Polyester resin for low-light type low-temperature curing powder coating and preparation method of polyester resin
By designing a polyester resin with a soft main chain segment and a highly active end group structure, the problems of low-gloss and low-temperature curing of TGIC powder coatings are solved, achieving low gloss and high leveling properties, reducing energy consumption, and achieving coating film performance of Application requirements for TGIC powder coatings.
Patent Information
- Application Number
- CN202410999250.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-24
AI Technical Summary
When preparing low-gloss powder coatings, existing TGIC system powder coatings require a large amount of matting agents and have poor compatibility with polyester resins, resulting in coating film leveling defects, and high-temperature curing results in high energy consumption, making it impossible to achieve low-temperature curing. light effects.
Starting from the design of the chain segment structure and the end group structure cured with TGIC, we used terephthalic acid, butylmalonic acid, neopentyl glycol, tartaric acid, 2-hydroxyethylbenzimidazole, 3,3',4, 4'-benzophenone tetracarboxylic dianhydride and other raw materials are polymerized, and soft main chain segments and highly active end group structures are designed to achieve low-temperature curing and low-gloss coatings.
The low-temperature curing of polyester resin achieves excellent leveling properties of the coating film, with a gloss of 15-30%, and improves the boiling resistance of the coating film, meeting the conventional performance requirements of TGIC powder coatings.
Smart Images

Figure BDA0004961101390000021 
Figure BDA0004961101390000041 
Figure BDA0004961101390000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder coatings, and in particular relates to a polyester resin for low-gloss, low-temperature curing powder coatings and a preparation method thereof. Background Art
[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. Unlike ordinary solvent-based coatings and water-based coatings, its dispersion medium is not solvent and water, but air. It has the characteristics of no solvent pollution, 100% film formation and low energy consumption, and is widely used in indoor and outdoor coatings. Among them, outdoor weather-resistant powder coatings are mainly products of HAA system powder coatings and TGIC system powder coatings, compared with HAA system products. TGIC system powder coatings have the advantages of good weather resistance and thick coating without pinholes and are widely used. TGIC, also known as triglycidyl isocyanurate, has a molecular structure of a curing agent containing three active epoxy groups and has the best comprehensive performance. As decorative powder coatings are increasingly used, the demand for low-gloss powder coatings is also increasing. The commonly used method is to add a matting agent. The addition of a matting agent not only consumes a large amount of curing agent TGIC, but also because it is added by physical mixing, it has poor compatibility with polyester resin, which often causes defects in the leveling of the coating film. Therefore, the preparation of matting powder coatings requires a long time of grinding to ensure the yield rate, and the energy consumption is high. At the same time, with the increasing requirements for energy conservation and emission reduction and the expansion of the range of powder coating substrates, low-temperature curing powder coatings are an important direction for the development of the industry. How to achieve a gloss of 15-30% for TGIC powder coatings based on the design and synthesis of the polyester resin molecular structure, and achieve low-temperature curing, has important practical significance. Summary of the invention
[0003] In view of the above problems, the present invention starts with the design of the segment structure and the end group structure cured with TGIC, and develops a low-gloss, low-temperature curing polyester resin for powder coatings, which is mainly obtained by polymerization using terephthalic acid, butylmalonic acid, neopentyl glycol, dipropylene glycol, tartaric acid, 2-hydroxyethylbenzimidazole, 3,3',4,4'-benzophenonetetracarboxylic dianhydride and the like as raw materials. The polyester resin finally obtained has a relatively soft main chain segment structure, which reduces the softening point of the polyester resin and is beneficial to increasing the high-temperature fluidity of the polyester resin, thereby achieving better leveling properties of the coating film under low-temperature curing; and the chain extension of an appropriate amount of tartaric acid can improve the functionality of the polyester resin and enhance the water boiling resistance of the cured coating film; 2-hydroxyethylbenzimidazole and 3,3',4,4'-dibenzophenonetetracarboxylic dianhydride are used as special end-capping agents, which make the end groups of the polyester resin carry highly active imidazole curing groups and acid anhydride curing groups, which can not only achieve full curing of the epoxy groups in the TGIC curing agent at low temperature, but also the initial curing activity of the imidazole group is relatively high, so that it begins to cure with the epoxy groups in TGIC at 125°C, while the curing temperature of the acid anhydride generally needs to be above 140°C to start curing. The difference in curing temperature between the imidazole group and the acid anhydride brings about the difference in curing of the coating film surface. The gloss of the finally prepared coating film is relatively low, basically at 15-30%, achieving the matting effect under low-temperature curing, and other conventional properties meet the application requirements of TGIC powder coatings.
[0004] The present invention relates to a polyester resin for low-gloss low-temperature curing powder coating, which comprises raw materials composed of the following molar parts:
[0005]
[0006] The raw materials also include a catalyst and an antioxidant; the molar amount of the catalyst is 0.05-0.1% of the molar amount of terephthalic acid; the molar amount of the antioxidant is 0.03-0.05% of the molar amount of terephthalic acid.
[0007] Preferably, the catalyst is tetrabutyl titanate; and the antioxidant is antioxidant 1076.
[0008] The method for preparing a polyester resin for low-gloss low-temperature curing powder coating as described above comprises the following steps:
[0009] A. Add the formulated amount of neopentyl glycol, dipropylene glycol and catalyst into the reaction kettle, stir and heat to 125-130°C, and mix thoroughly;
[0010] B. Add the formulated amount of terephthalic acid and butylmalonic acid to the above mixture, gradually raise the temperature to 210-220° C. under nitrogen protection, and then carry out heat preservation esterification polymerization reaction;
[0011] C. Take samples to test the acid value of the reaction polymer. When the acid value is 38-45 mgKOH / g, add the formula amount of chain extender tartaric acid, then gradually raise the temperature to 225-230°C and continue the heat preservation polymerization reaction;
[0012] D. When the acid value of the polymer reaches 30-35 mgKOH / g, add the formulated amount of antioxidant, start the vacuum system, and conduct vacuum polycondensation reaction at 225-230°C to obtain a product with a higher degree of polymerization;
[0013] E. When the acid value of the polymer drops below 15-20 mgKOH / g, stop the vacuum system, cool down to 200-210°C, then add the formulated amount of 2-hydroxyethylbenzimidazole, and keep the temperature to carry out the benzimidazole grafting and capping reaction;
[0014] F. Take samples and test them by liquid chromatography. When the conversion of free 2-hydroxyethylbenzimidazole reaches more than 98%, it means that the grafting and end-capping of 2-hydroxybenzimidazole is completed. At this time, add 3,3',4,4'-benzophenonetetracarboxylic dianhydride and heat to 220-225℃ to carry out anhydride end-capping reaction;
[0015] G. Take samples for testing. When the acid value of the reactant reaches 19-24 mgKOH / g, stop the reaction, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.
[0016] Preferably, in step B, the temperature is gradually increased to 210-220°C at a heating rate of 12-15°C / h; in step C, the temperature is gradually increased to 225-230°C at a heating rate of 5-7°C / h; in step D, the vacuum degree is maintained at -0.095Mpa to -0.097Mpa; in step G, the polyester resin is cooled with a steel belt with condensed water.
[0017] The obtained product is light yellow transparent particles with an acid value of 19-24 mgKOH / g and a softening point of 103-112°C.
[0018] The present invention also relates to the use of the polyester resin for low-gloss, low-temperature curing powder coatings described above or a polyester resin for low-gloss, low-temperature curing powder coatings prepared by the preparation method in TGIC powder coatings.
[0019] The TGIC powder coating formula includes not only polyester resin and TGIC curing agent, but also titanium dioxide, barium sulfate, leveling agent, brightener, benzoin, etc. The coating preparation method is as follows: according to the powder coating formula, the materials are mixed, extruded, tableted, and crushed by a twin-screw extruder, and then the tablets are crushed and sieved to form a powder coating. The powder coating is sprayed on the tinplate substrate after surface treatment by an electrostatic spray gun, and the coating is obtained after curing.
[0020] Beneficial effects:
[0021] The present invention starts with the design of the segment structure and the end group structure for TGIC curing, and develops a low-light type low-temperature curing TGIC powder coating polyester resin, which is mainly obtained by polymerization using terephthalic acid, butylmalonic acid, neopentyl glycol, dipropylene glycol, tartaric acid, 2-hydroxyethylbenzimidazole, 3,3',4,4'-benzophenonetetracarboxylic dianhydride and the like as raw materials. The main chain segment structure of the polyester resin finally obtained is relatively soft, which reduces the softening point of the polyester resin and is beneficial to increase the high-temperature fluidity of the polyester resin, so as to achieve better leveling property of the coating film under low-temperature curing, and the chain extension of an appropriate amount of tartaric acid can improve the functionality of the polyester resin and enhance the boiling resistance of the cured coating film; 2-hydroxyethylbenzimidazole and 3,3',4,4'-dibenzophenonetetracarboxylic dianhydride are used as special end-capping agents, which make the end groups of the polyester resin carry highly active imidazole curing groups and acid anhydride curing groups, which can not only achieve full curing with the epoxy groups in the TGIC curing agent at low temperatures (such as 150°C), but also the initial curing activity of the imidazole group is relatively high, so that it starts to cure with the epoxy groups in TGIC at 125°C, while the curing temperature of the acid anhydride generally needs to be above 140°C to start curing. The difference in curing temperature between the imidazole group and the acid anhydride brings about the difference in curing of the coating surface, and the gloss of the finally prepared coating film is relatively low, basically at 15-30%, achieving the matting effect under low-temperature curing, and other conventional properties meet the application requirements of TGIC powder coatings.
[0022] The present invention has been described in detail above, but the above embodiments are only exemplary in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. DETAILED DESCRIPTION
[0023] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.
[0024] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.
[0025] Preparation Example 1
[0026] A low-gloss, low-temperature curing powder coating polyester resin comprises the following raw materials in molar parts:
[0027]
[0028] The catalyst is tetrabutyl titanate, and the molar amount of the catalyst is 0.1% of the molar amount of terephthalic acid;
[0029] The antioxidant is antioxidant 1076, and the molar amount of the antioxidant is 0.05% of the molar amount of terephthalic acid.
[0030] The preparation method of the low-gloss type low-temperature curing powder coating polyester resin comprises the following steps:
[0031] A. Add the formulated amount of neopentyl glycol, dipropylene glycol and catalyst into the reaction kettle, stir and heat to 130°C, and mix thoroughly;
[0032] B. Adding the formulated amount of terephthalic acid and butylmalonic acid to the above mixture, gradually heating the mixture to 220° C. at a heating rate of 15° C. / h under nitrogen protection, and then performing an esterification polymerization reaction at a heat preservation temperature;
[0033] C. Take samples to test the acid value of the reaction polymer. When the acid value is 38-45 mgKOH / g, add the formula amount of chain extender tartaric acid, then gradually increase the temperature to 230°C at a rate of 7°C / h, and continue the heat preservation polymerization reaction;
[0034] D. When the acid value of the polymer reaches 30-35 mgKOH / g, add the formulated amount of antioxidant, start the vacuum system, maintain the vacuum degree at -0.097 MPa, and conduct vacuum polycondensation reaction at 230°C to obtain a product with a higher degree of polymerization;
[0035] E. When the acid value of the polymer drops below 15-20 mgKOH / g, stop the vacuum system, cool down to 210°C, then add the formulated amount of 2-hydroxyethylbenzimidazole, and keep the temperature to carry out the benzimidazole grafting and capping reaction;
[0036] F. Take samples and test them by liquid chromatography. When the conversion of free 2-hydroxyethylbenzimidazole reaches more than 98%, it means that the grafting and end-capping of 2-hydroxybenzimidazole is completed. At this time, 3,3',4,4'-benzophenonetetracarboxylic dianhydride is added and the temperature is raised to 225°C for anhydride end-capping reaction.
[0037] G. Take samples for testing. When the acid value of the reactant reaches 19-24 mgKOH / g, stop the reaction, discharge the material while hot, and cool the polyester resin with a steel belt with condensed water. Then, crush and granulate the polyester resin to obtain the polyester resin.
[0038] The obtained product is light yellow transparent particles with an acid value of 21 mgKOH / g and a softening point of 106°C.
[0039] Preparation Example 2
[0040] A low-gloss, low-temperature curing powder coating polyester resin comprises the following raw materials in molar parts:
[0041]
[0042] The catalyst is tetrabutyl titanate, and the amount of the catalyst is 0.1% of the molar amount of terephthalic acid;
[0043] The antioxidant is antioxidant 1076, and the amount of the antioxidant is 0.05% of the molar amount of terephthalic acid.
[0044] The preparation method is the same as Example 1.
[0045] The obtained product is light yellow transparent particles with an acid value of 24 mgKOH / g and a softening point of 109°C.
[0046] Preparation Example 3
[0047] A low-gloss, low-temperature curing powder coating polyester resin comprises the following raw materials in molar parts:
[0048]
[0049]
[0050] The catalyst is tetrabutyl titanate, and the amount of the catalyst is 0.1% of the molar amount of terephthalic acid;
[0051] The antioxidant is antioxidant 1076, and the amount of the antioxidant is 0.03% of the molar amount of terephthalic acid.
[0052] The preparation method is the same as Example 1.
[0053] The obtained product is light yellow transparent particles with an acid value of 23 mgKOH / g and a softening point of 111°C.
[0054] Preparation Example 4
[0055] A low-gloss, low-temperature curing powder coating polyester resin comprises the following raw materials in molar parts:
[0056]
[0057] The catalyst is tetrabutyl titanate, and the amount of the catalyst is 0.08% of the molar amount of terephthalic acid;
[0058] The antioxidant is antioxidant 1076, and the amount of the antioxidant is 0.05% of the molar amount of terephthalic acid.
[0059] The preparation method is the same as Example 1.
[0060] The obtained product is light yellow transparent particles with an acid value of 24 mgKOH / g and a softening point of 105°C.
[0061] Comparative Preparation Example 1
[0062] Commercially available TGIC polyester resin, acid value 34 mgKOH / g, softening point 115°C, model GH-2240; Zhejiang Guanghua Technology Co., Ltd.
[0063] Comparative Preparation Example 2
[0064] The polyester resin is the same as that in Comparative Example 1, except that the curing conditions are changed to 200°C / 15min.
[0065] Examples 1-4 and Comparative Examples 1 and 2 (polyester resins are obtained by the above corresponding preparation examples or comparative preparation examples)
[0066] According to the TGIC powder coating formula, the formula in parts by weight is as follows:
[0067]
[0068] Preparation of coating: Mix all materials according to the formula of TGIC powder coating, extrude, tablet and crush with a twin-screw extruder, and then crush and sieve the tablets (160-180 mesh) to make powder coating. The powder coating is sprayed on the surface treated tinplate substrate with an electrostatic spray gun, and cured at 150℃ / 15min to obtain the coating.
[0069] Performance comparison
[0070] The coating index test is based on: GB / T 21776-2008 "Testing Standard Guide for Powder Coatings and Their Coatings". The leveling performance adopts the PCI leveling grade, 1-10, the larger the number, the better the leveling.
[0071] The polyester resins prepared in the above examples and comparative examples were used to prepare coatings according to the coating formulations provided by the present invention, and the coating properties were tested as shown in Table 1 below.
[0072] Table 1 Coating properties of powder coatings
[0073]
[0074]
[0075] As can be seen from Table 1, the product of the present invention has high terminal activity of polyester resin and obvious curing difference by virtue of special raw material formula and process preparation technology. The polyester resin prepared by the product can be fully cured at 150°C / 15min for TGIC powder coating. The cured coating is not only flat and smooth, but also has excellent impact resistance and high leveling grade, reaching grade 6. Effective matting is achieved under the curing difference of terminal imidazole and acid anhydride, the gloss of the coating is basically between 15-30%, and the boiling water resistance effect is also outstanding.
[0076] The commercially available polyester resin product of Comparative Example 1 cannot be fully cured at 150°C / 15min, resulting in poor appearance, impact resistance and flow level of the coating film; Comparative Example 2 adopts the method of increasing the curing conditions to 200°C / 15min, under which sufficient curing is achieved, the leveling grade is high, and the impact resistance and water boiling performance meet the requirements, but the matte effect cannot be achieved, and the gloss is above 94%.
[0077] It can be seen that the polyester resin obtained by the scheme of the present invention can be fully cured at low temperature for TGIC powder coating, and the cured coating film is not only flat and smooth, but also has excellent impact resistance, and also has a high leveling grade and excellent boiling water resistance. The coating film has low gloss, and the matte effect under low temperature curing is achieved. Other conventional properties meet the application requirements of TGIC powder coating.
[0078] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and essence of the claims of the present invention; and these modifications or replacements are still within the scope defined by the claims of the present invention.
Claims
1. A polyester resin for low-gloss low-temperature curing powder coating, characterized in that: The raw materials comprising the following molar compositions: The raw materials also include a catalyst and an antioxidant; the amount of the catalyst is 0.05-0.1% of the molar amount of terephthalic acid; the amount of the antioxidant is 0.03-0.05% of the molar amount of terephthalic acid.
2. A polyester resin for low-gloss, low-temperature curing powder coating as claimed in claim 1, further characterized in that the catalyst is tetrabutyl titanate.
3. A polyester resin for low-gloss, low-temperature curing powder coating as claimed in claim 1, further characterized in that the antioxidant is antioxidant 1076.
4. A method for preparing a polyester resin for low-gloss, low-temperature curing powder coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: A. Add the formulated amount of neopentyl glycol, dipropylene glycol and catalyst into the reaction kettle, stir and heat to 125-130°C, and mix thoroughly; B. Add the formulated amount of terephthalic acid and butylmalonic acid to the above mixture, gradually raise the temperature to 210-220° C. under nitrogen protection, and then carry out heat preservation esterification polymerization reaction; C. Take samples to test the acid value of the reaction polymer. When the acid value is 38-45 mgKOH / g, add the formula amount of chain extender tartaric acid, then gradually raise the temperature to 225-230°C and continue the heat preservation polymerization reaction; D. When the acid value of the polymer reaches 30-35 mgKOH / g, add the formulated amount of antioxidant, start the vacuum system, and conduct vacuum polycondensation reaction at 225-230°C to obtain a product with a higher degree of polymerization; E. When the acid value of the polymer drops below 15-20 mgKOH / g, stop the vacuum system, cool down to 200-210°C, then add the formulated amount of 2-hydroxyethylbenzimidazole, and keep the temperature to carry out the benzimidazole grafting and capping reaction; F. Take samples and test them by liquid chromatography. When the conversion of free 2-hydroxyethylbenzimidazole reaches more than 98%, it means that the grafting and end-capping of 2-hydroxybenzimidazole is completed. At this time, add 3,3',4,4'-benzophenonetetracarboxylic dianhydride and heat to 220-225℃ to carry out anhydride end-capping reaction; G. Take samples for testing. When the acid value of the reactant reaches 19-24 mgKOH / g, stop the reaction, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.
5. The method for preparing a polyester resin for a low-gloss, low-temperature curing powder coating according to claim 4, further characterized in that in step B, the temperature is gradually increased to 210-220°C at a heating rate of 12-15°C / h.
6. The method for preparing a polyester resin for a low-gloss, low-temperature curing powder coating according to claim 4, further characterized in that in step C, the temperature is gradually increased to 225-230°C at a heating rate of 5-7°C / h.
7. The method for preparing a polyester resin for a low-gloss, low-temperature curing powder coating according to claim 4, further characterized in that in step D, the vacuum degree is maintained at -0.095 MPa to -0.097 MPa.
8. The method for preparing a polyester resin for a low-gloss, low-temperature curing powder coating according to claim 4, further characterized in that in step G, a steel belt with condensed water is used to cool the polyester resin.
9. Use of the polyester resin for low-gloss, low-temperature curing powder coatings according to any one of claims 1 to 3 or the polyester resin for low-gloss, low-temperature curing powder coatings prepared by the preparation method according to any one of claims 4 to 8 in TGIC powder coatings.
Citation Information
Patent Citations
Preparation method of indoor flatting powder paint
CN102850913A
Polyester resin with high hardness and high storage stability for 60 / 40 mixed powder and preparation method thereof
CN111333827A
50 / 50 fast-curing polyester resin for low-gloss powder coating and preparation method of 50 / 50 fast-curing polyester resin
CN115521447A
Polyester resin for powder coating as well as preparation method and application of polyester resin
CN115626978A