Alloy baking paint coating with imitated crocodile texture surface as well as preparation method and construction method of alloy baking paint coating
By using a specific composition of imitation crocodile pattern alloy baking paint in high-temperature baking paint, combined with diluent, cellulose acetate butyrate, and matting powder, the problem of long distance between primer and topcoat and environmentally friendly aesthetics is solved. It achieves fast self-drying, beautiful texture and high-performance paint film effects.
Patent Information
- Application Number
- CN202411155359.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In the existing high-temperature baking paint construction, the distance between the primer and the topcoat is long, making it difficult to form an entire paint surface with special texture, and the requirements for environmental protection standards and aesthetics are not fully met.
It adopts a specific composition of imitation crocodile pattern alloy baked paint, including primer and topcoat. Through the synergistic compounding of thermosetting acrylic resin, phenylamino resin, cellulose acetate butyrate and other components, combined with diluent, the paint can be realized. The film dries by itself at room temperature, quickly evaporates the solvent, and forms a concave and convex texture effect. The combination of cellulose acetate butyrate and matting powder improves the weather resistance and aesthetics of the paint film.
It achieves rapid construction and beautiful crocodile skin texture effect, meets the wear resistance and anti-slip feel in high temperature and high humidity environments, and complies with children's toy-level environmental protection standards, improving production efficiency and product performance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a high-temperature resistant crocodile-like pattern surface alloy baked lacquer coating and a preparation method and a construction method thereof. Background Art
[0002] There are many types of high-temperature baking paint on the market, such as sand-textured paint, wrinkled paint, orange-textured paint, etc. As people pay more attention to the environmental protection and safety of items they touch daily, the demand for green paint is more urgent because adults may touch the paint surface through their fingers on a daily basis, which may indirectly contact food and children. In addition, the aesthetics of the surface is also an important indicator considered by consumers. In the existing technology, the construction interval between the primer and the topcoat is long, and it is difficult to form a whole paint surface with special textures. Summary of the invention
[0003] In view of this, the present invention provides a high temperature resistant crocodile pattern imitation alloy baked lacquer coating and a preparation method and a construction method thereof.
[0004] The technical solution of the present invention is: A crocodile-grain-like alloy baked paint coating, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 52-75 of a thermosetting acrylic resin, 21-39 of a phenylamino resin, 3-12 of a blocked isocyanate, 0.1-0.5 of a leveling agent, 2-8 of n-butanol, and 3-15 of a nano-color paste; The topcoat comprises the following components in parts by weight: 28-52 of secondary butyl resin, 4-12 of cellulose acetate butyrate, 0.5-2 of wax powder, 6-13 of matting powder, 7-15 of cyclohexanone, 15-42 of butanone and 3-15 of nano color paste.
[0005] Furthermore, the primer comprises the following components in parts by weight: 60-70 of thermosetting acrylic resin, 25-35 of phenylamino resin, 5-8 of blocked isocyanate, 0.15-0.3 of leveling agent, 3-5 of n-butanol, and 7-10 of nano-color paste.
[0006] Furthermore, the topcoat comprises the following components in parts by weight: 35-41 parts of secondary butyl ester, 6-8 parts of cellulose acetate butyrate, 0.8-1.2 parts of wax powder, 7-11 parts of matting powder, 8-12 parts of cyclohexanone, 22-30 parts of butanone, and 7-10 parts of nano color paste.
[0007] In particular, each component in the present invention needs to be tested for heavy metals, plasticizers and other environmental protection standards to ensure that the product supply process is environmentally monitored and meets the environmental protection standards for children's toys.
[0008] Furthermore, the invention also comprises a primer diluent, wherein the primer diluent comprises the following components in parts by weight: 82-105 parts of ethyl acetate and 3-10 parts of cyclohexanone.
[0009] Furthermore, the primer diluent comprises the following components in parts by weight: 95 parts of ethyl acetate and 5 parts of cyclohexanone.
[0010] In the present invention, ethyl acetate and cyclohexanone are synergistically compounded as primer diluents, and after the primer components are diluted, they are sprayed onto the surface of the alloy workpiece, so that the paint film dries at room temperature, the solvent evaporates quickly, and the waiting time for the construction operation is short, that is, the topcoat component can be sprayed, which solves the shortcoming of "slow surface drying" of baked paint and provides support for large-scale production on site in factories.
[0011] Furthermore, it also includes a topcoat thinner, which includes the following components in parts by weight: 28-45 parts of sec-butyl ester, 8-18 parts of cyclohexanone, and 48-69 parts of acetone.
[0012] Furthermore, the topcoat thinner comprises the following components in parts by weight: 35 parts of sec-butyl ester, 10 parts of cyclohexanone, and 55 parts of acetone.
[0013] In the present invention, acetone, cyclohexanone and sec-butyl ester are used as a topcoat thinner in a synergistic combination, so that the thinner contains a ketone solvent, which has a strong dissolving power and dries quickly. During the drying process, due to the quick drying of acetone, the paint film after spraying changes its surface, which should be flat and smooth, during the self-drying process at room temperature for about 1 minute, shrinks the paint oil of the topcoat component, and produces a concave-convex texture effect, thereby achieving the formation of the concave-convex texture effect and achieving the appearance of the paint film with a crocodile leather texture effect.
[0014] Furthermore, the type of cellulose acetate butyrate includes at least one of the following: CAB-381-0.5, CAB-381-2, CAB-381-20, CAB-551-0.01. The details are as follows: CAB-381-0.5: medium butyryl content, low viscosity, suitable for low construction viscosity and high solid content; CAB-381-2: Good miscibility, excellent flexibility, good weather resistance and UV resistance, high viscosity; CAB-551-0.01: high butyryl content and low viscosity, soluble in monomers such as styrene and methyl methacrylate, and has better tolerance to diluents such as aliphatic and aromatic hydrocarbons; CAB-381-20: High butyryl content, high viscosity, good comprehensive properties such as solubility, compatibility, water resistance, excellent surface hardness and high film strength.
[0015] Cellulose acetate butyrate has the following effects in paint topcoats: Improved leveling: Reduce paint film defects, improve the uniformity and aesthetics of the coating; Directed arrangement of metallic pigments: Optimize the amount of aluminum powder, reduce costs, and enhance metallic luster; Improved weather resistance: No yellowing / no gloss loss, enhance the outdoor durability of the paint; Shortened drying time: Improve production efficiency and speed up construction progress; Enhanced wear resistance and color stability: Increase the toughness of plastic coatings and increase their service life.
[0016] In particular, the present invention is applied to the fields of metal door lock accessories, ceramic handicrafts, electrical switches and sockets (including bakelite plastics), alloy toy car models, hardware toys, and electrical metal accessories.
[0017] In the present invention, the raw material composition formula of children's toys that meet the requirements of export to various countries is adopted, such as PAHS meets the second category children's toy standard, heavy metals meet the EN71-3-2019 standard, and phthalates meet the export standards, RoHS, US F963, and Chinese national standards.
[0018] In the present invention, the paint film has the advantages of high temperature resistance (within 160°C) and no yellowing through the synergistic compounding of thermosetting acrylic resin and cellulose acetate butyrate. The phenylamino resin and blocked isocyanate are compounded to participate in the cross-linking reaction of the thermosetting acrylic resin, which effectively improves the water resistance, hand sweat resistance and salt spray resistance of the paint film. In particular, the present invention can form a pattern decoration with a crocodile-like surface, while effectively protecting the surface of metal parts from oxidation. After testing, the hardness of the paint film formed by the present invention reaches the high hardness of Mitsubishi Pencil H, and can withstand long-term baking at an altitude of 100 degrees without damaging the paint film. The paint film tested for 96 hours in a high temperature and humidity environment (temperature 60°C, humidity 90) does not bubble or fall off.
[0019] Through the synergistic compounding of the components of the present invention and the specific construction process, the baked paint can form a surface effect with a matte gloss, and can present a rich texture appearance effect from larger moire to smaller cotton grain, which can give people a "feeling of touch", has a unique texture effect and excellent physical and mechanical properties, and satisfies consumers' pursuit of high-quality baked paint.
[0020] A method for preparing a crocodile-like surface alloy baked paint coating, comprising the preparation of a primer and a topcoat; The preparation method of the primer comprises the following steps: Add thermosetting acrylic resin, phenylamino resin, blocked isocyanate and leveling agent in sequence, and gradually increase the speed to 800-1000RPM for dispersion for 10-18 minutes, and stop when the fineness / cleanliness is ≥6H / A; n-Butanol was added to adjust the viscosity; Add nano color paste to adjust the color; The preparation method of the topcoat comprises the following: Add sec-butyl ester, cellulose acetate butyrate, wax powder, matting powder, and cyclohexanone in sequence, and gradually increase the speed to 600-1000RPM for dispersion for 15-25 minutes until the fineness / cleanliness is ≥4H / A; Add butanone to adjust the viscosity; Add nano color paste to adjust the color.
[0021] Furthermore, the preparation method also includes the preparation of a primer thinner and the preparation of a topcoat thinner; The preparation method of the primer thinner comprises the following steps: mixing ethyl ester and cyclohexanone respectively, and dispersing at a rotation speed of 500-800 RPM for 30-60 seconds; The preparation method of the topcoat thinner comprises the following steps: mixing sec-butyl ester, cyclohexanone and acetone respectively, and dispersing at a rotation speed of 500-800 RPM for 30-60 seconds.
[0022] A construction method for an alloy baked paint coating with an imitation crocodile pattern, comprising a primer construction and a topcoat construction; The primer construction includes the following: Prepare the substrate and pre-treat the surface; the surface of the substrate must be clean. If the substrate is metal, degrease, clean and dry it first.
[0023] Dilution treatment: dilute the primer to primer thinner at a volume ratio of 1:0.5-0.7; when used in conjunction with the primer thinner of the present invention, the construction operation in production is easier, or when using mechanical automatic spraying, the setting of the sprayer is simpler to debug to the required effect, and the qualified rate of the sprayed workpiece is improved.
[0024] Spraying construction: Control the viscosity to 10-25s (NK-2 viscosity cup), spray evenly with a paint film thickness of 20-25um. After 10-20 minutes, enter the second topcoat process.
[0025] The topcoat application includes the following: Dilution treatment: dilute the paint to paint thinner at a volume ratio of 1:0.7-1; when used in conjunction with the paint thinner of the present invention, the construction operation in production is easier, or when using mechanical automatic spraying, the sprayer can be set up more simply and debugged to achieve the desired effect, while the qualified rate of the sprayed workpiece is improved.
[0026] Spraying construction: After the primer is sprayed, let it dry for 10-20 minutes, then spray the topcoat component, control the viscosity to 10-25s (NK-2 viscosity cup), and use wet-on-wet construction to make the primer and topcoat two layers of paint film completely bonded together, and provide conditions for the subsequent paint film to shrink and crack and form concave and convex lines; In particular, in actual construction, the size of the alloy workpiece to be sprayed is used as a reference, and the effect determined by the designer is used as a reference. If a pattern with obvious concave and convex lines is required, a higher construction viscosity is required, that is, less diluent is added.
[0027] Drying treatment: first bake at 100-120℃ for 10-20min to prevent bubbling of the paint film; then heat to 145-165℃ and bake for 25-40 minutes. After thorough baking, you can get a crocodile leather effect paint film with qualified appearance and performance.
[0028] During the spraying construction, the topcoat is sprayed once to a film thickness of 20-30um. Do not wait for the surface to dry before re-spraying, otherwise it will affect the shrinkage and concave-convex effect of the topcoat; the required shrinkage and cracking degree of the topcoat is reached, and the film thickness is such that the concave-convex texture forms the planned crocodile leather effect; if the paint is applied thickly, a large concave-convex effect texture can be obtained. During the spraying construction, the caliber of the spray gun is controlled at 2.5-3.5mm, and the surface texture forming effect is the best.
[0029] It also includes matte adjustment, including using different colors of baked paint to modify the color or spraying varnish of different glossiness to adjust the matte effect to be achieved.
[0030] In the present invention, through a large number of creative experiments, it is found that due to the poor surface treatment of the matting powder, the amount of water / solvent absorbed is very high, and when the solvent evaporates, it is easy to cause the paint film to crack; cellulose acetate butyrate is also a high-viscosity raw material, and the amount of water / solvent absorbed is also very high. When these two raw materials are combined in the same formula and an appropriate quick-drying strong solvent is added, the solvent evaporates during the drying process, which will shrink the paint film and form a concave-convex texture effect. Through the setting of the matching diluent of the primer component and the matching diluent of the topcoat component of the present invention, in each combined formula, after the paint oil is matched and diluted, the solubility and volatilization speed of the overall paint oil are coordinated with the process for construction and spraying, and the solvent evaporates after the final construction and spraying. During the drying process, the paint film changes the surface of the paint film that should be flat and smooth, and the desired concave-convex texture effect appears.
[0031] In addition, it is also very important to control the content of matting powder in the topcoat. When the content is low, the paint film will not shrink enough and no concave and convex lines will be formed or the formed lines will not have a concave and convex feel; when the content is too high, the paint film surface will be "powdered". After drying, the paint film will be cut by a light touch with a fingernail. The formation of concave and convex lines is uncontrolled and the beautiful crocodile leather effect cannot be formed. In addition, the paint film fails basic performance tests such as hardness, fails the 100℃ boiling water resistance test, and fails the hand sweat resistance test.
[0032] In the present invention, the amount of matting agent used in the formula plays an important role. When the amount of matting agent used is low, the shrinkage of the paint film is very low, and the surface of the paint film after spraying is a smooth full matte paint film without crocodile leather effect, or only a semi-matte flat paint film appears after spraying without any bumps.
[0033] When the amount of matting powder is high, after the paint is dry, the crocodile leather effect has no hardness and poor adhesion. At the same time, the topcoat will appear seriously false and thick, and the viscosity will be lost. For example, during production and stirring, the material on the edge of the barrel will not be completely dispersed, and the resulting paint will be difficult to spray, and it is difficult to spray out a qualified crocodile leather effect.
[0034] The invention forms a crocodile leather-like decoration with characteristics by synergistically compounding cellulose acetate butyrate liquid, matting powder, primer thinner, and topcoat thinner, and has the original performance of high-temperature baking paint, high hardness, excellent wear resistance, good hand sweat and salt spray resistance, and the crocodile leather pattern formed has concave and convex patterns to have an anti-slip effect. All the raw materials used have passed environmental protection tests and reached the children's toy grade standard.
[0035] The beneficial effects of the present invention are: 1. Form a beautiful crocodile leather-like paint film on the surface of the workpiece, which has a non-slip concave-convex effect; 2. The paint film has the basic properties that ordinary metal baked paint should have, such as qualified adhesion, wear resistance and high hardness, resistance to high temperature and high humidity, resistance to alcohol scrubbing, etc.; 3. The paint film meets the environmental protection requirements of children's toys, such as heavy metals, plasticizers, and PAHS (polycyclic aromatic hydrocarbons) standards; 4. The construction interval between primer and topcoat is effectively shortened, which improves production efficiency and provides a basis for large-scale production. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described here are only used to explain the present invention and do not limit the scope of protection of the present invention. Example 1
[0037] A crocodile-grain-like alloy baked paint, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 67 parts of a thermosetting acrylic resin, 33 parts of a phenylamino resin, 6 parts of a blocked isocyanate, 0.2 parts of a leveling agent, 3.8 parts of n-butanol, and 10 parts of a nano-color paste; The topcoat comprises the following components in parts by weight: 41 parts of secondary butyl resin, 7.5 parts of cellulose acetate butyrate, 1 part of wax powder, 10 parts of matting powder, 10 parts of cyclohexanone, 20.5 parts of butanone, and 10 parts of nano color paste.
[0038] In this embodiment, the thermosetting acrylic resin adopts the LM-3050 product of Langma Chemical, the phenylamino resin adopts the K444HB product of Shunying Company, the blocked isocyanate adopts the K3142HA product of Shunying Company, and the leveling agent adopts the BYK313 product of BYK Company; the cellulose acetate butyrate adopts the product of Eastman Company of the United States, and the wax powder adopts the LANCO 1400SF product of Lubrizol Corporation of Germany.
[0039] The invention also comprises a primer thinner, which comprises the following components in parts by weight: 95 parts of ethyl acetate and 5 parts of cyclohexanone.
[0040] The invention also comprises a topcoat thinner, which comprises the following components in parts by weight: 35 parts of sec-butyl ester, 10 parts of cyclohexanone and 55 parts of acetone.
[0041] The model of the cellulose acetate butyrate is CAB-381-20. Example 2
[0042] A crocodile-like surface alloy baked paint, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 54 of a thermosetting acrylic resin, 24 of a phenylamino resin, 5 of a blocked isocyanate, 0.2 of a leveling agent, 3 of n-butanol, and 5 of a nano-color paste; The topcoat comprises the following components in parts by weight: 31 parts of secondary butyl resin, 5 parts of cellulose acetate butyrate, 0.8 parts of wax powder, 7 parts of matting powder, 9 parts of cyclohexanone, 16 parts of butanone, and 5 parts of nano color paste.
[0043] The invention also comprises a primer diluent, which comprises the following components in parts by weight: 84 parts of ethyl acetate and 4 parts of cyclohexanone.
[0044] The invention also comprises a topcoat thinner, which comprises the following components in parts by weight: 30 parts of sec-butyl ester, 10 parts of cyclohexanone and 51 parts of acetone.
[0045] The cellulose acetate butyrate is a combination of CAB-381-2 and CAB-381-20, with a mass ratio of 1:5. Example 3
[0046] A crocodile-grain-like alloy baked paint coating, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 72 parts of a thermosetting acrylic resin, 36 parts of a phenylamino resin, 11 parts of a blocked isocyanate, 0.4 parts of a leveling agent, 7 parts of n-butanol, and 14 parts of a nano-color paste; The topcoat comprises the following components in parts by weight: 50 parts of secondary butyl resin, 10 parts of cellulose acetate butyrate, 1.7 parts of wax powder, 12 parts of matting powder, 13 parts of cyclohexanone, 38 parts of butanone, and 14 parts of nano color paste.
[0047] The invention also comprises a primer thinner, which comprises the following components in parts by weight: 101 parts of ethyl acetate and 9 parts of cyclohexanone.
[0048] The invention also comprises a topcoat thinner, which comprises the following components in parts by weight: 43 parts of sec-butyl ester, 16 parts of cyclohexanone and 63 parts of acetone.
[0049] The cellulose acetate butyrate model is a combination of CAB-381-0.5 and CAB-381-20, and the mass ratio thereof is 1:9. Example 4
[0050] A crocodile-grain-like alloy baked paint, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 60 parts of a thermosetting acrylic resin, 25 parts of a phenylamino resin, 5 parts of a blocked isocyanate, 0.15 parts of a leveling agent, 3 parts of n-butanol, and 7 parts of a nano-color paste.
[0051] The topcoat comprises the following components in parts by weight: 35 parts of secondary butyl resin, 6 parts of cellulose acetate butyrate, 0.8 parts of wax powder, 7 parts of matting powder, 8 parts of cyclohexanone, 22 parts of butanone, and 7 parts of nano color paste.
[0052] The invention also comprises a primer thinner, which comprises the following components in parts by weight: 82 parts of ethyl acetate and 3 parts of cyclohexanone.
[0053] The invention also comprises a topcoat thinner, which comprises the following components in parts by weight: 28 parts of sec-butyl ester, 8 parts of cyclohexanone and 48 parts of acetone.
[0054] The cellulose acetate butyrate is a combination of CAB-381-20 and CAB-551-0.01, and the mass ratio thereof is 10:1. Example 5
[0055] A crocodile-grain-like alloy baked paint, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 70 parts of a thermosetting acrylic resin, 35 parts of a phenylamino resin, 8 parts of a blocked isocyanate, 0.3 parts of a leveling agent, 5 parts of n-butanol, and 10 parts of a nano-color paste.
[0056] The topcoat comprises the following components in parts by weight: 41 parts of secondary butyl resin, 8 parts of cellulose acetate butyrate, 1.2 parts of wax powder, 11 parts of matting powder, 12 parts of cyclohexanone, 30 parts of butanone, and 10 parts of nano color paste.
[0057] The invention also comprises a primer thinner, which comprises the following components in parts by weight: 95 parts of ethyl acetate and 6 parts of cyclohexanone.
[0058] The invention also comprises a topcoat thinner, which comprises the following components in parts by weight: 36 parts of sec-butyl ester, 15 parts of cyclohexanone and 55 parts of acetone.
[0059] The model of the cellulose acetate butyrate is CAB-381-2. Example 6
[0060] A crocodile-grain-like alloy baked paint, characterized in that it comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 67 parts of a thermosetting acrylic resin, 33 parts of a phenylamino resin, 6 parts of a blocked isocyanate, 0.2 parts of a leveling agent, 3.8 parts of n-butanol, and 10 parts of a nano-color paste; The topcoat comprises the following components in parts by weight: 41 parts of secondary butyl resin, 7.5 parts of cellulose acetate butyrate, 1 part of wax powder, 10 parts of matting powder, 10 parts of cyclohexanone, 20.5 parts of butanone, and 10 parts of nano color paste.
[0061] In this embodiment, the thermosetting acrylic resin adopts the LM-3050 product of Langma Chemical, the phenylamino resin adopts the K444HB product of Shunying Company, the blocked isocyanate adopts the K3142HA product of Shunying Company, and the leveling agent adopts the BYK313 product of BYK Company; the cellulose acetate butyrate adopts the product of Eastman Company of the United States, and the wax powder adopts the LANCO 1400SF product of Lubrizol Corporation of Germany.
[0062] The invention also comprises a primer thinner, which comprises the following components in parts by weight: 95 parts of ethyl acetate and 5 parts of cyclohexanone.
[0063] The invention also comprises a topcoat thinner, which comprises the following components in parts by weight: 35 parts of sec-butyl ester, 10 parts of cyclohexanone and 55 parts of acetone.
[0064] The model of the cellulose acetate butyrate is CAB-381-2. Example 7
[0065] A method for preparing a crocodile-like surface alloy baked paint coating, comprising the preparation of a primer and a topcoat; The preparation method of the primer comprises the following steps: Add thermosetting acrylic resin, phenylamino resin, blocked isocyanate and leveling agent in sequence, and gradually increase the speed to 900RPM for 15 minutes of dispersion until the fineness / cleanliness is ≥6H / A; n-Butanol was added to adjust the viscosity; Add nano color paste to adjust the color; The preparation method of the topcoat comprises the following: Add sec-butyl ester, cellulose acetate butyrate, wax powder, matting powder, and cyclohexanone in sequence, and gradually increase the speed to 900RPM for 20 minutes, until the fineness / cleanliness is ≥4H / A, and then stop; Add butanone to adjust the viscosity; Add nano color paste to adjust the color.
[0066] Furthermore, the preparation method also includes the preparation of a primer thinner and the preparation of a topcoat thinner; The preparation method of the primer thinner comprises the following steps: mixing ethyl ester and cyclohexanone respectively, and dispersing at a rotation speed of 600 RPM for 45 seconds; The preparation method of the topcoat thinner comprises the following steps: mixing sec-butyl ester, cyclohexanone and acetone respectively, and dispersing them at a rotation speed of 600 RPM for 45 seconds. Example 8
[0067] A method for preparing a crocodile-like surface alloy baked paint coating, comprising the preparation of a primer and a topcoat; The preparation method of the primer comprises the following steps: Add thermosetting acrylic resin, phenylamino resin, blocked isocyanate and leveling agent in sequence, and gradually increase the speed to 800RPM for 18 minutes of dispersion until the fineness / cleanliness is ≥6H / A; n-Butanol was added to adjust the viscosity; Add nano color paste to adjust the color; The preparation method of the topcoat comprises the following: Add sec-butyl ester, cellulose acetate butyrate, wax powder, matting powder and cyclohexanone in sequence, and gradually increase the speed to 600RPM for dispersion for 25 minutes until the fineness / cleanliness is ≥4H / A; Add butanone to adjust the viscosity; Add nano color paste to adjust the color.
[0068] Furthermore, the preparation method also includes the preparation of a primer thinner and the preparation of a topcoat thinner; The preparation method of the primer thinner comprises the following steps: mixing ethyl ester and cyclohexanone respectively, and dispersing at a rotation speed of 500 RPM for 60 seconds; The preparation method of the topcoat thinner comprises the following steps: mixing sec-butyl ester, cyclohexanone and acetone respectively, and dispersing them at a rotation speed of 500 RPM for 60 seconds. Example 9
[0069] A method for preparing a crocodile-like surface alloy baked paint coating, comprising the preparation of a primer and a topcoat; The preparation method of the primer comprises the following steps: Add thermosetting acrylic resin, phenylamino resin, blocked isocyanate and leveling agent in sequence, and gradually increase the speed to 1000RPM for dispersion for 10 minutes, and stop when the fineness / cleanliness is ≥6H / A; n-Butanol was added to adjust the viscosity; Add nano color paste to adjust the color; The preparation method of the topcoat comprises the following: Add sec-butyl ester, cellulose acetate butyrate, wax powder, matting powder, and cyclohexanone in sequence, and gradually increase the speed to 1000RPM for dispersion for 15 minutes until the fineness / cleanliness is ≥4H / A; Add butanone to adjust the viscosity; Add nano color paste to adjust the color.
[0070] Furthermore, the preparation method also includes the preparation of a primer thinner and the preparation of a topcoat thinner; The preparation method of the primer thinner comprises the following steps: mixing ethyl ester and cyclohexanone respectively, and dispersing at a rotation speed of 800 RPM for 30 seconds; The preparation method of the topcoat thinner comprises the following steps: mixing sec-butyl ester, cyclohexanone and acetone respectively, and dispersing them at a rotation speed of 800 RPM for 30 seconds. Example 10
[0071] A construction method for an alloy baked paint coating with an imitation crocodile pattern, comprising a primer construction and a topcoat construction; The primer construction includes the following: Prepare the substrate and pre-treat the surface; Dilution treatment: dilute according to the volume ratio of primer to primer thinner 1:0.6; Spraying construction: Control the viscosity to 15s, spray evenly with a paint film of 22um thickness, and after 15 minutes, enter the second topcoat process.
[0072] The topcoat application includes the following: Dilution treatment: dilute according to the volume ratio of topcoat to topcoat thinner 1:0.8; Spraying construction: After spraying the primer, let it dry for 15 minutes, then spray the topcoat component, control the viscosity to 18s, and use wet-on-wet construction; Drying treatment: first bake at 110℃ for 15 minutes, then increase the temperature to 155℃ and bake for 30 minutes.
[0073] During the spraying construction, the topcoat is sprayed once to a paint film thickness of 25 um.
[0074] During the spraying construction, the caliber of the spray gun is controlled at 3 mm.
[0075] It also includes gloss and matte adjustment, including using different colors of baked paint to correct the color or spraying varnish with different gloss levels. Embodiment 11
[0076] A construction method for an alloy baked paint coating with an imitation crocodile pattern, comprising a primer construction and a topcoat construction; The primer construction includes the following: Prepare the substrate and pre-treat the surface; Dilution treatment: dilute according to the volume ratio of primer to primer thinner 1:0.5; Spraying construction: Control the viscosity to 10-25s, spray evenly with a 25um thick paint film, and after 20 minutes, enter the second topcoat process.
[0077] The topcoat application includes the following: Dilution: dilute according to the volume ratio of topcoat to topcoat thinner 1:0.7; Spraying construction: After spraying the primer, let it dry for 20 minutes, then spray the topcoat component, control the viscosity to 10-25s, and use wet-on-wet construction; Drying treatment: first bake at 100℃ for 20 minutes, then increase the temperature to 145℃ and bake for 35 minutes.
[0078] During the spraying construction, the topcoat is sprayed once to a paint film thickness of 20 um.
[0079] During the spraying construction, the caliber of the spray gun is controlled at 3.5 mm.
[0080] It also includes gloss and matte adjustment, including using different colors of baked paint to correct the color or spraying varnish with different gloss levels. Example 12
[0081] A construction method for an alloy baked paint coating with an imitation crocodile pattern, comprising a primer construction and a topcoat construction; The primer construction includes the following: Prepare the substrate and pre-treat the surface; Dilution treatment: dilute according to the volume ratio of primer to primer thinner 1:0.7; Spraying construction: Control the viscosity to 10-25s, spray evenly with a 20um thick paint film, and after 10 minutes, enter the second topcoat process.
[0082] The topcoat application includes the following: Dilution: dilute the topcoat to topcoat thinner in a volume ratio of 1:1; Spraying construction: After spraying the primer, let it dry for 10 minutes, then spray the topcoat component, control the viscosity to 10-25s, and use wet-on-wet construction; Drying treatment: first bake at 120℃ for 10 minutes, then increase the temperature to 165℃ and bake for 25 minutes.
[0083] During the spraying construction, the topcoat is sprayed once to a paint film thickness of 30 um.
[0084] During the spraying construction, the caliber of the spray gun is controlled at 2.5 mm.
[0085] It also includes gloss and matte adjustment, including using different colors of baked paint to correct the color or spraying varnish with different gloss levels.
[0086] Comparative Example 1 This comparative example provides an alloy baked paint coating with an imitation crocodile pattern surface that is the same as Example 1, except that in the topcoat, high-second nitrocellulose is used instead of cellulose acetate butyrate. Since nitrocellulose cannot withstand temperatures above 100°C, it will lose gloss and the paint film will turn yellow after high-temperature baking for 5 minutes, and therefore cannot be used in this formulation system.
[0087] Comparative Example 2 This comparative example provides an alloy baked paint coating with crocodile-like grain surface which is the same as that in Example 1, except that the primer thinner and the topcoat thinner are different from those in Example 1, and the formulas thereof are both composed of the following weight parts: 25 parts of xylene, 10 parts of butanol, 15 parts of cyclohexanone, and 50 parts of butyl resin.
[0088] In this comparative example, when this thinner formula is used as a primer thinner, the solvent evaporates slowly and dries slowly, which affects the construction efficiency. After spraying the primer, it takes more than 1 hour of self-drying time before spraying the topcoat, which affects the actual needs of mass production. When used as a topcoat thinner, since the topcoat needs a strong and fast-drying thinner to form the crocodile leather effect of the concave and convex pattern formation plan, this formula dries slowly, and during construction, a certain part will not have concave and convex patterns formed, or the crocodile leather effect does not meet the requirements.
[0089] Comparative Example 3 This comparative example provides an alloy baked paint coating with crocodile-like texture as in Example 1, except that the primer thinner and the topcoat thinner are different from those in Example 1, and the formulas thereof are both composed of the following weight parts: 90% xylene and 10% cyclohexanone.
[0090] In this comparative example, when this thinner formula is used as a primer thinner, xylene and cyclohexanone are very slow to evaporate, affecting the construction efficiency. When used in spring and winter, the quality problem of "sag and edge oil" will appear. After spraying the primer, it takes more than half a day to spray the topcoat, affecting the timeliness of the topcoat construction. When used as a topcoat thinner, since the topcoat needs a strong and fast-drying thinner to form the crocodile leather effect of the concave and convex pattern formation plan, this formula dries very slowly, and no concave and convex patterns will be formed during construction.
[0091] Comparative Example 4 This comparative example provides an alloy baked paint coating with crocodile-like grain surface which is the same as that in Example 1, except that the primer thinner and the topcoat thinner are different from those in Example 1, and the formulas thereof are different from those in Example 1. The primer thinner / topcoat thinner are different, and the thinner formula includes the following components in parts by weight: 90% xylene and 10% butyl resin.
[0092] In this comparative example, when this thinner formula is used as a primer thinner, xylene is the main volatilizer and is very slow to evaporate. When used in spring and winter, the quality problem of "sag and edge oil" will occur. After spraying the primer, it takes more than half a day to spray the topcoat, which affects the timeliness of the topcoat construction. When used as a topcoat thinner, since the topcoat needs a strong and fast-drying thinner to form the crocodile leather effect of the concave and convex pattern formation plan, this formula has insufficient solubility and dries slowly. After construction, no concave and convex patterns will be formed, or only small concave and convex patterns will appear in a certain position.
[0093] Experimental effect test
[0094] Performance Testing By using the components of Example 1, Example 6, and Comparative Example 1, the preparation method of Example 7, and the construction process of Example 10, a paint surface was obtained for performance testing, and the results are shown in the following table: project Example 1 Example 6 Comparative Example 1 Required standard value Create a crocodile leather effect Finished product qualification rate 97% The operability of workers in spraying construction is poor, the qualified rate of finished products is reduced by 10%, and when using mechanical automatic spraying equipment, the difficulty of adjusting the "spray gun" increases by 30%. Finished product qualification rate 97% Compare with the color sample provided Appearance Finished product qualification rate 97% When the demand is for a large concave-convex texture effect, the qualified rate of the finished product will be reduced by 20%. When the demand is for a small concave-convex texture effect, the qualified rate of the finished product will also be reduced by 10%. The paint film turns burnt yellow during the high temperature baking process Compare with the color sample provided Adhesion 100% qualified 65% Adhesion test on paint film surface: Use a knife to make 100 cross grids of 1*1mm in advance, and stick a layer of 3M tape (600#) tightly on the cross grid surface, and then quickly remove the tape at a 90-degree angle. Standard: No signs of paint peeling or degradation. hardness H H F Hardness test: Use a Sanling brand pencil to test with a force of 1kg on the coating surface, then push the pencil away from the operator with a stroke of 20mm, repeat 4 times at adjacent positions, and there is no scratch on the surface. Resistant to hand sweat qualified qualified Very bad Immerse the parts in the following hand sweat solution for 48 hours (Hand sweat solution: weak acid solution provided by the manufacturer). Standard: No cracking, discoloration, staining or blistering is allowed. Resistant to alcohol clearness qualified qualified Difference Use a white soft rag (100% cotton), Alcohol Test: Soak the soft cloth in 75% alcohol and rub the test surface with a load of 1kg for 15 seconds. Standard: No signs of paint peeling or degradation. Acetone resistant qualified qualified Difference Use a white soft rag (100% cotton), soak it with acetone and rub the paint within 15 seconds (speed: return movement for about one second, force 500 g ± 50 g. Standard: No signs of paint peeling or degradation. Resistant to detergent qualified qualified Difference Use a white soft rag (100% cotton), soak it with 1:9 detergent and water, and then wipe the paint within 15 seconds (speed: about one second of back and forth motion, force 1000g ± 200g). Standard: No signs of paint peeling or degradation Salt spray resistant qualified qualified Very bad Put it in a salt spray test machine (5% sodium chloride solution) for 48 hours, and no rust or oxidation should occur. High temperature and humidity resistance qualified qualified Very bad Put it into a high temperature and high humidity machine (temperature 50℃, humidity 90%) and test it for 120 hours without any bubbles or mold. Create a crocodile leather effect contrast By adopting the components of Example 1 and Comparative Examples 2-4, the preparation method of Example 7 and the construction process of Example 10, the paint surface after spraying the diluted topcoat can be observed: the paint film formed in Example 1 has a concave-convex texture effect; the paint surface of Comparative Examples 2-4 does not have a concave-convex texture effect, or a concave-convex texture effect appears in some parts, and most of the paint film surface is still flat and smooth.
[0095] From the perspective of the finished paint film, the quality and performance of the overall formula are considered, and each performance is required to be balanced and qualified. It can be seen from the experimental data that the experimental test uses high-second nitrocellulose instead of cellulose acetate butyrate, which confirms that after nitrocellulose is added to the formula, it is not resistant to high temperatures above 100°C and is prone to aging and discoloration. However, the formula using matting powder combined with cellulose acetate butyrate will not change color when baked at 150°C, and will not dissolve and deteriorate at high temperature. It is confirmed that the matting powder combined with cellulose acetate butyrate in the present invention as the main raw materials of the topcoat is the best combination selected through experimental comparison, which is the guarantee of the performance quality of the crocodile leather effect.
[0096] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0097] In addition, it should be understood that although this specification is described in accordance with the implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should take the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art. It should be noted that the technical features not described in detail in the present invention can be realized by any prior art in the art.
Claims
1. A crocodile-like surface alloy baked paint, characterized in that: The invention comprises a primer and a topcoat, wherein the primer comprises the following components in parts by weight: 52-75 of a thermosetting acrylic resin, 21-39 of a phenylamino resin, 3-12 of a blocked isocyanate, 0.1-0.5 of a leveling agent, 2-8 of n-butanol, and 3-15 of a nano-color paste; The topcoat comprises the following components in parts by weight: 28-52 of secondary butyl resin, 4-12 of cellulose acetate butyrate, 0.5-2 of wax powder, 4-16 of matting powder, 7-15 of cyclohexanone, 15-42 of butanone and 3-15 of nano color paste.
2. The crocodile-grain-like alloy baked lacquer coating according to claim 1, characterized in that: The primer comprises the following components in parts by weight: 60-70 parts of thermosetting acrylic resin, 25-35 parts of phenylamino resin, 5-8 parts of blocked isocyanate, 0.15-0.3 parts of leveling agent, 3-5 parts of n-butanol and 7-10 parts of nano-color paste.
3. The crocodile-grain-like alloy baked lacquer coating according to claim 1, characterized in that: The topcoat comprises the following components in parts by weight: 35-41 parts of secondary butyl resin, 6-8 parts of cellulose acetate butyrate, 0.8-1.2 parts of wax powder, 7-11 parts of matting powder, 8-12 parts of cyclohexanone, 22-30 parts of butanone and 7-10 parts of nano color paste.
4. The crocodile-grain-like alloy baked lacquer coating according to any one of claims 1 to 3, characterized in that: The invention also comprises a primer diluent, which comprises the following components in parts by weight: 82-105 parts of ethyl acetate and 3-10 parts of cyclohexanone.
5. The crocodile-grain-like alloy baked lacquer coating according to claim 4, further comprising a topcoat thinner, wherein the topcoat thinner comprises the following components in parts by weight: 28-45 parts of sec-butyl ester, 8-18 parts of cyclohexanone, and 48-69 parts of acetone.
6. The crocodile-grain-like alloy baked lacquer coating according to claim 5, wherein the type of cellulose acetate butyrate comprises at least one of the following: CAB-381-0.5, CAB-381-2, CAB-381-20, and CAB-551-0.
01.
7. A method for preparing the crocodile-like alloy baked lacquer coating according to claim 6, characterized in that: Including the preparation of primer and topcoat; The preparation method of the primer comprises the following steps: Add thermosetting acrylic resin, phenylamino resin, blocked isocyanate and leveling agent in sequence, and gradually increase the speed to 800-1000RPM for dispersion for 10-18 minutes, and stop when the fineness / cleanliness is ≥6H / A; n-Butanol was added to adjust the viscosity; Add nano color paste to adjust the color; The preparation method of the topcoat comprises the following: Add sec-butyl ester, cellulose acetate butyrate, wax powder, matting powder, and cyclohexanone in sequence, and gradually increase the speed to 600-1000RPM for dispersion for 15-25 minutes, and stop when the fineness / cleanliness is ≥4H / A; Add butanone to adjust the viscosity; Add nano color paste to adjust the color.
8. The method for preparing the crocodile-like surface alloy baked lacquer coating according to claim 7, characterized in that: It also includes the preparation of primer thinner and the preparation of topcoat thinner; The preparation method of the primer thinner comprises the following steps: mixing ethyl ester and cyclohexanone respectively, and dispersing at a rotation speed of 500-800 RPM for 30-60 seconds; The preparation method of the topcoat thinner comprises the following steps: mixing sec-butyl ester, cyclohexanone and acetone respectively, and dispersing at a rotation speed of 500-800 RPM for 30-60 seconds.
9. A construction method of the crocodile-grain-like alloy baked lacquer coating according to claim 6, characterized in that: Including primer construction and topcoat construction; The primer construction includes the following: Prepare the substrate and pre-treat the surface; Dilution treatment: dilute according to the volume ratio of primer to primer thinner 1:0.5-0.7; Spraying construction: Control the viscosity to 10-25s, spray evenly with a 20-25um thick paint film, and after 10-20 minutes, enter the second topcoat process; The topcoat application includes the following: Dilution treatment: dilute according to the volume ratio of topcoat to topcoat thinner 1:0.7-1; Spraying construction: After spraying the primer, let it dry for 10-20 minutes, then spray the topcoat component, control the viscosity to 10-25s, and use wet-on-wet construction; Drying treatment: first bake at 100-120℃ for 10-20min, then increase the temperature to 145-165℃ and bake for 25-40 minutes.
10. The construction method of the crocodile-like surface alloy baked lacquer coating according to claim 9, characterized in that: During the spraying construction, the topcoat is sprayed once to a paint film thickness of 20-30 um.
Citation Information
Patent Citations
Crack lacquer for glass surface
CN103073976A
Alligator skin imitation paint and preparation method thereof
CN109401492A
Gloss oil with cool color-changing effect and preparation method thereof
CN111454631A
Furniture unsaturated resin paint diluent and preparation method thereof
CN117534978A
Performance evaluation system for scrubber and method of performance evaluation
KR1020210151448A