple paste is a color paste after organic pigment purple is pretreated, and the weight of the purple paste is 0.1-1 part.

[0063] It is known to those skilled in the art that a variety of methods can be used to prepare black paste or other color pastes that meet the composite requirements, and the present invention does not impose any particular limitation. For example, some resins (such as acrylic resins), pigments, dispersing aids, etc. can be mixed evenly, sanded to a specified particle size, and then the required solvent is added to adjust to a specified viscosity and non-volatility, and the color is confirmed to be qualified.

[0064] The second problem is the selection of aluminum powder directional agent. Traditional solvent-based coatings use solvents to quickly dry, so that the aluminum paste is in a high viscosity state after spraying, so that the aluminum paste has good orientation. However, since water accounts for 50-80% of water in water-based coatings, there is still a lot of water in the coating film after spraying, and it needs to be preheated to 80 degrees, so the aluminum paste cannot be well oriented. The commonly used aluminum powder directional agent for solvent-based coatings is CAB (butyl cellulose acetate), and the technology of CAB application in water-based solvents is still imperfect. Moreover, since CAB is in a high solid and viscous state, a large amount of solvent is required for dissolution, which does not meet the requirements of national standards. After a large number of experimental studies, it is determined that when the selected aluminum powder directional agent is composed of 1.5-2.5 parts of organic bentonite, 96-98 parts of water and 0.8-1.2 parts of polypropylene glycol, it not only ensures good aluminum powder orientation, but also ensures good stability. Preferably, it is 2 parts of organic bentonite, 97 parts of water and 1 part of polypropylene glycol. If the proportion of organic bentonite is too high, the stability will deteriorate and it will easily gel; if the proportion of organic bentonite is too low, more aluminum powder orienting agent needs to be added to achieve good orientation, and the aluminum powder orienting agent has a high water content. If too much is added, the NV of the coating will decrease.

[0065] Furthermore, the aluminum powder directing agent is prepared by the following steps:

[0066] Add water into the container, add organic bentonite under high-speed stirring, stir evenly and then add polypropylene glycol. After passing the test, set aside.

[0067] Furthermore, the aqueous coating composition further comprises, by weight, 0.4-0.8 parts of a rheological additive, 0.1-0.4 parts of a viscous agent, 0.1-0.4 parts of a dispersant, 0-0.2 parts of a defoaming agent, and 0.1-0.4 parts of a pH adjuster. For example, the rheological additive includes, but is not limited to, AQ-630; the viscous agent includes, but is not limited to, UH-814N; the dispersant includes, but is not limited to, BYK-345; the defoaming agent includes, but is not limited to, SN 1341; and the pH adjuster includes, but is not limited to, dimethylethanolamine.

[0068] The third problem is the control of VOC. The national standard for coatings with a water content of ≥70% is based on the VOC detection method of GB / T 23986-2009 10.4 (solvent volume = VOC weight / (1-ρcoating*(water mass / water density)*ρcoating*1000). In order to reduce VOC (≤420g / L) to the greatest extent, it is necessary to reduce the solvent volume and increase NV at the same time. After calculation, to meet the regulatory requirements of VOC≤420g / L, the organic solvent volume of the coating must be ≤7.4%, the density must be ≤1.01g / ml, and the NV must be ≥11%. The higher the NV of the coating, the lower the VOC, but the higher the viscosity, the higher the film thickness, and the worse the FF property. Because the density of the resin, pigment, additive, etc. in the coating is greater than 1g / ml, the density can only be lowered by adding water or organic solvents. If there is too much organic solvent, the VOC exceeds the standard. If too much water is added, the defoaming will deteriorate and the appearance will be abnormal. Therefore, it is necessary to Comprehensive adjustments are required. The sources of organic solvents in water-based paints include: 1) organic solvents, additives, and resins used to dissolve aluminum-silver paste; 2) organic solvents contained in additives such as defoamers; 3) organic solvents directly added to the paint formula, so the amount of organic solvents needs to be reduced from the above three aspects respectively, but if the amount of organic solvents is too low, it will lead to paint workability problems such as incomplete dissolution of aluminum-silver paste, poor wrapping, and poor defoaming; and the sources of NV (non-volatile matter) in water-based paints include: 1) non-volatile matter in resins and color pastes in paints; 2) non-volatile matter in additives; as NV increases, viscosity will also increase accordingly, resulting in poor spreading of the coating film at low film thickness, so it is necessary to comprehensively consider and match the defoamer, amount of organic solvent added, and NV, and a large number of experiments are needed to screen out the appropriate combination.

[0069] The technical solution of the present invention is described below in conjunction with some specific embodiments, wherein the reagents used in the embodiments include:

[0070] Organobentonite was purchased from BYK's Laponite RD;

[0071] Silver dollar aluminum silver paste was purchased from Dongyang FD-5090D50 9μm;

[0072] The thermosetting acrylic resin containing phosphoric acid groups was purchased from Nippon Paint as ACS-1016;

[0073] Thermosetting acrylic resin was purchased from Mitsubishi Chemical HR-7066;

[0074] Acrylic emulsion was purchased from Nippon Paint's EMA-1032;

[0075] The surfactant was purchased from Air Products and Chemicals as SURFYNOL 465;

[0076] Trimethylbenzene and isooctyl alcohol were purchased from Hualun Chemical;

[0077] Organic solvents were purchased from Shell Oriental Chemical Company's TK, BYKETOL-WS from BYK;

[0078] The waterborne amino resin was purchased from CyMEL 250 of Cytec Industries;

[0079] The water-based polyester was purchased from Nippon Paint's PRS-1045RESIN;

[0080] Waterborne polyurethane was purchased from Sanyo Chemical as UCOAT N-800;

[0081] Polypropylene glycol was purchased from Sanyo Chemical Industries, Ltd. as PX-100;

[0082] The rheological additive was purchased from AQ-630 from Kusumoto Chemicals;

[0083] The adhesive was purchased from ADEKA Corporation UH-814N;

[0084] The defoamer was purchased from San Nopco as SN 1341;

[0085] The dispersant was purchased from BYK-345;

[0086] Experimental Example 1: Preparation of wrapped aluminum paste

[0087] The formula of the encapsulated aluminum paste in this experimental example is shown in Example 1 in Table 1. Five groups of comparative examples were designed to confirm factors such as the amount of solvent added, the dissolution of aluminum paste, and the encapsulating resin.

[0088] Table 1

[0089]

[0090] Production process: Add raw material 1 to the container, then add raw material 2 or 3, stir evenly, add raw material 4, slowly add raw material 5 or 6 under high-speed stirring, add raw material 7 after stirring evenly, confirm that the fineness range is less than or equal to 20μm, and the test is qualified; subsequently, add the mixture of 1-7 to the paint, 8 is used to clean the cylinder residue, clean it, and add the cleaned solution to the paint.

[0091] Table 2 is a test comparison of Example 1 and Comparative Examples 1-5. It can be seen from Table 2 that only Example 1 and Comparative Example 4 meet all the requirements. Comparative Example 1 uses toluene, which results in the coating not meeting regulatory requirements. In Comparative Example 2, part of the aluminum silver paste is not dissolved. In Comparative Example 3, the amount of hydrogen generated exceeds the standard. The aluminum powder is not wrapped and reacts with water, posing a safety hazard. The thermosetting acrylic resin used in Comparative Example 5 contains only hydroxyl groups but no phosphate groups. It is only a form of physical protection for the aluminum powder. Under high shear, the thermosetting acrylic resin will be peeled off, and the integrity of the aluminum powder wrapping will be reduced, which also poses a certain safety hazard. Therefore, Comparative Examples 1, 2, 3, and 5 are judged to be unqualified.

[0092] Table 2

[0093]

[0094] Note: The regulatory requirements are HJ 2537-Table 2 Limits of Hazardous Substances in Industrial Coatings

[0095] Experimental Example 2: Preparation of aluminum powder directional agent

[0096] The formula of the aluminum powder directing agent in this experimental example is shown in Example 2 in Table 3. At the same time, two groups of comparative examples are designed to confirm factors such as the ratio of the aluminum powder directing agent.

[0097] Production process: Add raw material 1 or 2 to the container, then add raw material 3 or 4, stir evenly under high-speed stirring, add raw material 5 or 6, and after the fineness is detected to be less than 5μm, package for later use.

[0098] Table 3

[0099] Aluminum powder directing agent Example 2 Comparative Example 6 Comparative Example 7 Serial number name Number of copies Number of copies Number of copies 1 Organic bentonite 2 3 - 2 Water-based CAB - - 20 3 water 97 97 28.4 4 Ethylene glycol - - 50 5 Polypropylene glycol 1 - - 6 dimethylethanolamine - - 1.6 Fineness ≤5μm OK OK OK Storage 1 month at room temperature OK NG OK

[0100] After testing, Example 2 and Comparative Example 7 meet the storage requirements, while Comparative Example 6 does not meet the storage requirements.

[0101] Experimental Example 3: Preparation of water-based coating composition

[0102] The formula of the water-based coating composition in this experimental example is shown in Examples 3 and 4 in Table 4. At the same time, Comparative Examples 8, 9, and 10 are set for parallel comparison, and the different encapsulated aluminum silver paste schemes (Comparative Example 4) and different aluminum powder directing agents (Comparative Example 7) selected above are respectively confirmed. At the same time, the difference between Examples 3 and 4 is that the coating density is different, so as to obtain the density and solvent amount control range that meet the requirements of VOC regulations. The specific formula is shown in Table 4.

[0103] Production process: Take a container and add raw materials 1-13 in sequence under stirring, then slowly add raw material 14 or 15, stir evenly, and after confirming that the fineness range is ≤20μm, add raw material 16, and add raw material 17 or 18 under high-speed stirring. During the production process, the pH is controlled at 8.0-8.4 through raw material 19, and finally raw material 20 is added and stirred evenly, and the viscosity is adjusted to 50-150mPa·s (60 rpm).

[0104] Table 4

[0105] Waterborne coating composition Example 3 Example 4 Comparative Example 8 Comparative Example 9 Comparative Example 10 Serial number name Number of copies Number of copies Number of copies Number of copies Number of copies 1 Acrylic Emulsion 6 6 6 6 6 2 Waterborne amino resin 2.4 2.4 2.4 2.4 2.4 3 Waterborne polyester resin 1 1 1 1 1 4 Waterborne polyurethane 1.2 1.2 1.2 1.2 1.2 5 Rheology additives 0.5 0.5 0.5 0.5 0.5 6 Adhesive 0.2 0.2 0.2 0.2 0.2 7 Defoamer (SN 1341) 0.1 0.2 0.1 0.1 - 8 Organic solvent TK 0.85 1.05 0.85 0.85 2 9 Organic solvent BYKETOL-WS 0.85 1.05 0.85 0.85 2 10 Water-based black paste 10 10 10 10 10 11 Water-based white paste 1 1 1 1 1 12 Water-based blue paste 2 2 2 2 2 13 Water-based purple paste 0.5 0.5 0.5 0.5 0.5 14 Wrapped aluminum paste (Example 1) 5.1 5.1 5.1 - - 15 Wrapped aluminum paste (Comparative Example 4) - - - 6.3 6.3 16 Dispersants 0.2 0.2 0.2 0.2 0.2 17 Aluminum powder directional agent (Example 2) 12 12 - 12 - 18 Aluminum powder directing agent (Comparative Example 7) - - 12 - - 19 dimethylethanolamine 0.3 0.3 0.3 0.3 0.3 20 water 55.8 55.8 55.8 55.8 44.4 total 100 100.5 100 101.2 80

[0106] The prepared coating was subjected to the following performance test items: appearance, FF property, etc. The results are shown in Table 5.

[0107] Table 5

[0108]

[0109]

[0110] Note: FI value is the metal texture index measured by X-Rite's spectrophotometer.

[0111] Conclusion: By adding the screened aluminum powder directing agent and the encapsulated aluminum silver paste of the present invention into the automotive water-based paint system, a silver-plating effect coating film with high FF property that meets the national VOC standard requirements can be obtained.

[0112] Experimental Example 4: Water-based coating compositions with different solvent addition amounts

[0113] The formula of the water-based coating composition in this experimental example can also be as shown in Examples 5 and 6 in Table 6. The difference between the two is the difference in NV. At the same time, three groups of comparative examples 11, 12, and 13 are designed to confirm different defoaming agents and different solvent reduction schemes to determine a formula that meets the requirements.

[0114] Production process: Take a container and add raw materials 1-14 in sequence under stirring, then slowly add raw material 15, stir evenly, confirm that the fineness range is ≤20μm, then add raw material 16, add raw material 17 under high-speed stirring, control the pH at 8.0-8.4 through raw material 18 during the production process, finally add raw material 19 and stir evenly, and adjust the viscosity to 50-150mPa·s (60 rpm).

[0115] Table 6

[0116]

[0117] The prepared coating was subjected to the following performance test items: appearance, FF property, etc. The results are shown in Table 7.

[0118] Table 7

[0119] project Require Example 5 Example 6 Comparative Example 11 Comparative Example 12 Comparative Example 13 NV % 11% 12% 11% 11% 11% Viscosity Rotor viscometer (60 rpm) 110 150 130 145 145 density g / ml 1.01 1.01 1.01 1.01 1.01 Fineness ≤20μm 20 20 20 20 20 pH 8.0-8.4 8.2 8.1 8.2 8.2 8.2 Film thickness μm 1-2 1-2 1-2 1-2 1-2 FF FI value 36 34 36 36 36 Defoaming Specific gravity after stirring / before stirring 84% 85% 79% 83% 81% Solvent ratio % 7.40% 8.1% 7.40% 9.20% 9.20% Solvent amount ≤420g / L 420 420 420 474 474 Coating appearance The coating surface has good appearance and no abnormality OK OK There are black spots OK OK determination qualified qualified Failure Failure Failure

[0120] Note: Black spots are caused by the poor defoaming ability of the defoaming agent. During spraying, the bubbles fail to burst in time, forming cavities on the surface of the coating, exposing the underlying color.

[0121] Defoaming is aimed at reducing bubbles generated in the production process or after spraying. Water-based paint is easy to bubble due to the high surface tension of water, and it is not easy to break after bubble formation. In the production process, the paint is mixed and dispersed evenly by high-speed stirring of the mixer. A large number of bubbles will be generated in this process, so it is necessary to add specific solvents or defoaming agents in the production process to reduce the generation of bubbles. At the same time, in the spraying process, the paint is atomized into small droplets by the high-speed rotation of the rotary cup on the spraying robot (30,000-60,000 rpm). A large number of bubbles will also be generated in this process, so the bubbles need to be broken as soon as possible after spraying to avoid problems such as pinholes. Therefore, qualified defoaming agents or solvents are screened out to achieve multiple functions of one raw material. It has been found through research that the defoaming agent SN1341 has a good defoaming effect in both production and spraying. The solvent TK has good defoaming properties in the spraying process while adjusting the volatilization rate of the paint. The solvent BYKETOL-WS has good defoaming properties in the production process of the paint while adjusting the volatilization rate of the paint.

[0122] According to the comparison between Examples 3, 4, 5, 6 and Comparative Examples 8-13, it can be concluded that in order to meet the regulatory requirement of VOC≤420g / L, at least the density of 1.0-1.01g / ml, the amount of organic solvent of 7-8.1%, and NV of 11-12% must be met.

[0123] Since it is applied to automobile bodies, the coatings that meet the coating properties requirements (Examples 3, 4, 5, and 6) need to be made into composite coatings for evaluation according to the process shown in Table 8 below. The results are shown in Table 9.

[0124] Table 8

[0125] Application Car body Effect Imitation electroplating effect Substrate Steel Primer Electrophoretic paint First coat of paint Dark pigment paint Second coat of paint Metallic paint (invention) Varnish Two-component varnish

[0126] Table 9

[0127]

[0128] The above implementation scheme has been put into mass production and application on automobile bodies. The automobile production line has confirmed that the laboratory results are consistent with expectations. It can provide colors that meet the national VOC standards and have high FF properties, and at the same time meet the requirements of continuous production of automobile production lines and qualified comprehensive performance.

[0129] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. An aqueous coating composition for imitating electroplating silver, characterized in that: The following raw materials are included by weight: 5-7 parts of acrylic emulsion, 2-4 parts of water-based amino resin, 0.5-2 parts of water-based polyester resin, 0.5-2 parts of water-based polyurethane, 10-16 parts of water-based color paste, 4-7 parts of encapsulated aluminum silver paste, 1.5-3 parts of organic solvent, 10-14 parts of aluminum powder directing agent and 45-60 parts of water; The encapsulated aluminum paste is prepared by encapsulating aluminum paste with a thermosetting acrylic resin containing a phosphoric acid group, and the raw materials of the encapsulated aluminum paste include aluminum paste, trimethylbenzene, isooctyl alcohol, a thermosetting acrylic resin containing a phosphoric acid group, and a surfactant.

2. The water-based coating composition according to claim 1, characterized in that: In terms of weight, the raw materials of the encapsulated aluminum paste include 1-2 parts of aluminum paste, 1-2 parts of trimethylbenzene, 1-2 parts of isooctyl alcohol, 0.7-1.4 parts of thermosetting acrylic resin containing phosphoric acid group and 0.5-1 parts of surfactant; Preferably, the mass ratio of the aluminum paste, trimethylbenzene and isooctyl alcohol is 1:1:

1.

3. The water-based coating composition according to claim 1, characterized in that: The wrapped aluminum silver paste is prepared by the following method: Dissolve the aluminum silver paste in a mixed solution of trimethylbenzene and isooctyl alcohol; Adding a thermosetting acrylic resin containing a phosphoric acid group under stirring conditions to encapsulate the aluminum paste; When the particle size is ≤20μm, add the surfactant and mix well.

4. The water-based coating composition according to claim 1, characterized in that: The aluminum-silver paste is a silver dollar type aluminum-silver paste; Preferably, the aluminum-silver paste has a particle size D50 of 8-12 μm measured from small to large. Preferably, the thickness-to-diameter ratio of the aluminum-silver paste is 60:1-80:

1.

5. The water-based coating composition according to claim 1, characterized in that: In terms of weight, the aluminum powder directing agent consists of 1.5-2.5 parts of organic bentonite, 96-98 parts of water and 0.8-1.2 parts of polypropylene glycol.

6. The water-based coating composition according to claim 1, characterized in that: The aqueous color paste contains 9-11 parts of black paste by weight; Preferably, the aqueous coating composition further comprises, by weight, 0.4-0.8 parts of a rheological additive, 0.1-0.4 parts of a tackifier, 0.1-0.4 parts of a dispersant, 0-0.2 parts of a defoamer and 0.1-0.4 parts of a pH adjuster.

7. A water-based paint imitating electroplating silver, characterized in that: The water-based coating is prepared from raw materials comprising the water-based coating composition according to any one of claims 1 to 6.

8. The method for preparing the water-based paint imitating electroplating silver according to claim 7, characterized in that: The steps include: Add organic solvent, acrylic emulsion, water-based amino resin, water-based polyester resin, water-based polyurethane, water-based color paste, encapsulated aluminum silver paste, and aluminum powder directing agent into the container in sequence, control the pH to 8.0-8.4, add water and stir until the required viscosity is reached.

9. Use of the water-based coating composition according to any one of claims 1 to 6 or the water-based coating imitating electroplating silver according to claim 7 in automobile painting.

10. The use according to claim 9, characterized in that: The application method comprises the following steps: A primer is sprayed on the metal substrate, and then the water-based paint imitating electroplating silver as claimed in claim 7 is sprayed.