A highly weather-resistant super-hydrophobic nano-insulating composite coating

By using nanosilicon dioxide, multi-wall carbon nanotubes and porous hollow particles in the coating, the composite coating is formed, which solves the problem of insufficient durability of traditional hydrophobic coatings in low temperature environments, and achieves high weather resistance and self-repair performance. Paint, suitable for a variety of application scenarios.

CN118725737BActive Publication Date: 2024-11-08GANSU ELECTRIC POWER TIANSHUI POWER SUPPLY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411219882.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-08
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The existing hydrophobic surface coatings have insufficient durability and stability in the anti-icing field under low temperature environments, and traditional deicing methods are low in efficiency, high energy consumption and environmental pollution.

Method used

High weather resistance superhydrophobic nano-insulated composite coating is composed of nanosilicon dioxide particles, multi-wall carbon nanotubes, polysilicon nitrogen resin, epoxy resin, ethyl acetate and porous hollow particles. The porous hollow particles are passed through polysulfone and nanoparticles. After mixing, it disperses to form a complex porous structure, combining nanotitanium dioxide particles and dicyclopentadiene catalysts to enhance the hydrophobicity and durability of the coating.

Benefits of technology

It significantly improves the hydrophobicity and weather resistance of the paint, has good self-repair performance and antibacterial properties, and is suitable for a variety of application scenarios that require insulation, waterproofing and high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a highly weatherable super-hydrophobic nano-insulating composite coating, specifically relating to the field of hydrophobic coatings, wherein a highly weatherable super-hydrophobic nano-insulating composite coating includes the following components in parts by weight: 1 to 6 parts of nano-silicon dioxide particles, 1 to 6 parts of multi-walled carbon nanotubes, 20 to 80 parts of polysilicon nitrogen resins, 10 to 50 parts of epoxy resins, 100 to 150 parts of ethyl acetate, 1 to 3 parts of porous hollow particles, and the porous hollow particles are polysulfones containing nanoparticles. The coating prepared by the coating of the present invention has high super-hydrophobicity, antibacterial properties and self-repairing high durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite coatings, and in particular to a highly weather-resistant super-hydrophobic nano-insulating composite coating. Background Art

[0002] Ice and frost, as natural phenomena in low-temperature environments, often pose a major safety hazard to facilities in various industries. In order to remove ice or frost on the surface, active deicing methods are widely used, such as mechanical deicing, electric deicing, and chemical deicing. However, these traditional deicing methods have disadvantages such as low efficiency, high energy consumption, and environmental pollution.

[0003] The surface with super-hydrophobic structure shows extreme water repellency due to its micro-nano structure with low surface energy, that is, water droplets have very little adhesion to the surface and are easy to fall off, so it has a wide range of application prospects in the field of anti-icing. At present, the common hydrophobic surface coating is obtained by adding nanoparticles to the resin coating to obtain a micro-nano structure surface, but the super-hydrophobicity of the hydrophobic surface of the micro-nano structure surface obtained by relying solely on nanoparticles is not stable and strong enough, and its durability is also difficult to withstand the test of the environment. Summary of the invention

[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a highly weather-resistant super-hydrophobic nano-insulating composite coating.

[0005] The above object of the present invention is achieved through the following technical solutions:

[0006] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0007] 1 to 6 parts of nano silicon dioxide particles;

[0008] 1 to 6 parts of multi-walled carbon nanotubes;

[0009] 20-80 parts of polysilicon resin;

[0010] 10-50 parts of epoxy resin;

[0011] 100-150 parts of ethyl acetate;

[0012] 1 to 3 parts of porous hollow particles;

[0013] The porous hollow microparticles are polysulfone containing nanoparticles.

[0014] Furthermore, the preparation method of the porous hollow particles is as follows:

[0015] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of each component are: 10-12 parts of polysulfone, 40-45 parts of N,N-dimethylacetamide, 40-45 parts of diethylene glycol, 1-2 parts of nanoparticles, and 8-10 parts of tetradecane;

[0016] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0017] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours. After changing and washing at least 3 times, dry at room temperature.

[0018] By adopting the above technical solution, the porous hollow particles are first dispersed into the water phase by using the polysulfone oil phase to obtain fine particles, and the polysulfone particles have a complex porous structure after curing by controlling the temperature and solvent selection. Then, by adding the porous hollow particles into the coating, the porous hollow particles form the micro-nano structure of the coating through the porous structure on the surface, the nano-silicon dioxide particles and the multi-walled carbon nanotubes, and the nanoparticles added to the porous hollow particles can also make the surface of the porous hollow particles have a more three-dimensional micro-nano structure, thereby greatly improving the hydrophobicity of the coating.

[0019] Furthermore, the nanoparticles are nano titanium dioxide particles.

[0020] Furthermore, the D50 particle size of the nano titanium dioxide particles is 20 to 50 nm.

[0021] Furthermore, the nanoparticles are silver-loaded nano-titanium dioxide particles.

[0022] Furthermore, the D50 particle size of the silver-loaded nano-titanium dioxide particles is 30 to 50 nm.

[0023] The silver ions in the silver-loaded nano-titanium dioxide particles can give the coating a certain antibacterial property, so that the coating can be used in environments with high antibacterial requirements, thereby increasing the scope of application of the coating.

[0024] Furthermore, the porous hollow particles are post-treated, and the post-treatment includes immersing the porous hollow particles in a dicyclopentadiene emulsion for 1 to 3 hours, then filtering and washing with deionized water and ethanol for 2 to 3 times, and then drying at room temperature;

[0025] The composite coating also includes a dicyclopentadiene catalyst, and the added amount of the dicyclopentadiene catalyst is 0.2 to 0.5 parts.

[0026] Further, the dicyclopentadiene emulsion comprises the following components in parts by weight:

[0027] 2-3 parts of ethylene maleic anhydride copolymer;

[0028] 200-300 parts of deionized water;

[0029] 30-40 parts of dicyclopentadiene.

[0030] After the porous hollow particles are post-treated with dicyclopentadiene, the porous structure of the porous hollow particles contains dicyclopentadiene. After the porous hollow particles are mixed with other components in the coating, under the action of the dicyclopentadiene catalyst, the dicyclopentadiene on the surface of the porous hollow particles will undergo a cross-linking reaction with the epoxy resin, so that a more solid and stable polymer network chain is formed between the porous hollow particles and the resin, making the coating adhesion more stable and the fastness improved. Secondly, part of the dicyclopentadiene is located inside the porous hollow particles and does not completely react when the coating is cured. When the coating is worn, the dicyclopentadiene will be further released to the worn part through capillary action and contact with the dicyclopentadiene catalyst, achieving the effect of self-repairing the coating and improving the durability of the coating.

[0031] Furthermore, it also includes phase change microcapsules with paraffin as core material and melamine resin as wall material, and the added amount of the phase change microcapsules is 1 to 2 parts.

[0032] The addition of phase change microcapsules is beneficial to improving the high temperature resistance of the coating.

[0033] A method for preparing the highly weather-resistant super-hydrophobic nano-insulation composite coating using the above-mentioned method comprises the following steps: mixing the components in proportion and stirring them uniformly.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The coating of the present invention is composed of nano silicon dioxide particles, multi-walled carbon nanotubes, polysilicon nitrogen resin, epoxy resin, ethyl acetate and porous hollow microparticles, wherein the porous hollow microparticles adopt polysulfone containing nanoparticles as a substrate. The preparation process of the porous hollow microparticles is dispersed in an oil phase after the polysulfone is mixed with the nanoparticles, and then dropped into the water phase for dispersion and solidification. By selecting a suitable solvent and temperature control, polysulfone microparticles with a complex porous structure are formed. After these microparticles are added to the coating, the micro-nano structure of the coating is constructed together with the nano silicon dioxide particles and the multi-walled carbon nanotubes, thereby greatly improving the hydrophobicity of the coating. At the same time, the addition of nanoparticles forms a more three-dimensional three-dimensional micro-nano structure on the surface of the porous hollow microparticles, further enhancing the waterproof effect of the coating.

[0036] In addition, silver-loaded nano-titanium dioxide particles, as a type of nanoparticles, can give the coating antibacterial properties, broadening the application range of the coating in environments that require high antibacterial properties. After post-treatment with dicyclopentadiene, the porous hollow particles can undergo a cross-linking reaction with the epoxy resin in the coating to form a strong polymer network chain structure, which enhances the adhesion and stability of the coating. At the same time, dicyclopentadiene can be released through capillary action when the coating is worn and participate in the self-repair reaction, which improves the durability of the coating.

[0037] In order to further improve the high temperature resistance of the coating, the present invention also introduces phase change microcapsules with paraffin as the core material and melamine resin as the wall material into the coating. When the components of the coating are evenly mixed in proportion, the formed coating not only has excellent hydrophobicity and weather resistance, but also has good self-healing performance and antibacterial properties, and is suitable for a variety of application scenarios that require insulation, waterproofing and high temperature resistance. DETAILED DESCRIPTION

[0038] The present invention is described in detail below in conjunction with embodiments.

[0039] Example 1

[0040] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0041] 1 part of nano silicon dioxide particles;

[0042] 1 part of multi-walled carbon nanotubes;

[0043] 20 parts of polysilicon resin;

[0044] Epoxy resin 10 parts;

[0045] 100 parts of ethyl acetate;

[0046] 1 part of porous hollow particles;

[0047] The preparation method of porous hollow microparticles is as follows:

[0048] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 12 parts of polysulfone, 45 parts of N,N-dimethylacetamide, 45 parts of diethylene glycol, 2 parts of nanoparticles, and 10 parts of tetradecane;

[0049] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0050] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0051] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 20 nm.

[0052] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0053] Example 2

[0054] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0055] 6 parts of nano silicon dioxide particles;

[0056] 6 parts of multi-walled carbon nanotubes;

[0057] 80 parts of polysilicon resin;

[0058] Epoxy resin 50 parts;

[0059] 150 parts of ethyl acetate;

[0060] 3 parts of porous hollow microparticles;

[0061] The preparation method of porous hollow microparticles is as follows:

[0062] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of each component are: 10 parts of polysulfone, 40 parts of N,N-dimethylacetamide, 40 parts of diethylene glycol, 1 part of nanoparticles, and 8 parts of tetradecane;

[0063] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0064] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0065] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 20 nm.

[0066] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0067] Example 3

[0068] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0069] 1 part of nano silicon dioxide particles;

[0070] 1 part of multi-walled carbon nanotubes;

[0071] 20 parts of polysilicon resin;

[0072] Epoxy resin 10 parts;

[0073] 100 parts of ethyl acetate;

[0074] 1 part of porous hollow particles;

[0075] The preparation method of porous hollow microparticles is as follows:

[0076] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of each component are: 10 parts of polysulfone, 40 parts of N,N-dimethylacetamide, 40 parts of diethylene glycol, 1 part of nanoparticles, and 8 parts of tetradecane;

[0077] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0078] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0079] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 20 nm.

[0080] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0081] Example 4

[0082] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0083] 6 parts of nano silicon dioxide particles;

[0084] 6 parts of multi-walled carbon nanotubes;

[0085] 80 parts of polysilicon resin;

[0086] Epoxy resin 50 parts;

[0087] 150 parts of ethyl acetate;

[0088] 3 parts of porous hollow microparticles;

[0089] The preparation method of porous hollow microparticles is as follows:

[0090] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 12 parts of polysulfone, 45 parts of N,N-dimethylacetamide, 45 parts of diethylene glycol, 2 parts of nanoparticles, and 10 parts of tetradecane;

[0091] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0092] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0093] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 20 nm.

[0094] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0095] Example 5

[0096] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0097] 1 part of nano silicon dioxide particles;

[0098] 1 part of multi-walled carbon nanotubes;

[0099] 20 parts of polysilicon resin;

[0100] Epoxy resin 10 parts;

[0101] 100 parts of ethyl acetate;

[0102] 1 part of porous hollow particles;

[0103] The preparation method of porous hollow microparticles is as follows:

[0104] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0105] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0106] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0107] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 20 nm.

[0108] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0109] Example 6

[0110] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0111] 3 parts of nano silicon dioxide particles;

[0112] 3 parts of multi-walled carbon nanotubes;

[0113] 50 parts of polysilicon resin;

[0114] Epoxy resin 30 parts;

[0115] 120 parts of ethyl acetate;

[0116] 2 parts of porous hollow microparticles;

[0117] The preparation method of porous hollow microparticles is as follows:

[0118] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 12 parts of polysulfone, 45 parts of N,N-dimethylacetamide, 45 parts of diethylene glycol, 2 parts of nanoparticles, and 10 parts of tetradecane;

[0119] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0120] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0121] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 30 nm.

[0122] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0123] Example 7

[0124] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0125] 1 part of nano silicon dioxide particles;

[0126] 1 part of multi-walled carbon nanotubes;

[0127] 20 parts of polysilicon resin;

[0128] Epoxy resin 10 parts;

[0129] 100 parts of ethyl acetate;

[0130] 1 part of porous hollow particles;

[0131] The preparation method of porous hollow microparticles is as follows:

[0132] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0133] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0134] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0135] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 35 nm.

[0136] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0137] Example 8

[0138] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0139] 3 parts of nano silicon dioxide particles;

[0140] 3 parts of multi-walled carbon nanotubes;

[0141] 50 parts of polysilicon resin;

[0142] Epoxy resin 30 parts;

[0143] 120 parts of ethyl acetate;

[0144] 2 parts of porous hollow microparticles;

[0145] The preparation method of porous hollow microparticles is as follows:

[0146] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 12 parts of polysulfone, 45 parts of N,N-dimethylacetamide, 45 parts of diethylene glycol, 2 parts of nanoparticles, and 10 parts of tetradecane;

[0147] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0148] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0149] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 40 nm.

[0150] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0151] Example 9

[0152] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0153] 3 parts of nano silicon dioxide particles;

[0154] 3 parts of multi-walled carbon nanotubes;

[0155] 50 parts of polysilicon resin;

[0156] Epoxy resin 30 parts;

[0157] 120 parts of ethyl acetate;

[0158] 2 parts of porous hollow microparticles;

[0159] The preparation method of porous hollow microparticles is as follows:

[0160] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0161] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0162] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0163] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 50 nm.

[0164] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0165] Example 10

[0166] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0167] 3 parts of nano silicon dioxide particles;

[0168] 3 parts of multi-walled carbon nanotubes;

[0169] 50 parts of polysilicon resin;

[0170] Epoxy resin 30 parts;

[0171] 120 parts of ethyl acetate;

[0172] 2 parts of porous hollow microparticles;

[0173] The preparation method of porous hollow microparticles is as follows:

[0174] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0175] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0176] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0177] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0178] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0179] Embodiment 11

[0180] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0181] 3 parts of nano silicon dioxide particles;

[0182] 3 parts of multi-walled carbon nanotubes;

[0183] 50 parts of polysilicon resin;

[0184] Epoxy resin 30 parts;

[0185] 120 parts of ethyl acetate;

[0186] 2 parts of porous hollow microparticles;

[0187] The preparation method of porous hollow microparticles is as follows:

[0188] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0189] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0190] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0191] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0192] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in a dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0193] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0194] 2 parts of ethylene maleic anhydride copolymer;

[0195] 200 parts of deionized water;

[0196] 30 parts of dicyclopentadiene.

[0197] The dicyclopentadiene catalyst is Grubbs catalyst.

[0198] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0199] Example 12

[0200] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0201] 3 parts of nano silicon dioxide particles;

[0202] 3 parts of multi-walled carbon nanotubes;

[0203] 50 parts of polysilicon resin;

[0204] Epoxy resin 30 parts;

[0205] 120 parts of ethyl acetate;

[0206] 2 parts of porous hollow microparticles;

[0207] The preparation method of porous hollow microparticles is as follows:

[0208] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0209] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0210] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0211] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0212] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0213] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0214] 3 parts of ethylene maleic anhydride copolymer;

[0215] 300 parts of deionized water;

[0216] 40 parts of dicyclopentadiene.

[0217] The dicyclopentadiene catalyst is Grubbs catalyst.

[0218] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0219] Embodiment 13

[0220] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0221] 3 parts of nano silicon dioxide particles;

[0222] 3 parts of multi-walled carbon nanotubes;

[0223] 50 parts of polysilicon resin;

[0224] Epoxy resin 30 parts;

[0225] 120 parts of ethyl acetate;

[0226] 2 parts of porous hollow microparticles;

[0227] The preparation method of porous hollow microparticles is as follows:

[0228] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0229] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0230] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0231] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0232] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in a dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0233] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0234] 2 parts of ethylene maleic anhydride copolymer;

[0235] 300 parts of deionized water;

[0236] 40 parts of dicyclopentadiene.

[0237] The dicyclopentadiene catalyst is Grubbs catalyst.

[0238] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0239] Embodiment 14

[0240] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0241] 3 parts of nano silicon dioxide particles;

[0242] 3 parts of multi-walled carbon nanotubes;

[0243] 50 parts of polysilicon resin;

[0244] Epoxy resin 30 parts;

[0245] 120 parts of ethyl acetate;

[0246] 2 parts of porous hollow microparticles;

[0247] The preparation method of porous hollow microparticles is as follows:

[0248] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0249] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0250] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0251] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0252] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in a dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0253] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0254] 3 parts of ethylene maleic anhydride copolymer;

[0255] 200 parts of deionized water;

[0256] 30 parts of dicyclopentadiene.

[0257] The dicyclopentadiene catalyst is Grubbs catalyst.

[0258] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0259] Embodiment 15

[0260] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0261] 3 parts of nano silicon dioxide particles;

[0262] 3 parts of multi-walled carbon nanotubes;

[0263] 50 parts of polysilicon resin;

[0264] Epoxy resin 30 parts;

[0265] 120 parts of ethyl acetate;

[0266] 2 parts of porous hollow microparticles;

[0267] The preparation method of porous hollow microparticles is as follows:

[0268] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0269] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0270] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0271] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0272] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in a dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0273] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0274] 2 parts of ethylene maleic anhydride copolymer;

[0275] 300 parts of deionized water;

[0276] 30 parts of dicyclopentadiene.

[0277] The dicyclopentadiene catalyst is Grubbs catalyst.

[0278] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0279] Example 16

[0280] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0281] 3 parts of nano silicon dioxide particles;

[0282] 3 parts of multi-walled carbon nanotubes;

[0283] 50 parts of polysilicon resin;

[0284] Epoxy resin 30 parts;

[0285] 120 parts of ethyl acetate;

[0286] 2 parts of porous hollow microparticles;

[0287] 2 parts of phase change microcapsules;

[0288] 0.2 parts of dicyclopentadiene catalyst;

[0289] The preparation method of porous hollow microparticles is as follows:

[0290] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0291] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0292] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0293] The nanoparticles are silver-loaded nano-titanium dioxide particles, and the D50 particle size of the silver-loaded nano-titanium dioxide particles is 45 nm.

[0294] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in a dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0295] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0296] 2 parts of ethylene maleic anhydride copolymer;

[0297] 300 parts of deionized water;

[0298] 30 parts of dicyclopentadiene.

[0299] Phase change microcapsules are phase change microcapsules with paraffin as core material and melamine resin as wall material.

[0300] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0301] Embodiment 17

[0302] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0303] 3 parts of nano silicon dioxide particles;

[0304] 3 parts of multi-walled carbon nanotubes;

[0305] 50 parts of polysilicon resin;

[0306] Epoxy resin 30 parts;

[0307] 120 parts of ethyl acetate;

[0308] 2 parts of porous hollow microparticles;

[0309] The preparation method of porous hollow microparticles is as follows:

[0310] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0311] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0312] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0313] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 50 nm.

[0314] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in dicyclopentadiene emulsion for 1 hour, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0315] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0316] 2 parts of ethylene maleic anhydride copolymer;

[0317] 200 parts of deionized water;

[0318] 30 parts of dicyclopentadiene.

[0319] The dicyclopentadiene catalyst is Grubbs catalyst.

[0320] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0321] Embodiment 18

[0322] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0323] 3 parts of nano silicon dioxide particles;

[0324] 3 parts of multi-walled carbon nanotubes;

[0325] 50 parts of polysilicon resin;

[0326] Epoxy resin 30 parts;

[0327] 120 parts of ethyl acetate;

[0328] 2 parts of porous hollow microparticles;

[0329] The preparation method of porous hollow microparticles is as follows:

[0330] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0331] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0332] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0333] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 35 nm.

[0334] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in dicyclopentadiene emulsion for 2 hours, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0335] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0336] 2 parts of ethylene maleic anhydride copolymer;

[0337] 200 parts of deionized water;

[0338] 30 parts of dicyclopentadiene.

[0339] The dicyclopentadiene catalyst is Grubbs catalyst.

[0340] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0341] Embodiment 19

[0342] A highly weather-resistant super-hydrophobic nano-insulating composite coating comprises the following components in parts by weight:

[0343] 3 parts of nano silicon dioxide particles;

[0344] 3 parts of multi-walled carbon nanotubes;

[0345] 50 parts of polysilicon resin;

[0346] Epoxy resin 30 parts;

[0347] 120 parts of ethyl acetate;

[0348] 2 parts of porous hollow microparticles;

[0349] The preparation method of porous hollow microparticles is as follows:

[0350] Step A1: adding nanoparticles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 11 parts of polysulfone, 43 parts of N,N-dimethylacetamide, 43 parts of diethylene glycol, 1.5 parts of nanoparticles, and 9 parts of tetradecane;

[0351] Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min;

[0352] Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours, change and wash three times, and then dry at room temperature.

[0353] The nanoparticles are nano titanium dioxide particles, and the D50 particle size of the nano titanium dioxide particles is 20 nm.

[0354] The post-treatment steps of the porous hollow particles are as follows: the porous hollow particles are immersed in dicyclopentadiene emulsion for 3 hours, then filtered and rinsed with deionized water and ethanol for 3 times, and then dried at room temperature.

[0355] The dicyclopentadiene emulsion comprises the following components in parts by weight:

[0356] 2 parts of ethylene maleic anhydride copolymer;

[0357] 200 parts of deionized water;

[0358] 30 parts of dicyclopentadiene.

[0359] The dicyclopentadiene catalyst is Grubbs catalyst.

[0360] A method for preparing a highly weather-resistant super-hydrophobic nano-insulation composite coating comprises the following steps: mixing and stirring the components in proportion and uniformly.

[0361] Comparative Example

[0362] Comparative Example 1

[0363] A composite coating comprises the following components in parts by weight:

[0364] 1 part of nano silicon dioxide particles;

[0365] 1 part of multi-walled carbon nanotubes;

[0366] 20 parts of polysilicon resin;

[0367] Epoxy resin 10 parts;

[0368] 100 parts of ethyl acetate;

[0369] The preparation method of the coating comprises the following steps: mixing the components in proportion and stirring them evenly.

[0370] Detection Methods

[0371] 1. Contact angle test: The surface wettability of the coating was tested using a contact angle meter (OCA 25, Dataphysics GmbH, Germany). The contact angle (CA) and sliding angle (SA) of the coating were tested with 5 μL of deionized water. The average value was taken after testing at 5 different locations.

[0372] 2. Contact angle test after self-repairing: The coating was contacted with 800-mesh, 1000-mesh, and 1200-mesh sandpapers, and a 100g weight was placed on the sample. It was pushed horizontally back and forth along a straight line for 10 cm each time (20 cm in total) as one friction cycle. After 10 friction cycles, the surface wettability of the coating was tested with a contact angle meter (OCA 25, Dataphysics GmbH, Germany) for 1 month. The contact angle (CA) and rolling angle (SA) of the coating were tested with 5 μL of deionized water, and the average value was taken after testing at 5 different positions.

[0373] The contact angle test results of the coating and the contact angle after self-repair are shown in Table 1 below:

[0374]

[0375] Conclusion: It can be seen from the above test results that the coating prepared by the coating of the present invention after spraying has excellent super-hydrophobic properties, and after scratching, the coating prepared by the coating of the present invention has a certain self-repairing ability and can maintain the original hydrophobicity to a greater extent.

[0376] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A highly weather-resistant super-hydrophobic nano-insulating composite coating, characterized in that: The composition comprises the following components in parts by weight: 1 to 6 parts of nano silicon dioxide particles; 1 to 6 parts of multi-walled carbon nanotubes; 20-80 parts of polysilicon resin; 10-50 parts of epoxy resin; 100-150 parts of ethyl acetate; 1 to 3 parts of porous hollow particles; The porous hollow particles are polysulfone containing nano titanium dioxide particles; The porous hollow particles are also post-treated with a dicyclopentadiene emulsion, wherein the dicyclopentadiene emulsion comprises the following components in parts by weight: 2-3 parts of ethylene maleic anhydride copolymer; 200-300 parts of deionized water; 30-40 parts of dicyclopentadiene; The preparation method of the porous hollow microparticles is as follows: Step A1: adding nano titanium dioxide particles and polysulfone to a solution of N,N-dimethylacetamide and diethylene glycol mixed in proportion, adding tetradecane after the polysulfone is completely dissolved, and obtaining an oil phase after the dissolution; wherein the weight proportions of the components are: 10-12 parts of polysulfone, 40-45 parts of N,N-dimethylacetamide, 40-45 parts of diethylene glycol, 1-2 parts of nano titanium dioxide particles, and 8-10 parts of tetradecane; Step A2: dripping the oil phase into the water phase, the water phase is a polyvinyl alcohol solution with a mass concentration of 1%, the mass ratio of the oil phase to the water phase is 1:10, and the temperature of the polyvinyl alcohol solution is controlled to be 70° C., and the polyvinyl alcohol solution is stirred at a speed of 1000 r / min; Step A3: After standing, remove the supernatant and soak the obtained particles in 50% mass concentration ethanol. Change the soaking solution every 12 hours. After changing and washing at least 3 times, dry at room temperature.

2. A highly weather-resistant super-hydrophobic nano-insulating composite coating according to claim 1, characterized in that: The D50 particle size of the nano titanium dioxide particles is 20-50 nm.

3. A highly weather-resistant super-hydrophobic nano-insulating composite coating according to claim 1, characterized in that: The nano titanium dioxide particles are silver-loaded nano titanium dioxide particles.

4. A highly weather-resistant super-hydrophobic nano-insulating composite coating according to claim 3, characterized in that: The D50 particle size of the silver-carrying nano-titanium dioxide particles is 30-50 nm.

5. A highly weather-resistant super-hydrophobic nano-insulating composite coating according to claim 1, characterized in that: The post-treatment comprises soaking the porous hollow particles in a dicyclopentadiene emulsion for 1 to 3 hours, then filtering and washing with deionized water and ethanol for 2 to 3 times, and then drying at room temperature; The composite coating also includes a dicyclopentadiene catalyst, and the added amount of the dicyclopentadiene catalyst is 0.2 to 0.5 parts.

6. A highly weather-resistant super-hydrophobic nano-insulating composite coating according to claim 1, characterized in that: It also includes phase-change microcapsules with paraffin as core material and melamine resin as wall material. The added amount of the phase-change microcapsules is 1 to 2 parts.