Water-resistant polyurethane adhesive for shoes and preparation method thereof

By using ingredients such as superhydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer and superhydrophobic inorganic particles in the adhesive, combined with epoxy resin modification and polydimethylsiloxane grafting technology, the adhesive problem is solved The problem of insufficient water resistance of the agent is significantly improved, and the water resistance and solvent resistance are significantly improved, extending the service life of the shoes.

CN118725812AInactive Publication Date: 2024-10-01JIAN XUNDA TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410878924.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the use of existing adhesives, it is easy to cause the soles and uppers to deglue due to insufficient water resistance, which affects the service life of the shoes. In particular, the demand for branded shoes and co-branded shoes is higher.

Method used

It uses ingredients such as superhydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, superhydrophobic inorganic particles and epoxy resin modified polyurethane, through the combination of polydimethylsiloxane grafting and styrene-maleic anhydride copolymer. , improve the water resistance and solvent resistance of the adhesive.

Benefits of technology

It significantly improves the water resistance and solvent resistance of the adhesive, extends the service life of the shoes, and improves the overall performance of the adhesive while ensuring peeling strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004923940500000091
    Figure BDA0004923940500000091
Patent Text Reader

Abstract

The invention discloses a water-resistant polyurethane adhesive for shoes, which is prepared from the following ingredients in parts by weight: 60 to 80 parts of super-hydrophobic polyurethane dispersoid, 30 to 40 parts of ethylene-vinyl acetate copolymers, 3 to 8 parts of super-hydrophobic inorganic particles, 0.5 to 1.0 part of styrene-maleic anhydride copolymers, 0.5 to 0.8 part of RHEOLATE 299 nonionic polyurethane associative thickeners, 0.5 to 0.8 part of 2, 2, 4-trimethyl-1, 3-pentanediol monoisobutyrate, 0.5 to 0.8 part of 2, 2, 4-trimethyl-1, 3-pentanediol monoisobutyrate, 0.5 to 0.8 part of 2, 3-pentanediol monoisobutyrate, the coating is prepared from the following components in parts by weight: 0.1 to 0.3 part of 2, 6-di-tert-butyl-4-methylphenol, 0.1 to 0.4 part of a defoaming agent Foamex 830 and 0.2 to 0.5 part of a flatting agent BYK-345. According to the invention, from the perspective of modification and grafting of a polyurethane dispersion, polydimethylsiloxane is introduced in the reaction process and is grafted on a polyurethane main body to form a macromolecular group, so that the super-hydrophobicity of polyurethane can be effectively improved, and the water resistance of the adhesive is further improved; meanwhile, the epoxy resin is adopted to modify the polyurethane dispersion, so that the peel strength, the water resistance and the yellowing resistance of the adhesive can be effectively guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and particularly relates to a water-resistant polyurethane adhesive for shoes and a preparation method thereof. Background Art

[0002] Adhesives are in great demand in the shoemaking industry. The performance of adhesives determines the quality of the shoe products, especially the pull-out strength and water resistance, which are the focus of research. The soles and uppers of shoes on the market are not worn or damaged, but the user experience is often poor due to the debonding between the soles and uppers. Even after users purchase adhesives for repairs, the adhesives are often prone to debonding again due to the uneven performance of the purchased adhesives. For brand shoes and some co-branded shoes, the demand for adhesive performance is even higher.

[0003] Patent CN 113913146 A discloses an adhesive, which comprises component A and component B, wherein the component A comprises: 20-70 parts by weight of aqueous polyurethane dispersion; 20-70 parts by weight of natural latex; 10-50 parts by weight of ethylene-vinyl acetate copolymer emulsion; wherein the aqueous polyurethane dispersion, natural latex and ethylene-vinyl acetate copolymer emulsion total 100 parts by weight, and the component B comprises: curing agent, which is 1-10 parts by weight based on the total weight of the aqueous polyurethane dispersion, natural latex and ethylene-vinyl acetate copolymer emulsion. By introducing aqueous polyurethane emulsion and ethylene-vinyl acetate emulsion, the adhesive of the present invention has obvious improvements in initial strength, later strength and water washing resistance, and can meet the bonding requirements of different upper substrates.

[0004] Patent CN 105400481 A discloses a method for synthesizing a waterborne polyurethane adhesive with high solid content, good stable dispersibility, high initial adhesion strength, and good resistance to moisture and heat aging. Castor oil has a functionality of 2.7 and contains a relatively long fatty acid chain. Introducing a certain amount of castor oil into the WPU structure can improve the crosslinking density of WPU to a certain extent. The side-hanging fatty acid chain also has good hydrophobicity and flexibility. While improving water resistance and heat resistance, it can also improve its crystallinity and wettability to substrates (such as leather, etc.).

[0005] Patent CN 105348469 A discloses a heat-resistant and water-resistant high-strength polyurethane adhesive and a preparation method thereof, which is composed of a main component and a modifier component in a mass ratio of 10 to 15:1; the synthetic raw materials of the main component include polybutylene adipate, polyhexanediol adipate, castor oil-modified polyol H-1823, castor oil-modified polyol H-52, castor oil-modified polyol AC-006, isocyanate a, etc.; the synthetic raw materials of the modifier component include chain extender b, isocyanate b and ethyl acetate; the two highly crystalline polyester polyols selected by the present invention and their addition ratio make the polyurethane adhesive have good initial adhesion, high peel strength and temperature resistance, and the addition of castor oil-modified polyol improves the water resistance of the polyurethane adhesive.

[0006] Existing patents have studied waterborne polyurethane adhesives and have also improved their corresponding properties. However, the performance improvement of adhesives, especially water resistance, is still a demand of the prior art. Summary of the invention

[0007] Based on the deficiencies and needs of the prior art, the purpose of the present invention is to provide a water-resistant polyurethane adhesive for shoes and a preparation method thereof, which effectively improves the water resistance of the adhesive while ensuring the peel strength of the adhesive, can extend the time that the shoes do not come apart, and thus increase the service life of the shoes.

[0008] To achieve the above-mentioned purpose and effect, one of the technical solutions adopted by the present invention is as follows: a water-resistant polyurethane adhesive for shoes, comprising the following components, by weight: 60 to 80 parts of super-hydrophobic polyurethane dispersion, 30 to 40 parts of ethylene-vinyl acetate copolymer, 3 to 8 parts of super-hydrophobic inorganic particles, 0.5 to 1.0 parts of styrene-maleic anhydride copolymer, 0.5 to 0.8 parts of RHEOLATE299 non-ionic polyurethane associative thickener, 0.1 to 0.3 parts of 2,6-di-tert-butyl-4-methylphenol, 0.1 to 0.4 parts of defoamer Foamex830, and 0.2 to 0.5 parts of leveling agent BYK-345.

[0009] Furthermore, the water-resistant polyurethane adhesive for shoes is composed of the following ingredients, in parts by weight: 60 to 80 parts of super-hydrophobic polyurethane dispersion, 30 to 40 parts of ethylene-vinyl acetate copolymer, 3 to 8 parts of super-hydrophobic inorganic particles, 0.5 to 1.0 parts of styrene-maleic anhydride copolymer, 0.5 to 0.8 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.1 to 0.3 parts of 2,6-di-tert-butyl-4-methylphenol, 0.1 to 0.4 parts of defoaming agent Foamex830, and 0.2 to 0.5 parts of leveling agent BYK-345.

[0010] Furthermore, the water-resistant polyurethane adhesive for shoes is composed of the following ingredients, in parts by weight: 65 to 75 parts of super-hydrophobic polyurethane dispersion, 33 to 36 parts of ethylene-vinyl acetate copolymer, 5 to 6 parts of super-hydrophobic inorganic particles, 0.7 to 0.8 parts of styrene-maleic anhydride copolymer, 0.6 to 0.7 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2 to 0.3 parts of 2,6-di-tert-butyl-4-methylphenol, 0.2 to 0.3 parts of defoaming agent Foamex830, and 0.3 to 0.4 parts of leveling agent BYK-345.

[0011] Furthermore, the water-resistant polyurethane adhesive for shoes is composed of the following ingredients, in parts by weight: 70 parts of super-hydrophobic polyurethane dispersion, 35 parts of ethylene-vinyl acetate copolymer, 6 parts of super-hydrophobic inorganic particles, 0.7 parts of styrene-maleic anhydride copolymer, 0.6 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2 parts of 2,6-di-tert-butyl-4-methylphenol, 0.3 parts of defoamer Foamex830, and 0.4 parts of leveling agent BYK-345.

[0012] Furthermore, the preparation steps of the super hydrophobic polyurethane dispersion include:

[0013] (1) Add 50-70 parts of poly(1,4-butylene adipate), 100-130 parts of 1,4-cyclohexane diisocyanate, and 1-2 parts of polydimethylsiloxane to a reactor equipped with a condensing device, a stirring device, and gas protection, and keep the temperature in a water bath at 70-80°C. Then slowly drop 1-2 parts of dibutyltin dilaurate and 20-25 parts of propylene glycol to start the reaction; after 30-60 minutes, add 10-25 parts of dimethylol propionic acid. After reacting for 2-3 hours, cool the reaction system to 40-45°C, add 2-3 parts of acetone to reduce its viscosity, and continue the reaction for 20-30 minutes; then add 5-10 parts of hydroxyethyl methacrylate to react for 20-30 minutes, then add 3-5 parts of triethanolamine and 1-2 parts of deionized water, and emulsify by high-speed stirring to obtain a polyurethane dispersion.

[0014] (2) heating the polyurethane dispersion to 70-90° C., slowly dropping 6-12 parts of epoxidized styrene monomer and 1.0-1.5 parts of sodium persulfate thereto, reacting for 2-3 hours while continuously stirring, and cooling to room temperature after the reaction to obtain a superhydrophobic polyurethane dispersion;

[0015] (3) filtering the super hydrophobic polyurethane dispersion obtained in step (2) and removing low molecular weight organic matter and water by vacuum distillation.

[0016] Epoxy resin modified polyurethane can improve various properties of polyurethane, which is also the subject of much research in the prior art. Based on epoxy resin modification, this application seeks to further improve the performance of the adhesive in terms of ensuring water resistance, solvent resistance and yellowing resistance.

[0017] This application starts from the modification and grafting of polyurethane dispersion, synthesizes polyurethane dispersion from raw materials such as poly(1,4-butylene adipate) and 1,4-cyclohexane diisocyanate, and introduces polydimethylsiloxane during the reaction to make it grafted on the polyurethane body to form a macromolecular group, which can effectively improve the super-hydrophobicity of polyurethane and thus improve the water resistance of adhesive. If the content of polydimethylsiloxane is too low, the super-hydrophobicity will be weak, and if the content is too high, it will affect the chemical properties of polyurethane. Based on this, the applicant has experimentally determined that the reaction amount of polydimethylsiloxane is 1 to 2 parts.

[0018] Furthermore, the super-hydrophobic inorganic particles are selected from super-hydrophobic nano-silicon oxide powder. The present application further adopts a compounding of super-hydrophobic inorganic particles and a hydrophobic polyurethane dispersion as a means to achieve ultra-high water resistance of the polyurethane adhesive. The addition of super-hydrophobic inorganic particles further improves its water resistance to a certain extent. Styrene-maleic anhydride copolymer is added to the polyurethane adhesive as a polymer dispersant, which can effectively improve the dispersion uniformity of nanoparticles.

[0019] To achieve the above-mentioned purpose and effect, the second technical solution adopted by the present invention is as follows: a method for preparing a water-resistant polyurethane adhesive for shoes, comprising the following steps:

[0020] (1) pouring a super-hydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, super-hydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heating to 40-50° C., mixing and stirring at a stirring speed of 300-400 rpm for 15-20 min to obtain a uniform mixture A;

[0021] (2) The mixture A is cooled to room temperature, and under continuous stirring, 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence and the viscosity is adjusted to 4000-5000 cps to obtain the water-resistant polyurethane adhesive for shoes.

[0022] Furthermore, in step (2), the stirring speed is 200-300 rpm and the stirring time is 15-20 min.

[0023] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0024] (1) The present application modifies and grafts the polyurethane dispersion with epoxy resin and polydimethylsiloxane, so that the polyurethane dispersion has super hydrophobicity, thereby further improving the water resistance of the adhesive while ensuring the water resistance, solvent resistance and yellowing resistance of the adhesive, thereby greatly improving the service life of the shoes.

[0025] (2) The synergistic effect of superhydrophobic polyurethane dispersion and superhydrophobic inorganic particles can also improve the water resistance of the adhesive to a certain extent.

[0026] (3) The water-resistant polyurethane adhesive for shoes prepared by the present invention can also be used in other fields, such as electronic device packaging and other technical fields, and still has good bonding strength. DETAILED DESCRIPTION

[0027] The following is a specific implementation case of the present invention, and the present invention is further described in detail. However, the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents, wherein the super-hydrophobic nano-silicon oxide powder is purchased from Angxing New Carbon Material Changzhou Co., Ltd., wherein the epoxy resin is GR828D TM .

[0028] Example 1

[0029] A preparation step of a super hydrophobic polyurethane dispersion comprises:

[0030] (1) Add 60 parts of poly(1,4-butylene adipate), 120 parts of 1,4-cyclohexane diisocyanate, and 1 part of polydimethylsiloxane to a reactor equipped with a condensing device, a stirring device, and gas protection, and keep the temperature in a water bath at 75°C. Then slowly add 2 parts of dibutyltin dilaurate and 23 parts of propylene glycol to start the reaction; 15 parts of dimethylol propionic acid are added after 40 minutes. After reacting for 3 hours, the reaction system is cooled to 40°C, and 2 parts of acetone are added to reduce its viscosity. The reaction is continued for 20 minutes; then 6 parts of hydroxyethyl methacrylate are added to react for 25 minutes, and then 4 parts of triethanolamine and 2 parts of deionized water are added. After high-speed stirring and emulsification, a polyurethane dispersion is obtained.

[0031] (2) heating the polyurethane dispersion to 80° C., slowly dropping 10 parts of epoxidized styrene monomer and 1.3 parts of sodium persulfate thereto, reacting for 2 hours while continuously stirring, and cooling to room temperature after the reaction to obtain a superhydrophobic polyurethane dispersion;

[0032] (3) filtering the super hydrophobic polyurethane dispersion obtained in step (2) and removing low molecular weight organic matter and water by vacuum distillation.

[0033] Comparative Example 1

[0034] A preparation step of a polyurethane dispersion comprises:

[0035] (1) Add 60 parts of poly(1,4-butylene adipate) and 120 parts of 1,4-cyclohexane diisocyanate to a reactor equipped with a condensing device, a stirring device and gas protection, keep the temperature in a 75°C water bath, then slowly drop 2 parts of dibutyltin dilaurate and 23 parts of propylene glycol to start the reaction; 15 parts of dimethylol propionic acid are added after 40 minutes. After reacting for 3 hours, cool the reaction system to 40°C, add 2 parts of acetone to reduce its viscosity, and continue the reaction for 20 minutes; then add 6 parts of hydroxyethyl methacrylate to react for 25 minutes, then add 4 parts of triethanolamine and 2 parts of deionized water, and emulsify by high-speed stirring to obtain a polyurethane dispersion.

[0036] (2) heating the polyurethane dispersion to 80° C., slowly dropping 10 parts of epoxidized styrene monomer and 1.3 parts of sodium persulfate thereto, reacting for 2 hours while continuously stirring, and cooling to room temperature after the reaction to obtain a polyurethane dispersion;

[0037] (3) filtering the polyurethane dispersion obtained in step (2) and removing low molecular weight organic matter and water by vacuum distillation.

[0038] In order to test the effect of polydimethylsiloxane on the polyurethane dispersion, the polyurethane dispersions prepared in Example 1 and Comparative Example 1 were brushed on the flat substrate surface and dried to obtain polyurethane coatings; the contact angle test was performed on the coatings.

[0039] The contact angle of the polyurethane coating surface of Example 1 is 157.8° and the rolling angle is 3.4°, and the surface exhibits superhydrophobicity; while the contact angle of the polyurethane coating surface of Comparative Example 1 is 94.3° and the rolling angle is 10.7°. It can be seen that the introduction of polydimethylsiloxane can significantly improve the superhydrophobicity of polyurethane.

[0040] Unless otherwise specified, the super-hydrophobic polyurethane dispersion used in the following examples and comparative examples is the one prepared in Example 1.

[0041] Example 2

[0042] A water-resistant polyurethane adhesive for shoes consists of the following components, measured in parts by weight: 60 parts of super-hydrophobic polyurethane dispersion, 30 parts of ethylene-vinyl acetate copolymer, 3 parts of super-hydrophobic inorganic particles, 0.5 parts of styrene-maleic anhydride copolymer, 0.5 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.1 parts of 2,6-di-tert-butyl-4-methylphenol, 0.1 parts of defoamer Foamex830, and 0.2 parts of leveling agent BYK-345.

[0043] The preparation method of the water-resistant polyurethane adhesive for shoes comprises the following steps:

[0044] (1) pouring the super-hydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, super-hydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heating to 40° C., mixing and stirring at a stirring speed of 3000 rpm for 15 min to obtain a uniform mixture A;

[0045] (2) The mixture A is cooled to room temperature, and 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence under continuous stirring, and the viscosity is adjusted to 4200 cps, thereby obtaining the water-resistant polyurethane adhesive for shoes.

[0046] Wherein, in step (2), the stirring speed is 200 rpm and the stirring time is 15 min.

[0047] Example 3

[0048] A water-resistant polyurethane adhesive for shoes consists of the following components, measured in parts by weight: 80 parts of super-hydrophobic polyurethane dispersion, 40 parts of ethylene-vinyl acetate copolymer, 8 parts of super-hydrophobic inorganic particles, 1.0 part of styrene-maleic anhydride copolymer, 0.8 part of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.3 part of 2,6-di-tert-butyl-4-methylphenol, 0.4 part of defoamer Foamex830, and 0.5 part of leveling agent BYK-345.

[0049] The preparation method of the water-resistant polyurethane adhesive for shoes comprises the following steps:

[0050] (1) pouring the super-hydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, super-hydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heating to 45° C., mixing and stirring at a stirring speed of 400 rpm for 20 min to obtain a uniform mixture A;

[0051] (2) The mixture A is cooled to room temperature, and 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence under continuous stirring, and the viscosity is adjusted to 4800 cps, thereby obtaining the water-resistant polyurethane adhesive for shoes.

[0052] Wherein, in step (2), the stirring speed is 300 rpm and the stirring time is 20 min.

[0053] Example 4

[0054] A water-resistant polyurethane adhesive for shoes consists of the following components, measured in parts by weight: 70 parts of super-hydrophobic polyurethane dispersion, 35 parts of ethylene-vinyl acetate copolymer, 6 parts of super-hydrophobic inorganic particles, 0.7 parts of styrene-maleic anhydride copolymer, 0.6 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2 parts of 2,6-di-tert-butyl-4-methylphenol, 0.3 parts of defoamer Foamex830, and 0.4 parts of leveling agent BYK-345.

[0055] The preparation method of the water-resistant polyurethane adhesive for shoes comprises the following steps:

[0056] (1) pouring the super-hydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, super-hydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heating to 43° C., mixing and stirring at a stirring speed of 350 rpm for 18 min to obtain a uniform mixture A;

[0057] (2) The mixture A is cooled to room temperature, and 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence under continuous stirring, and the viscosity is adjusted to 4600 cps, thereby obtaining the water-resistant polyurethane adhesive for shoes.

[0058] Wherein, in step (2), the stirring speed is 250 rpm and the stirring time is 17 min.

[0059] In order to better examine and compare the role and effect of certain components in the adhesive, the following comparative examples are provided based on Example 4.

[0060] Comparative Example 2

[0061] A water-resistant polyurethane adhesive for shoes is composed of the following components, measured in parts by weight: 70 parts of a polyurethane dispersion (prepared in Comparative Example 1), 35 parts of an ethylene-vinyl acetate copolymer, 6 parts of superhydrophobic inorganic particles, 0.7 parts of a styrene-maleic anhydride copolymer, 0.6 parts of a RHEOLATE 299 nonionic polyurethane associative thickener, 0.2 parts of 2,6-di-tert-butyl-4-methylphenol, 0.3 parts of a defoamer Foamex830, and 0.4 parts of a leveling agent BYK-345.

[0062] The preparation method of the water-resistant polyurethane adhesive for shoes comprises the following steps:

[0063] (1) Pour the polyurethane dispersion, ethylene-vinyl acetate copolymer, superhydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heat to 43° C., mix and stir at a stirring speed of 350 rpm for 18 min to obtain a uniform mixture A;

[0064] (2) The mixture A is cooled to room temperature, and 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence under continuous stirring, and the viscosity is adjusted to 4600 cps, thereby obtaining the water-resistant polyurethane adhesive for shoes.

[0065] Wherein, in step (2), the stirring speed is 250 rpm and the stirring time is 17 min.

[0066] Comparative Example 3

[0067] A water-resistant polyurethane adhesive for shoes consists of the following components, measured in parts by weight: 70 parts of super-hydrophobic polyurethane dispersion, 6 parts of super-hydrophobic inorganic particles, 0.7 parts of styrene-maleic anhydride copolymer, 0.6 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2 parts of 2,6-di-tert-butyl-4-methylphenol, 0.3 parts of defoamer Foamex830, and 0.4 parts of leveling agent BYK-345.

[0068] The preparation method of the water-resistant polyurethane adhesive for shoes comprises the following steps:

[0069] (1) Pour the polyurethane dispersion, superhydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heat to 43° C., mix and stir at a stirring speed of 350 rpm for 18 min to obtain a uniform mixture A;

[0070] (2) The mixture A is cooled to room temperature, and 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence under continuous stirring, and the viscosity is adjusted to 4600 cps, thereby obtaining the water-resistant polyurethane adhesive for shoes.

[0071] Wherein, in step (2), the stirring speed is 250 rpm and the stirring time is 17 min.

[0072] Comparative Example 4

[0073] A water-resistant polyurethane adhesive for shoes consists of the following components, measured in parts by weight: 70 parts of super-hydrophobic polyurethane dispersion, 35 parts of ethylene-vinyl acetate copolymer, 0.7 parts of styrene-maleic anhydride copolymer, 0.6 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2 parts of 2,6-di-tert-butyl-4-methylphenol, 0.3 parts of defoamer Foamex830, and 0.4 parts of leveling agent BYK-345.

[0074] The preparation method of the water-resistant polyurethane adhesive for shoes comprises the following steps:

[0075] (1) Pour the polyurethane dispersion, ethylene-vinyl acetate copolymer, and styrene-maleic anhydride copolymer into a stirrer, heat to 43° C., mix and stir at a stirring speed of 350 rpm for 18 min to obtain a uniform mixture A;

[0076] (2) The mixture A is cooled to room temperature, and 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence under continuous stirring, and the viscosity is adjusted to 4600 cps, thereby obtaining the water-resistant polyurethane adhesive for shoes.

[0077] Wherein, in step (2), the stirring speed is 250 rpm and the stirring time is 17 min.

[0078] The relevant properties of the high-strength, heat-resistant shoe adhesive prepared in this application were examined, specifically the peel strength and water resistance were mainly tested.

[0079] (1) Peel strength test: The test conditions are rubber sole and PU leather upper. Cut the two into 150mm×30mm×5mm size specimens, apply adhesive evenly on one side of the two surfaces, stagger the applied surfaces and bond them together, dry at 50℃, and press at 1.2MPa for 10s. Measure the peel strength after 24h. The peel strength is measured by a tensile tester clamped at the non-overlapping parts of the rubber and PU specimens at 200mm·min -1 The measurement results are shown in Table 1.

[0080] (2) Water absorption test: Pour the adhesive into a container of 20 mm × 20 mm × 20 mm, allow it to solidify, demould it, weigh the mass of the sample as w1, and then soak it in deionized water. Take it out after 72 hours, blow dry the surface moisture, weigh the mass of the sample as w2, and calculate the water absorption of the adhesive = (w2-w1) / w1×100%. The calculation results are shown in Table 1.

[0081] (3) The adhesive is brushed onto the flat substrate surface, cured, and dried to obtain an adhesive coating; the contact angle of the coating is tested, and the measurement results are shown in Table 1.

[0082] Table 1

[0083]

[0084] It can be seen from the data in Table 1 that the water-resistant polyurethane adhesive for shoes prepared in the embodiment of the present invention has excellent peel strength and water resistance. Compared with Comparative Examples 2-4, which do not use super-hydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, and super-hydrophobic inorganic particles, the performance of the adhesive in various aspects has decreased. This shows that the above components play an important role in the adhesive system.

[0085] The composition of Comparative Example 2 is basically the same as that of Example 4, but the difference is that the polyurethane dispersion of Comparative Example 2 is not grafted with polydimethylsiloxane, and the peel strength of the obtained adhesive is reduced, but not significantly; however, the water absorption rate and contact angle data show that the water resistance of the adhesive of Comparative Example 2 is significantly reduced, and the test shows that it does not have superhydrophobicity; this is consistent with the conclusions obtained in Example 1 and Comparative Example 1. It can be seen that polydimethylsiloxane has a significant effect on the grafting of polyurethane dispersions.

[0086] The composition of Comparative Example 3 is basically the same as that of Example 4, but the difference is that Comparative Example 3 does not use ethylene-vinyl acetate copolymer, and the obtained adhesive has a more obvious decrease in peel strength; in addition, the water absorption rate increases and the contact angle decreases, but the amplitude is not large. Superhydrophobic polyurethane dispersion and ethylene-vinyl acetate copolymer are the main components of the adhesive system, which also have a great influence on the guarantee of basic mechanical properties.

[0087] The composition of Comparative Example 4 is basically the same as that of Example 4, but the difference is that Comparative Example 4 does not use super-hydrophobic inorganic particles, and the obtained adhesive also has a certain degree of decrease in peel strength; however, the water absorption rate increases and the contact angle decreases, and the amplitude is also large. It shows that the use of super-hydrophobic inorganic particles can produce a synergistic effect with the super-hydrophobic polyurethane dispersion, thereby improving the water resistance of the adhesive.

[0088] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A water-resistant polyurethane adhesive for shoes, characterized in that: The invention comprises the following components in parts by weight: 60 to 80 parts of super-hydrophobic polyurethane dispersion, 30 to 40 parts of ethylene-vinyl acetate copolymer, 3 to 8 parts of super-hydrophobic inorganic particles, 0.5 to 1.0 parts of styrene-maleic anhydride copolymer, 0.5 to 0.8 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.1 to 0.3 parts of 2,6-di-tert-butyl-4-methylphenol, 0.1 to 0.4 parts of defoamer Foamex830, and 0.2 to 0.5 parts of leveling agent BYK-345.

2. The water-resistant polyurethane adhesive for shoes according to claim 1, characterized in that: The invention is composed of the following components in parts by weight: 60 to 80 parts of super-hydrophobic polyurethane dispersion, 30 to 40 parts of ethylene-vinyl acetate copolymer, 3 to 8 parts of super-hydrophobic inorganic particles, 0.5 to 1.0 parts of styrene-maleic anhydride copolymer, 0.5 to 0.8 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.1 to 0.3 parts of 2,6-di-tert-butyl-4-methylphenol, 0.1 to 0.4 parts of defoamer Foamex830, and 0.2 to 0.5 parts of leveling agent BYK-345.

3. The water-resistant polyurethane adhesive for shoes according to any one of claims 1 to 2, characterized in that: The invention is composed of the following components in parts by weight: 65-75 parts of super-hydrophobic polyurethane dispersion, 33-36 parts of ethylene-vinyl acetate copolymer, 5-6 parts of super-hydrophobic inorganic particles, 0.7-0.8 parts of styrene-maleic anhydride copolymer, 0.6-0.7 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2-0.3 parts of 2,6-di-tert-butyl-4-methylphenol, 0.2-0.3 parts of defoamer Foamex830 and 0.3-0.4 parts of leveling agent BYK-345.

4. The water-resistant polyurethane adhesive for shoes according to any one of claims 1 to 2, characterized in that: The invention is composed of the following components in parts by weight: 70 parts of super-hydrophobic polyurethane dispersion, 35 parts of ethylene-vinyl acetate copolymer, 6 parts of super-hydrophobic inorganic particles, 0.7 parts of styrene-maleic anhydride copolymer, 0.6 parts of RHEOLATE 299 non-ionic polyurethane associative thickener, 0.2 parts of 2,6-di-tert-butyl-4-methylphenol, 0.3 parts of defoamer Foamex830, and 0.4 parts of leveling agent BYK-345.

5. The water-resistant polyurethane adhesive for shoes according to any one of claims 1 to 4, characterized in that: The preparation steps of the super hydrophobic polyurethane dispersion include: (1) Add 50-70 parts of poly(1,4-butylene adipate), 100-130 parts of 1,4-cyclohexane diisocyanate, and 1-2 parts of polydimethylsiloxane to a reactor equipped with a condensing device, a stirring device, and gas protection, and keep the temperature in a water bath at 70-80°C. Then slowly drop 1-2 parts of dibutyltin dilaurate and 20-25 parts of propylene glycol to start the reaction; after 30-60 minutes, add 10-25 parts of dimethylol propionic acid. After reacting for 2-3 hours, cool the reaction system to 40-45°C, add 2-3 parts of acetone to reduce its viscosity, and continue the reaction for 20-30 minutes; then add 5-10 parts of hydroxyethyl methacrylate to react for 20-30 minutes, then add 3-5 parts of triethanolamine and 1-2 parts of deionized water, and emulsify by high-speed stirring to obtain a polyurethane dispersion. (2) heating the polyurethane dispersion to 70-90° C., slowly dropping 6-12 parts of epoxidized styrene monomer and 1.0-1.5 parts of sodium persulfate thereto, reacting for 2-3 hours while continuously stirring, and cooling to room temperature after the reaction to obtain a superhydrophobic polyurethane dispersion; (3) filtering the super hydrophobic polyurethane dispersion obtained in step (2) and removing low molecular weight organic matter and water by vacuum distillation.

6. The water-resistant polyurethane adhesive for shoes according to any one of claims 1 to 2, characterized in that: The super-hydrophobic inorganic particles are selected from super-hydrophobic nano-silicon oxide powder.

7. A method for preparing the water-resistant polyurethane adhesive for shoes as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: (1) pouring a super-hydrophobic polyurethane dispersion, ethylene-vinyl acetate copolymer, super-hydrophobic inorganic particles, and styrene-maleic anhydride copolymer into a stirrer, heating to 40-50° C., mixing and stirring at a stirring speed of 300-400 rpm for 15-20 min to obtain a uniform mixture A; (2) The mixture A is cooled to room temperature, and under continuous stirring, 2,6-di-tert-butyl-4-methylphenol, leveling agent BYK-345, RHEOLATE 299 nonionic polyurethane associative thickener, and defoaming agent Foamex 830 are added to the mixture A in sequence and the viscosity is adjusted to 4000-5000 cps to obtain the water-resistant polyurethane adhesive for shoes.

8. The preparation method according to claim 7, characterized in that: In step (2), the stirring speed is 300-500 rpm and the stirring time is 20-30 min.

Citation Information

Patent Citations

  • Waterborne polyurethane glue and preparation method thereof

    CN106398623A

  • Waterborne polyurethane-polyacrylate composite emulsion used for waterproof coating and preparation method thereof

    CN108467463A

  • Preparation method of bionic super-hydrophobic acrylate modified polyurethane / nano particle composite coating

    CN112409916A

  • Adhesive as well as preparation method and application thereof

    CN113913146A

  • Single-component polyurethane spot welding adhesive as well as preparation method and application thereof

    CN114410265A