Antibacterial nano-cellulose-based waterborne polyurethane resin coating film and preparation method thereof

By using materials such as copper ion-modified nanocellulose and polysiloxane oligomers to prepare antibacterial water-based polyurethane resin coatings, it solves the problem of insufficient performance of traditional water-based polyurethane and achieves efficient multi-functional improvements and biomass materials high-value utilization.

CN118725713APending Publication Date: 2024-10-01广东睿鹏材料科学有限公司

Patent Information

Application Number
CN202410848094.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional water-based polyurethane has insufficient water resistance and mechanical properties, and has a single function, making it difficult to meet the needs of sustainable development and multi-functionality.

Method used

Using copper ion modified nanocellulose as raw material, combined with aromatic isocyanate, polysiloxane oligomer and chain extender, an antibacterial water-based polyurethane resin coating film is prepared through a specific preparation method to form a three-dimensional network structure to improve performance.

Benefits of technology

The antibacterial performance, water resistance and scratch resistance of water-based polyurethane are significantly improved, meeting the need for multifunctionality and realizing high-value utilization of biomass materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725713A_ABST
    Figure CN118725713A_ABST
Patent Text Reader

Abstract

The invention relates to an antibacterial nano-cellulose-based waterborne polyurethane resin coating film and a preparation method thereof, and belongs to the technical field of intersection of high value-added utilization of biomass resources and polyurethane resin coating films. The antibacterial nanocellulose-based waterborne polyurethane resin coating film is prepared from the following components in parts by weight: 100 parts of copper ion modified nanocellulose, 60 to 80 parts of aromatic isocyanate, 20 to 40 parts of siloxane, 10 to 30 parts of chain extender, 30 to 60 parts of deionized water and 10 to 20 parts of acetone. The preparation method of the copper ion modified nanocellulose comprises the following steps: acidifying nanocellulose, filtering, washing, reacting with a copper ion solution, filtering, washing, and drying to obtain the copper ion modified nanocellulose. The modified nanocellulose containing copper ions is introduced in the synthesis route, so that the product is endowed with antibacterial performance. The polysiloxane oligomer is also added, so that the molecular structure of the product forms a three-dimensional network structure, and the scratch resistance and water resistance of the product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the cross-technical field of high value-added utilization of biomass resources and polyurethane resin coating, in particular to an antibacterial waterborne polyurethane resin coating using copper ion-modified nanocellulose as a raw material and a preparation method thereof. Background Art

[0002] Polyurethane is a type of polymer containing carbamate units on the main chain. It has both the elasticity of rubber and the excellent processing properties of plastic. It is widely used in many fields such as automobiles, furniture, construction and footwear. However, the traditional polyurethane preparation formula relies on a large amount of petroleum derivatives, which does not meet the requirements of sustainable development. Waterborne polyurethane is an environmentally friendly polyurethane with an environmentally friendly production process, but the water resistance and mechanical properties of the currently prepared waterborne polyurethane need to be further improved. In addition, the relatively single functionality also limits its development. Therefore, it is necessary to develop waterborne polyurethane resins with good mechanical properties and multifunctionality. Summary of the invention

[0003] The purpose of the present invention is to provide an antibacterial nano-cellulose-based waterborne polyurethane resin coating and a preparation method thereof, in particular to provide an antibacterial waterborne polyurethane resin coating made of nano-cellulose raw materials modified with copper ions.

[0004] The specific technical solutions are as follows:

[0005] An antibacterial nanocellulose-based waterborne polyurethane resin coating film, wherein the raw materials of the hydrophobic polyurethane resin coating film are composed of 80 to 100 parts of copper ion-modified nanocellulose, 60 to 80 parts of aromatic isocyanate, 20 to 40 parts of polysiloxane oligomer, 10 to 30 parts of chain extender, 30 to 60 parts of deionized water, and 10 to 20 parts of acetone in parts by weight;

[0006] The preparation method of the copper ion modified nanocellulose comprises the following steps:

[0007] S1: mixing commercially available nanocellulose and 60 wt % sulfuric acid in a weight ratio of 1: (0.1-0.2), reacting at 40-60° C. for 1-2 hours, filtering and washing with deionized water for 3-5 times to obtain acidified nanocellulose;

[0008] S2: Evenly mix the acidified nanocellulose and the divalent copper ion solution in a weight ratio of 1:(0.4-0.5), stir at 20-30° C. for 1-2 hours, filter, wash with deionized water 3-5 times, and dry at 20-35° C. for 0.5-1 hour to obtain the copper ion modified nanocellulose.

[0009] In some embodiments, the copper ion solution in S2 is selected from one or more of copper chloride solution, copper sulfate solution, copper nitrate solution, and copper acetate solution; the concentration of the copper ion solution is 5wt% to 10wt%.

[0010] In some embodiments, the aromatic isocyanate is selected from one or more of phenylene diisocyanate, toluene diisocyanate, o-phenylene diisocyanate, p-phenylene diisocyanate, and naphthalene diisocyanate.

[0011] In some embodiments, the siloxane is selected from one or more of hexamethyldisiloxane, hexaethyldisiloxane, pentamethyldisiloxane, octamethylcyclotetrasiloxane, and polydimethylsiloxane with a viscosity of 10 Pa.s to 1000 Pa.s.

[0012] In some embodiments, the chain extender is selected from one or more of polyvinyl alcohol, polyoxypropylene alcohol, polyoxyethylene alcohol, polybutyl methacrylate, polyethylene cyclohexanedicarboxylate, polybutylene glycol, and polycaprolactone.

[0013] The present invention also provides a method for preparing the above antibacterial nanocellulose-based waterborne polyurethane resin coating film, and the preparation method comprises the following steps:

[0014] S3: In a multifunctional reactor, adding modified nanocellulose and polysiloxane oligomer according to weight, stirring at a temperature of 20 to 40° C. and a speed of 2000 to 3000 rpm for 1 to 2 hours;

[0015] S4: In a multifunctional reaction kettle, add aromatic isocyanate according to weight, raise the temperature to 60-80° C., and continue stirring for 1-2 hours to obtain a prepolymer;

[0016] S5: adding acetone and chain extender in parts by weight, raising the temperature to 70-90° C., and reacting for 1-3 hours under stirring;

[0017] S6: Cooling to 20-30°C, adding deionized water by weight for emulsification, maintaining under 10-30 kPa for 20-60 minutes for reduced pressure rotary evaporation concentration to obtain an antibacterial nano-cellulose-based waterborne polyurethane emulsion; pouring the emulsion into a polyethylene mold and drying at 50-80°C for 12-24 hours to obtain an antibacterial nano-cellulose-based waterborne polyurethane resin coating.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] (1) High-value utilization of biomass material nanocellulose, using it to carry antibacterial copper ions, so that the prepared products have antibacterial properties;

[0020] (2) Polysiloxane oligomers are added to the formula, which enables the molecular structure of the product to form a three-dimensional network structure, thereby improving the mechanical properties and water resistance of the product;

[0021] (3) The active hydroxyl groups on the modified nanocellulose molecular chains and polysiloxane oligomer molecular chains promoted the reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 : The microstructure of the copper ion modified nanocellulose prepared in Example 1;

[0023] Figure 2 : The microstructure of the copper ion modified nanocellulose prepared in Example 2;

[0024] Figure 3 : The microstructure of copper ion modified nanocellulose prepared in Example 3. DETAILED DESCRIPTION

[0025] The following will combine the technical process steps, specific implementation conditions and materials in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] In a multifunctional reactor, nanocellulose was mixed with 60wt% sulfuric acid in a weight ratio of 1:0.1, reacted at 50°C for 1 hour, filtered and washed 3 times with deionized water to obtain acidified nanocellulose. Acidified nanocellulose was mixed with 10wt% copper sulfate solution in a weight ratio of 1:0.4, stirred at 30°C for 1 hour, filtered, washed 3 times with deionized water, and dried at 30°C for 0.5 hour to obtain copper ion modified nanocellulose for use. Scanning electron microscopy characterization of the microstructure of the prepared copper ion modified nanocellulose is shown in Figure 1 a, the diameter of nanocellulose is about 27nm, and the length is about 648nm; the microstructure of nanocellulose modified by copper ion is shown in Figure 1. Figure 1 b and Figure 1 c, it can be found that copper ions can adhere well to the surface of nanocellulose.

[0028] Example 2

[0029] In a multifunctional reactor, nanocellulose was mixed with 60wt% sulfuric acid in a weight ratio of 1:0.1, reacted at 50°C for 1 hour, filtered and washed 3 times with deionized water to obtain acidified nanocellulose. Acidified nanocellulose was mixed with 10wt% copper chloride solution in a weight ratio of 1:0.4, stirred at 30°C for 1 hour, filtered, washed 3 times with deionized water, and dried at 30°C for 0.5 hour to obtain copper ion modified nanocellulose for use. Scanning electron microscopy characterization of the microstructure of the prepared copper ion modified nanocellulose is shown in Figure 2 a, the diameter of nanocellulose is about 17nm, and the length is about 385nm; the microstructure of nanocellulose modified by copper ion is shown in Figure 1. Figure 2 b and Figure 2 c, it can be found that copper ions can adhere well to the surface of nanocellulose.

[0030] Example 3

[0031] In a multifunctional reactor, commercially available nanocellulose was mixed with 60wt% sulfuric acid in a weight ratio of 1:0.2, reacted at 50°C for 1 hour, filtered and washed 3 times with deionized water to obtain acidified nanocellulose. Acidified nanocellulose was mixed with 10wt% copper chloride solution in a weight ratio of 1:0.5, stirred at 30°C for 2 hours, filtered, washed 3 times with deionized water, and dried at 35°C for 1 hour to obtain copper ion-modified nanocellulose for use. Scanning electron microscopy characterization of the microstructure of the prepared copper ion-modified nanocellulose is shown in Figure 3 a, the diameter of nanocellulose is about 22nm, and the length is about 433nm; the microstructure of nanocellulose modified by copper ion is shown in Figure 1. Figure 3 b and Figure 3 c. It can be found that copper ions can adhere to the surface of nanocellulose well, and the copper ion content is higher than that of the modified nanocellulose surface prepared in Example 1.

[0032] Example 4

[0033] In a multifunctional reactor, add modified nanocellulose and polysiloxane oligomers by weight, and stir at 2000 rpm for 1 hour at a temperature of 20°C. Add aromatic isocyanate by weight, raise the temperature to 60°C, and continue stirring for 1 hour to obtain a prepolymer. Add acetone and chain extender by weight, raise the temperature to 75°C, and react for 2 hours under stirring. Cool to 25°C, add deionized water by weight for emulsification, maintain at 20kPa for 40 minutes for reduced pressure rotary evaporation and concentration to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. Pour the resin emulsion into a polyethylene mold and dry it at 60°C for 15 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0034] Table 1 Raw material ratio of the synthetic polyurethane resin coating of Example 4

[0035] Copper ion modified nanocellulose 100 copies Toluene diisocyanate 60 servings Hexamethyldisiloxane 20 servings Polyvinyl alcohol 10 servings Deionized water 30 servings acetone 10 servings

[0036] The copper ion-modified nanocellulose in Table 1 is the copper ion-modified nanocellulose prepared by the method of Example 1.

[0037] According to QT / T 4341-2012 "Antibacterial polyurethane synthetic leather - Antibacterial performance test method and antibacterial effect", the prepared polyurethane resin coating was tested for antibacterial properties, and the antibacterial rate was calculated according to the following formula:

[0038]

[0039] R is the antibacterial rate; B is the average number of bacteria recovered from the blank sample, in (CFU / piece); A is the average number of bacteria recovered from the antibacterial test sample, in (CFU / piece)

[0040] The inhibition rates of the polyurethane resin coating prepared in Example 4 against Staphylococcus aureus and Escherichia coli were 94.6% and 91.2%, respectively.

[0041] Cut the sample film into 2cm×2cm squares and weigh them m 0, Soak in water for 72 hours, take out the film and absorb the surface moisture, weigh the mass as m1, and calculate the water absorption (S). The water absorption is calculated according to the following formula:

[0042]

[0043] The water absorption rate of the polyurethane resin coating film prepared in Example 4 is 22%.

[0044] The scratch resistance of the polyurethane resin coating prepared in Example 4 was tested in accordance with GB / T 31591-2015 "Determination of the scratch resistance of paints and varnishes", and the test result was 1400g.

[0045] Example 5

[0046] In a multifunctional reactor, modified nanocellulose and polysiloxane oligomers are added by weight, and stirred at a temperature of 30°C at a rate of 2000rpm for 1 hour. Aromatic isocyanate is added by weight, the temperature is raised to 70°C, and stirring is continued for 1 hour to obtain a prepolymer. Acetone and chain extender are added by weight, the temperature is raised to 80°C, and the reaction is carried out for 2 hours under stirring. The temperature is lowered to 25°C, deionized water is added by weight for emulsification, and vacuum rotary evaporation is maintained at 20kPa for 40 minutes to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. The resin emulsion is poured into a polyethylene mold and dried at 60°C for 18 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0047] Table 2 Raw material ratio of the synthetic polyurethane resin coating of Example 5

[0048] Copper ion modified nanocellulose 100 copies Toluene diisocyanate 70 servings 50Pa.s Polydimethylsiloxane 25 servings Polyoxyethylene alcohol 15 servings Deionized water 32 servings acetone 13 servings

[0049] The copper ion-modified nanocellulose in Table 2 is the copper ion-modified nanocellulose prepared by the method of Example 2.

[0050] The inhibition rates of the polyurethane resin coating prepared in Example 5 against Staphylococcus aureus and Escherichia coli were 91.0% and 92.2%, respectively.

[0051] The water absorption rate of the polyurethane resin coating film prepared in Example 5 is 17%.

[0052] The scratch resistance of the polyurethane resin coating prepared in Example 5 was tested in accordance with GB / T 31591-2015 "Determination of the scratch resistance of paints and varnishes", and the test result was 1500g.

[0053] Example 6

[0054] In a multifunctional reactor, modified nanocellulose and polysiloxane oligomers are added by weight, and stirred at a temperature of 30°C at a rate of 2000rpm for 1 hour. Aromatic isocyanate is added by weight, the temperature is raised to 80°C, and stirring is continued for 1 hour to obtain a prepolymer. Acetone and chain extender are added by weight, the temperature is maintained at 80°C, and the reaction is carried out for 3 hours under stirring. The temperature is lowered to 25°C, deionized water is added by weight for emulsification, and vacuum rotary evaporation is performed for 40 minutes at 20kPa to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. The resin emulsion is poured into a polyethylene mold and dried at 60°C for 20 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0055] Table 3 Raw material ratio of the synthetic polyurethane resin coating of Example 6

[0056] Copper ion modified nanocellulose 100 copies o-Phenyl diisocyanate 71 copies Octamethylcyclotetrasiloxane 30 servings Polyvinyl alcohol 15 servings Deionized water 40 servings acetone 15 servings

[0057] The copper ion-modified nanocellulose in Table 3 is the copper ion-modified nanocellulose prepared by the method of Example 3.

[0058] The inhibition rates of the polyurethane resin coating prepared in Example 6 against Staphylococcus aureus and Escherichia coli were 96.3% and 93.2%, respectively.

[0059] The water absorption rate of the polyurethane resin coating film prepared in Example 6 is 12%.

[0060] The scratch resistance of the polyurethane resin coating prepared in Example 6 was tested in accordance with GB / T 31591-2015 "Determination of the scratch resistance of paints and varnishes", and the test result was 1600g.

[0061] Example 7

[0062] In a multifunctional reactor, modified nanocellulose and polysiloxane oligomers are added by weight, and stirred at a temperature of 30°C at a rate of 2000rpm for 1 hour. Aromatic isocyanate is added by weight, the temperature is raised to 75°C, and stirring is continued for 1 hour to obtain a prepolymer. Acetone and chain extender are added by weight, the temperature is raised to 85°C, and the reaction is carried out for 2 hours under stirring. The temperature is lowered to 25°C, deionized water is added by weight for emulsification, and vacuum rotary evaporation is performed for 40 minutes at 20kPa to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. The resin emulsion is poured into a polyethylene mold and dried at 60°C for 20 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0063] Table 4 Raw material ratio of the synthetic polyurethane resin coating of Example 7

[0064] Copper ion modified nanocellulose 100 copies P-phenylene diisocyanate 60 servings Octamethylcyclotetrasiloxane 40 servings Polybutyl methacrylate 20 servings Deionized water 40 servings acetone 15 servings

[0065] The copper ion-modified nanocellulose in Table 4 is the copper ion-modified nanocellulose prepared by the method of Example 3.

[0066] The inhibition rates of the polyurethane resin coating prepared in Example 7 against Staphylococcus aureus and Escherichia coli were 94.6% and 90.6%, respectively.

[0067] The water absorption of the polyurethane resin coating film prepared in Example 7 is 16%.

[0068] The scratch resistance of the polyurethane resin coating prepared in Example 7 was tested in accordance with GB / T 31591-2015 "Determination of the scratch resistance of paints and varnishes", and the test result was 1500g.

[0069] Comparative Example 1

[0070] In a multifunctional reactor, commercially available unmodified nanocellulose and polysiloxane oligomers are added by weight, and stirred at a temperature of 30°C at a rate of 2000rpm for 2 hours. Aromatic isocyanate is added by weight, the temperature is raised to 60°C, and stirring is continued for 1 hour to obtain a prepolymer. Acetone and chain extender are added by weight, the temperature is raised to 70°C, and the reaction is carried out for 3 hours under stirring. The temperature is lowered to 25°C, deionized water is added by weight for emulsification, and vacuum rotary evaporation is maintained at 20kPa for 40 minutes to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. The resin emulsion is poured into a polyethylene mold and dried at 60°C for 20 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0071] Table 5 Raw material ratio of synthetic polyurethane resin coating film in comparative example 1

[0072] Commercially available unmodified nanocellulose 100 copies o-Phenyl diisocyanate 71 copies Octamethylcyclotetrasiloxane 30 servings Polyvinyl alcohol 15 servings Deionized water 40 servings acetone 15 servings

[0073] The inhibition rates of the polyurethane resin coating prepared in Comparative Example 1 on Staphylococcus aureus and Escherichia coli were 11.6% and 5.3%, respectively.

[0074] The water absorption rate of the polyurethane resin coating film prepared in Comparative Example 1 is 18%.

[0075] The scratch resistance of the polyurethane resin coating prepared in Comparative Example 1 was tested in accordance with GB / T 31591-2015 “Determination of Scratch Resistance of Paints and Varnishes”, and the test result was 1400g.

[0076] Comparative Example 2

[0077] In a multifunctional reactor, add modified nanocellulose and aromatic isocyanate by weight, heat to 70°C, and continue stirring for 1 hour to obtain a prepolymer. Add acetone and chain extender by weight, heat to 80°C, and react for 3 hours under stirring. Cool to 25°C, add deionized water by weight for emulsification, maintain under 20kPa for 40 minutes for reduced pressure rotary evaporation and concentration to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. Pour the resin emulsion into a polyethylene mold and dry it at 60°C for 20 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0078] Table 6 Raw material ratio of synthetic polyurethane resin coating in comparative example 2

[0079] Copper ion modified nanocellulose 100 copies o-Phenyl diisocyanate 71 copies Polyvinyl alcohol 15 servings Deionized water 40 servings acetone 15 servings

[0080] The copper ion-modified nanocellulose in Table 6 is the copper ion-modified nanocellulose prepared by the method of Example 3.

[0081] The inhibition rates of the polyurethane resin coating prepared in Comparative Example 2 on Staphylococcus aureus and Escherichia coli were 93.3% and 91.2%, respectively.

[0082] The water absorption rate of the polyurethane resin coating film prepared in Comparative Example 2 is 52%.

[0083] The scratch resistance of the polyurethane resin coating prepared in Comparative Example 2 was tested in accordance with GB / T 31591-2015 "Determination of Scratch Resistance of Paints and Varnishes", and the test result was 600g.

[0084] Comparative Example 3

[0085] In a multifunctional reactor, modified nanocellulose and polysiloxane oligomers are added by weight, and stirred at a temperature of 30°C at a rate of 2000rpm for 1 hour. Aromatic isocyanate is added by weight, the temperature is raised to 70°C, and stirring is continued for 1 hour to obtain a prepolymer. Acetone and chain extender are added by weight, the temperature is raised to 80°C, and the reaction is carried out for 3 hours under stirring. The temperature is lowered to 25°C, deionized water is added by weight for emulsification, and vacuum rotary evaporation is maintained at 20kPa for 40 minutes to obtain an antibacterial nanocellulose-based waterborne polyurethane resin emulsion. The resin emulsion is poured into a polyethylene mold and dried at 60°C for 20 hours to obtain an antibacterial nanocellulose-based waterborne polyurethane resin coating.

[0086] Table 7 Raw material ratio of synthetic polyurethane resin coating film in comparative example 3

[0087] Copper ion modified nanocellulose 100 copies o-Phenyl diisocyanate 71 copies Octamethylcyclotetrasiloxane 5 servings Polyvinyl alcohol 15 servings Deionized water 40 servings acetone 15 servings

[0088] The copper ion-modified nanocellulose in Table 7 is the copper ion-modified nanocellulose prepared by the method of Example 3.

[0089] The inhibition rates of the polyurethane resin coating prepared in Comparative Example 3 on Staphylococcus aureus and Escherichia coli were 94.7% and 93.6%, respectively.

[0090] The water absorption rate of the polyurethane resin coating film prepared in Comparative Example 3 is 45%.

[0091] The scratch resistance of the polyurethane resin coating prepared in Comparative Example 3 was tested in accordance with GB / T 31591-2015 "Determination of Scratch Resistance of Paints and Varnishes", and the test result was 700g.

[0092] The present invention adds copper ion modified nanocellulose to the synthesis of waterborne polyurethane, and by comparing Examples 4 to 7 and Comparative Example 1, it is shown that adding copper ion modified nanocellulose in the process of preparing waterborne polyurethane can significantly improve the antibacterial properties of waterborne polyurethane. By comparing Examples 4 to 7 and Comparative Examples 2 to 3, it is shown that the amount of polysiloxane oligomer added in the process of preparing waterborne polyurethane has a significant effect on waterborne polyurethane, and increasing the amount of polysiloxane oligomer added can improve the scratch resistance and water resistance of waterborne polyurethane. When the amount of polysiloxane oligomer added is 30 parts relative to 100 parts of copper ion modified nanocellulose, waterborne polyurethane has the best scratch resistance and water resistance.

[0093] Technical personnel should note that although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept will be included in the scope of protection of this patent.

Claims

1. An antibacterial nanocellulose-based waterborne polyurethane resin coating film, characterized in that: The raw material composition of the hydrophobic polyurethane resin coating is as follows: 80-100 parts of copper ion modified nanocellulose, 60-80 parts of aromatic isocyanate, 20-40 parts of siloxane, 10-30 parts of chain extender, 30-60 parts of deionized water, and 10-20 parts of acetone by weight. The preparation method of the copper ion modified nanocellulose comprises the following steps: S1: mixing nanocellulose and 60 wt % sulfuric acid in a weight ratio of 1: (0.1-0.2), reacting at 40-60° C. for 1-2 hours, filtering and washing with deionized water for 3-5 times to obtain acidified nanocellulose; S2: Evenly mix the acidified nanocellulose and the divalent copper ion solution in a weight ratio of 1:(0.4-0.5), stir at 20-30° C. for 1-2 hours, filter, wash with deionized water 3-5 times, and dry at 20-35° C. for 0.5-1 hour to obtain the copper ion modified nanocellulose.

2. The antibacterial nanocellulose-based waterborne polyurethane resin coating according to claim 1, characterized in that: The copper ion solution in S2 is selected from one or more of copper chloride solution, copper sulfate solution, copper nitrate solution and copper acetate solution; the concentration of the copper ion solution is 5wt% to 10wt%.

3. The antibacterial nanocellulose-based waterborne polyurethane resin coating according to claim 1, characterized in that: The aromatic isocyanate is selected from one or more of phenylene diisocyanate, toluene diisocyanate, o-phenylene diisocyanate, p-phenylene diisocyanate and naphthalene diisocyanate.

4. The antibacterial nanocellulose-based waterborne polyurethane resin coating film according to claim 1, characterized in that: The siloxane is selected from one or more of hexamethyldisiloxane, hexaethyldisiloxane, pentamethyldisiloxane, octamethylcyclotetrasiloxane, and polydimethylsiloxane with a viscosity of 10 Pa.s to 1000 Pa.s.

5. The antibacterial nanocellulose-based waterborne polyurethane resin coating film according to claim 1, characterized in that: The chain extender is selected from one or more of polyvinyl alcohol, polyoxypropylene alcohol, polyoxyethylene alcohol, polybutyl methacrylate, polyethylene cyclohexanedicarboxylate, polybutylene glycol, and polycaprolactone.

6. The method for preparing the antibacterial nanocellulose-based waterborne polyurethane resin coating according to any one of claims 1 to 5, characterized in that: The specific steps are as follows: S3: In a multifunctional reactor, adding modified nanocellulose and polysiloxane oligomer according to weight, stirring at a temperature of 20 to 40° C. and a speed of 2000 to 3000 rpm for 1 to 2 hours; S4: In a multifunctional reaction kettle, add aromatic isocyanate according to weight, raise the temperature to 60-80° C., and continue stirring for 1-2 hours to obtain a prepolymer; S5: adding acetone and chain extender in parts by weight, raising the temperature to 70-90° C., and reacting for 1-3 hours under stirring; S6: Cooling to 20-30°C, adding deionized water by weight for emulsification, maintaining under 10-30 kPa for 20-60 minutes for reduced pressure rotary evaporation concentration to obtain an antibacterial nano-cellulose-based waterborne polyurethane emulsion; pouring the emulsion into a polyethylene mold and drying at 50-80°C for 12-24 hours to obtain an antibacterial nano-cellulose-based waterborne polyurethane resin coating.

Citation Information

Patent Citations

  • Synthesis method for in situ polymerization preparation of ZnO / nanocellulose modified waterborne polyurethane

    CN108752564A

  • Preparation method of carboxylation nanocellulose whisker modified waterborne polyurethane

    CN110387028A

  • Waterborne polyurethane resin as well as preparation method and application thereof

    CN115873201A

  • Antimicrobial substrate and method for manufacturing same

    WO2019107195A1

Cited By

  • Preparation process of waterproof paint for roads and bridges

    CN119639330A

  • Preparation process of a waterproof coating for road bridges

    CN119639330B