Abrasive particles for polishing solution, preparation method of abrasive particles, polishing solution and substrate polishing method

By using silica-coated glucose nanoparticles and ultraviolet light-assisted technology, the problems of low SiC substrate polishing efficiency and surface defects are solved, and high-speed, high-quality SiC substrate polishing is achieved, which is suitable for mass production.

CN118725825APending Publication Date: 2024-10-01TJ INNOVATIVE SEMICON SUBSTRATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410820894.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, the polishing efficiency of SiC substrates is low and surface defects are prone to occur. Especially in the rough polishing and fine polishing processes, strong acidic polishing fluids cause serious corrosion phenomena, while alkaline polishing fluids remove too slowly, making it difficult to meet the needs of large quantities. production needs.

Method used

Silica-coated glucose nanoparticles are used as abrasive particles, and hydroxyl radicals are generated through the assistance of ultraviolet light to react with the SiC substrate to form a soft modified layer. The modified layer is removed by mechanical friction, and combined with an alkaline polishing solution to Improve polishing rate and surface quality.

Benefits of technology

Achieve high-rate, high-quality polishing of SiC substrates. The surface roughness after polishing is extremely low, Ra<0.1nm. There are no scratches or defects under the AFM field of view. The polishing rate is fast, meeting mass production requirements and extending the polishing pad. service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004909067040000191
    Figure BDA0004909067040000191
  • Figure BDA0004909067040000201
    Figure BDA0004909067040000201
Patent Text Reader

Abstract

The invention relates to an abrasive particle for a polishing solution, a preparation method of the abrasive particle, the polishing solution and a substrate polishing method, in particular to the field of substrate surface treatment.The abrasive particle for the polishing solution comprises glucose nanoparticles coated with silicon dioxide; the grain size of the abrasive particles for the polishing solution is 30-100 nm. According to the abrasive particles for the polishing solution, provided by the invention, under the auxiliary action of ultraviolet light, the glucose nanoparticles lose one hydrogen atom to form hydroxyl radicals. And then the formed hydroxyl free radicals. OH and the SiC substrate are subjected to oxidation reaction to generate a soft surface modification layer, so that the surface hardness is reduced, and the polishing rate is increased. Meanwhile, the Mohs hardness of the coated silicon dioxide is higher than that of soluble SiO3 < 2-> generated by glucose nanoparticles and SiC, a modified layer can be easily removed through the mechanical friction effect of an abrasive material, the hardness of silicon oxide abrasive particles is lower than that of the SiC substrate, and the SiC surface cannot be scratched in the polishing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of substrate surface treatment, and specifically to an abrasive grain for polishing liquid and a preparation method thereof, a polishing liquid, and a substrate polishing method, and in particular to an abrasive grain for polishing a SiC substrate and a preparation method thereof, a polishing liquid, and a substrate polishing method. Background Art

[0002] Silicon carbide is a wide bandgap semiconductor material. It has attracted much attention due to its good thermal conductivity, high temperature resistance, high breakdown field, high saturated electron drift velocity and strong radiation resistance. It will become a composite key semiconductor material widely used in light-emitting diode substrates and high-power devices in the future. In the manufacturing and epitaxial growth of next-generation power devices, there are strict requirements for the final surface quality control of SiC single crystal materials. Atomically flat, damage-free and defect-free SiC substrates are crucial. Any micro-defects on the substrate surface may affect the growth results of the epitaxial layer.

[0003] At present, chemical mechanical polishing (CMP) is one of the most effective technical methods to achieve global flattening. However, the ultra-high mechanical hardness and ultra-strong chemical inertness make it difficult for SiC substrates to achieve high removal rates and atomic-level flat surfaces. Currently, ultra-precision polishing of SiC substrates mostly uses chemical mechanical polishing technology that effectively combines surface chemical modification and soft abrasive polishing. CMP technology first uses chemical reactions to modify the surface of SiC substrates to reduce their surface hardness, and then uses the mechanical friction between soft abrasives and the modified layer on the substrate surface to remove the modified layer. Through the continuous alternation of chemical and mechanical actions, the SiC substrate is finally polished to obtain a high-quality surface.

[0004] Specifically, the CMP process in the SiC substrate manufacturing process is mainly divided into rough polishing and fine polishing. Rough polishing process: strong acid polishing liquid (potassium permanganate oxidant, aluminum oxide abrasive) with polyurethane or high hardness non-woven polishing pad. Fine polishing process: alkaline polishing liquid (hydrogen peroxide oxidant, silicon oxide abrasive) with low hardness damping polishing pad.

[0005] For example, CN115418170A discloses an alumina polishing liquid for CMP polishing of SiC substrates, comprising: in parts by mass, 10-20 parts of alumina powder, 5-10 parts of silicon carbide powder, 1-5 parts of a defoaming agent, 1-5 parts of a dispersant, 2-5 parts of a surfactant, 2-3 parts of a pH adjuster, 0.1-0.3 parts of an antioxidant, and 50-100 parts of deionized water, wherein the polishing liquid is alkaline.

[0006] The rough polishing process has a fast polishing rate, but due to the strong oxidizing property of the strongly acidic potassium permanganate, the SiC substrate surface is severely corroded after polishing, and there are a lot of scratches on the C surface when working with a hard pad, which requires fine polishing repair. However, the alkaline polishing liquid currently used for fine polishing has a too slow rate, and it takes a very long time to remove the scratches and surface defects left by the rough polishing. The polishing time is about 1-2 hours, and the polishing cost is too high, which is not suitable for mass production of SiC substrates.

[0007] In summary, it can be seen that in the art, when polishing a substrate, there are still problems such as low polishing efficiency and easy occurrence of surface defects after polishing. Summary of the invention

[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide an abrasive for polishing liquid and a preparation method thereof, a polishing liquid, and a substrate polishing method to solve the problems of low polishing efficiency and easy occurrence of surface defects after polishing when polishing SiC substrates.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides an abrasive grain for a polishing liquid, wherein the abrasive grain for a polishing liquid comprises glucose nanoparticles coated with silicon dioxide;

[0011] The particle size of the abrasive particles used in the polishing liquid is 30-100 nm.

[0012] The polishing liquid abrasive provided by the present invention causes the glucose nanoparticles to lose a hydrogen atom to form a hydroxyl radical under the assistance of ultraviolet light. The hydroxyl radical OH formed subsequently undergoes an oxidation reaction with the SiC substrate to form a softer surface modification layer, thereby reducing the surface hardness and increasing the polishing rate. At the same time, the Mohs hardness of the coated silicon dioxide is higher than the soluble This modified layer can be easily removed by mechanical friction of abrasives, and the hardness of silicon oxide abrasive grains is lower than that of the SiC substrate itself, so the SiC surface will not be scratched during the polishing process.

[0013] In a second aspect, the present invention provides a method for preparing abrasive grains for polishing liquid as described in the first aspect, the preparation method comprising:

[0014] Glucose nanoparticles and silica sol are mixed, and then subjected to gelation and precipitation operations to obtain silica-coated glucose nanoparticles.

[0015] As a preferred technical solution of the present invention, the silica sol is obtained by mixing a silicon agent, a first surfactant and a first solvent.

[0016] Preferably, the mass percentage of the silicon agent in the silica sol is 5-20%.

[0017] Preferably, the mass percentage of the first surfactant in the silica sol is 0.1-0.25%.

[0018] Preferably, the particle size of the glucose nanoparticles is 20-80 nm, preferably 35-60 nm.

[0019] Preferably, the solid-liquid ratio of glucose nanoparticles to silica sol in the mixture is 1:(5-10) g / mL, preferably 1:(6-8).

[0020] As a preferred technical solution of the present invention, ultrasound or stirring is performed during the mixing.

[0021] Preferably, the mixing time is 5-10 min.

[0022] Preferably, acid or base is added during the gelation.

[0023] Preferably, the amount of acid or alkali added in the gelation is 0.1-5%, preferably 0.2-0.3%, of the total mass of the glucose nanoparticles and the silica sol.

[0024] Preferably, the pH of the precipitation operation is 7-10.

[0025] Preferably, the temperature of the precipitation operation is 10-60°C.

[0026] In a third aspect, the present invention provides a polishing liquid, comprising: the abrasive particles for the polishing liquid as described in the first aspect, an oxidizing agent, a second surfactant, a thickener, a pH adjuster and a second solvent.

[0027] As a preferred technical solution of the present invention, the polishing liquid comprises, by mass percentage:

[0028] The polishing liquid contains 1-40% abrasive grains, 0.1-0.5% oxidant, 0.5-2% second surfactant, 0.15-0.4% thickener, and the balance is the second solvent.

[0029] As a preferred technical solution of the present invention, the oxidant includes hydrogen peroxide.

[0030] Preferably, the thickener comprises one or a combination of at least two of hydroxypropyl methylcellulose, sodium carboxymethyl cellulose or polyacrylamide.

[0031] Preferably, the second surfactant comprises one or a combination of at least two of sodium octanoate, potassium octanoate, cetyltrimethylammonium bromide or Triton X-100.

[0032] Preferably, the pH adjuster comprises sodium hydroxide and / or potassium hydroxide.

[0033] In a fourth aspect, the present invention provides a substrate polishing method, the substrate polishing method comprising:

[0034] Mechanochemical polishing is performed using the polishing liquid as described in the third aspect.

[0035] As a preferred technical solution of the present invention, the mechanochemical grinding is assisted by ultraviolet light irradiation.

[0036] Preferably, the wavelength of the ultraviolet light used in the mechanochemical polishing is 300-400 nm.

[0037] Preferably, the power of the ultraviolet light used in the mechanochemical polishing is 10-100 mW.

[0038] As a preferred technical solution of the present invention, the pressure applied during the mechanical chemical grinding is 3-10 psi.

[0039] Preferably, the pressure applied during the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 7-9 psi.

[0040] Preferably, the pressure applied during the mechanochemical polishing when polishing the SiC-C surface of the substrate is 2-5 psi.

[0041] Preferably, the rotation speed of the polishing head in the mechanochemical polishing is 30-120 r / min.

[0042] Preferably, the flow rate of the polishing liquid in the mechanochemical polishing is 50-300 mL / min.

[0043] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0044] (1) The polishing abrasive provided by the present invention can achieve high-speed and high-quality polishing of the Si surface and C surface of the SiC substrate when polishing the substrate. The surface roughness of the SiC wafer after polishing is extremely low, Ra < 0.1nm, and there are no scratches or defects under the AFM field of view. The polishing rate is relatively fast, and the polishing rate of the SiC-Si surface is not less than C surface rate is not less than It takes into account both high surface quality and high removal rate of SiC substrate after polishing.

[0045] (2) The polishing liquid of the present invention is alkaline, and the alkalinity has a weaker corrosive effect on the polishing pad, which solves the problem of slow polishing rate in the current SiC polishing process, prolongs the service life of the polishing pad, improves the polishing efficiency, and can better meet mass production needs. DETAILED DESCRIPTION

[0046] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0047] This embodiment provides an abrasive grain for a polishing liquid, wherein the abrasive grain for a polishing liquid includes glucose nanoparticles coated with silicon dioxide;

[0048] The particle size of the abrasive particles used in the polishing liquid is 30-100 nm.

[0049] The glucose nanoparticles provided by the present invention are easy to generate hydroxyl radicals under conditions such as ultraviolet light, high temperature or chemical oxidants. The present invention mainly causes the glucose nanoparticles to lose a hydrogen atom to form hydroxyl radicals under the auxiliary action of ultraviolet light. The subsequently formed hydroxyl radicals OH react with the SiC substrate to generate a softer surface modification layer, thereby reducing the surface hardness and improving the polishing rate.

[0050] C 6 H 12 O 6 +hν(ultraviolet light)→C 6 H 11 O 5 + OH (1)

[0051]

[0052] The glucose nanoparticles used can react with the SiC substrate under the assistance of ultraviolet light to generate soluble The modified layer is then removed by mechanical friction of soft abrasive particles. However, due to the low hardness of glucose nanoparticles, when they are mixed with the oxidant hydrogen peroxide, a redox reaction occurs, glucose is oxidized to gluconic acid, and hydrogen peroxide is reduced to water.

[0053] C 6 H 12 O 6 + 6H 2 O 2 → 6C 6 H 10 O 7 + 6H 2 O (3)

[0054] When making polishing liquid, this redox reaction will affect the photocatalytic effect of glucose nanoparticles and reduce the polishing rate of SiC. In order to prevent them from undergoing redox reaction and enable the glucose nanoparticles to be used only as abrasive particles, the present invention coats the glucose nanoparticles to prevent the occurrence of redox reaction, thereby preventing them from contacting with hydrogen peroxide and increasing the hardness of the abrasive particles.

[0055] In the present invention, the particle size refers to the aggregates of particles of any particle size within a range, or the aggregates of all particles within a certain particle size range. The particle size of the abrasive particles for the polishing liquid is 30-100nm for exemplary explanation, and other limitations on particle size can be deduced by analogy, such as the aggregates of 30nm particles, 40nm particles, 50nm particles, 60nm particles, 70nm particles, 80nm particles, etc.; for example, the aggregates of all particles in the range of 30-50nm are used, for example, the aggregates of all particles in the range of 40-60nm are used, for example, the aggregates of all particles in the range of 50-70nm are used, for example, the aggregates of all particles in the range of 60-80nm are used, for example, the aggregates of all particles in the range of 70-100nm are used, for example, the aggregates of all particles in the range of 30-80nm are used, etc.

[0056] Furthermore, this embodiment provides a method for preparing the abrasive grains for the polishing liquid, the preparation method comprising:

[0057] Glucose nanoparticles and silica sol are mixed, and then subjected to gelation and precipitation operations to obtain silica-coated glucose nanoparticles.

[0058] The silica sol is obtained by mixing a silicon agent, a first surfactant and a first solvent.

[0059] Among them, the mass percentage of silicon agent in the silica sol is 5-20%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, etc., but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0060] In the present invention, the silicon agent used includes silicate or sodium silicate, and being within a specific range is helpful to achieve an effective coating effect.

[0061] Among them, the mass percentage of the first surfactant in the silica sol is 0.1-0.25%, for example, it can be 0.1%, 0.12%, 0.14%, 0.16%, 0.18%, 0.2%, 0.22%, 0.24% or 0.25%, but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0062] Among them, the first surfactant includes one or a combination of at least two of sodium octanoate, potassium octanoate, hexadecyltrimethylammonium bromide or Triton X-100, which are commonly used surfactants in the art. They can reduce the surface tension of the liquid surface, form colloids in the sol, stabilize the sol, and promote the uniform coating of silica on the surface of glucose nanoparticles.

[0063] In the present invention, an appropriate amount of surfactant can help to evenly disperse the glucose nanoparticles in the sol, and at the same time adjust the viscosity and surface tension of the sol, which is beneficial to the subsequent coating process.

[0064] Wherein, the first solvent includes water and other commonly used solvents in the art.

[0065] The particle size of the glucose nanoparticles is 20-80 nm, preferably 35-60 nm, and aggregates of particles with any particle size within the range can be selected, or aggregates of all particles within a certain particle size range can be used.

[0066] In the present invention, the particle size of the glucose nanoparticles can be selected according to the above description of the particle size.

[0067] In the present invention, the glucose nanoparticles can be selected from commercially available glucose nanoparticles that meet the specified requirements, or can be selected from glucose nanoparticles prepared according to the prior art. An exemplary method for preparing glucose nanoparticles is as follows:

[0068] 1. Mix the glucose solution with an equal volume of chloroform and add a surfactant, followed by ultrasonic treatment to form a stable emulsion.

[0069] 2. Evaporate the emulsion to remove the chloroform and retain the glucose nanoparticles.

[0070] 3. The ultrasonically treated solution is centrifuged to remove large particles and impurities, and the desired glucose nanoparticles are separated and washed with deionized water to remove residual surfactants and solvents.

[0071] 4. The separated glucose nanoparticles are vacuum dried.

[0072] Among them, the mass concentration of the glucose solution used in the preparation process of glucose nanoparticles is 8-15%, for example, it can be 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5% or 15%, etc., but is not limited to the listed values, and other values ​​not listed within this range also meet the requirements.

[0073] Among them, the amount of surfactant added in the preparation of glucose nanoparticles is 0.2-1% of the total mass of the glucose solution and chloroform, for example, it can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc., but is not limited to the listed values, and other values ​​not listed within this range also meet the requirements.

[0074] Among them, the surfactants used in the preparation of glucose nanoparticles include PVA and other commonly used surfactants for preparing nanoparticles in the art.

[0075] The ultrasonic power in the ultrasonic treatment is 150-250 W, for example, 150 W, 160 W, 180 W, 200 W, 220 W, 240 W or 250 W, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0076] The ultrasonic treatment time is 5-10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0077] The evaporation temperature is 30-40°C, for example, 30°C, 32°C, 34°C, 36°C, 38°C, or 40°C, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0078] The evaporation time is ≥ 24 h, for example, it can be 24 h, 25 h, 26 h, 28 h, 29 h or 30 h, but is not limited to the listed values. Other values ​​not listed within the range also meet the requirements.

[0079] The vacuum drying temperature is 50-70°C, for example, it can be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0080] The vacuum drying time is 3-5 h, for example, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0081] Among them, the solid-to-liquid ratio of glucose nanoparticles and silica sol in the mixture is 1:(5-10) g / mL, for example, it can be 1:6, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5 or 1:10, but is not limited to the listed values. Other unlisted values ​​within this range also meet the requirements, preferably 1:(6-8).

[0082] Wherein, ultrasound or stirring is performed during the mixing.

[0083] In the present invention, the particles are uniformly dispersed by ultrasonic treatment or stirring during the mixing process to avoid particle agglomeration and uneven coating layer formation.

[0084] The mixing time is 5-10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0085] Wherein, acid or alkali is added during the gelation.

[0086] Among them, the added amount of acid or alkali in the gelation is 0.1-5% of the total mass of glucose nanoparticles and silica sol, for example, it can be 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., but is not limited to the listed values. Other unlisted values ​​within this range also meet the requirements, preferably 0.2-0.3%.

[0087] The pH value of the precipitation operation is 7-10, for example, it can be 7, 7.5, 8, 8.5, 9, 9.5 or 10, but is not limited to the listed values. Other values ​​not listed in this range also meet the requirements.

[0088] Among them, the temperature of the precipitation operation is 10-60°C, for example, it can be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0089] Furthermore, the present invention provides a polishing liquid, the polishing liquid comprising:

[0090] The abrasive particles, oxidizing agent, second surfactant, thickener, pH adjuster and second solvent are as described above.

[0091] Wherein, the polishing liquid comprises, by mass percentage:

[0092] As mentioned above, 1-40% abrasive, 0.1-0.5% oxidant, 0.5-2% second surfactant, 0.15-0.4% thickener, and the balance is the second solvent;

[0093] The pH value of the polishing liquid is 7-10.

[0094] An exemplary polishing liquid preparation process is as follows: the ingredients are prepared according to the mass percentage formula, and then the oxidant is dissolved in water and stirred; then a certain amount of abrasive, surfactant, and thickener are added to the solution, and deionized water is added to the required volume to obtain an abrasive suspension of a certain concentration; finally, a pH adjuster is added to adjust to the required pH value and continuously stirred to obtain a polishing liquid.

[0095] In the present invention, the abrasive content in the polishing liquid is 1-40% by mass, for example, it can be 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38% or 40%, etc., but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0096] In the present invention, the oxidant in the polishing liquid is 0.1-0.5% by mass, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%, etc., but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0097] In the present invention, the second surfactant in the polishing liquid is 0.5-2% by mass, for example, it can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.6%, 1.7%, 1.8%, 1.9% or 2%, etc., but is not limited to the listed values, and other values ​​not listed within this range also meet the requirements.

[0098] In the present invention, the mass percentage of the thickener in the polishing liquid is 0.15-0.4%, for example, it can be 0.15%, 0.16%, 0.18%, 0.2%, 0.22%, 0.24%, 0.26%, 0.28%, 0.3%, 0.32%, 0.34%, 0.36%, 0.38% or 0.4%, etc., but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0099] In the present invention, the pH value of the polishing liquid is 7-10, for example, it can be 7, 7.5, 8, 8.5, 9, 9.5 or 10, but is not limited to the listed values, and other values ​​not listed in the range also meet the requirements.

[0100] Wherein, the oxidant comprises hydrogen peroxide.

[0101] Wherein, the thickener includes one or a combination of at least two of hydroxypropyl methylcellulose, sodium carboxymethyl cellulose or polyacrylamide.

[0102] In the present invention, the thickener is used to increase the viscosity of the polishing liquid, effectively disperse the abrasive particles evenly in the polishing liquid, and improve the durability and uniformity of the polishing effect.

[0103] Wherein, the second surfactant includes one or a combination of at least two of sodium octanoate, potassium octanoate, hexadecyltrimethylammonium bromide or TritonX-100.

[0104] In the present invention, the second surfactant has good emulsification and dispersing effects, which helps the abrasive particles to be evenly dispersed in the liquid, thereby improving the working efficiency and uniformity of the polishing liquid. An appropriate amount of surfactant can effectively enhance the dispersibility and stability of the abrasive particles in the liquid, while too high a concentration may cause foaming and affect the polishing effect.

[0105] In the present invention, the pH value of the polishing liquid is adjusted by an acid or alkali commonly used in the art.

[0106] Wherein, the pH adjuster includes sodium hydroxide and / or potassium hydroxide.

[0107] In the present invention, the second solvent includes water and other commonly used solvents in the art.

[0108] Furthermore, this embodiment provides a substrate polishing method, the substrate polishing method comprising:

[0109] The polishing liquid is used to perform mechanical chemical polishing.

[0110] Specifically, the SiC wafer to be polished is fixed in the polishing head, and pressure is applied to the back of the polishing head, so that the substrate in the polishing head contacts the polishing pad and performs rotation and translation motion, and the polishing liquid is transported to the substrate surface by the polishing pad. During the polishing process, the control system controls the polishing pressure, polishing liquid flow, polishing speed, and polishing time to complete the removal of wafer surface material and realize the polishing process of the wafer. In ultraviolet photocatalytic assisted chemical mechanical polishing, an ultraviolet light generator is used to irradiate the glucose nanoparticles in the polishing liquid to cause a photocatalytic reaction, thereby generating more hydroxyl radicals to increase the removal rate of the SiC substrate.

[0111] Wherein, the mechanical chemical grinding is assisted by ultraviolet light irradiation.

[0112] Among them, the wavelength of the ultraviolet light used in the mechanochemical polishing is 300-400nm, for example, it can be 300nm, 310nm, 320nm, 330nm, 340nm, 350nm, 360nm, 370nm, 380nm, 390nm or 400nm, but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0113] Among them, the power of the ultraviolet light used in the mechanochemical polishing is 10-100mW, for example, it can be 10mW, 20mW, 30mW, 40mW, 50mW, 60mW, 70mW, 80mW, 90mW or 100mW, but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0114] In the present invention, a reasonable power can effectively excite glucose nanoparticles, but will not cause photodegradation or thermal effects caused by overexcitation. Too high power (>100mW) may cause overexcitation of glucose nanoparticles, triggering photodegradation or thermal effects, and reducing the photocatalytic efficiency. While too low power (<5mW) will not be sufficiently excited, hydroxyl radicals cannot be effectively generated, and the photocatalytic efficiency is low.

[0115] The pressure applied during the mechanical chemical polishing is 3-10 psi, for example, 3 psi, 4 psi, 5 psi, 6 psi, 7 psi, 8 psi, 9 psi or 10 psi, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0116] Among them, the pressure applied in the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 7-9psi, for example, it can be 7psi, 7.2psi, 7.4psi, 7.6psi, 7.8psi, 8psi, 8.2psi, 8.4psi, 8.6psi, 8.8psi or 9psi, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0117] Among them, the pressure applied in the mechanochemical polishing when polishing the SiC-C surface of the substrate is 2-5psi, for example, it can be 2psi, 2.2psi, 2.4psi, 2.6psi, 2.8psi, 3psi, 3.2psi, 3.4psi, 3.6psi, 3.8psi, 4psi, 4.2psi, 4.4psi, 4.6psi, 4.8psi or 5psi, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0118] Among them, the rotation speed of the polishing head in the mechanochemical grinding is 30-120r / min, for example, it can be 30r / min, 40r / min, 50r / min, 60r / min, 70r / min, 80r / min, 90r / min, 100r / min, 110r / min or 120r / min, but is not limited to the listed values, and other values ​​not listed in this range also meet the requirements.

[0119] Wherein, the flow rate of the polishing liquid in the mechanochemical polishing is 50-300mL / min, for example, it can be 50mL / min, 60mL / min, 70mL / min, 80mL / min, 90mL / min, 100mL / min, 120mL / min, 140mL / min, 160mL / min, 180mL / min, 200mL / min, 220mL / min, 240mL / min, 260mL / min, 280mL / min or 300mL / min, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0120] In the present invention, the time of the mechanical chemical polishing can be reasonably selected according to the actual processing needs. For example, according to the processing requirements of the substrate in the art, the time can be selected to be 2-30 minutes, for example, it can be 2 minutes, 4 minutes, 6 minutes, 8 minutes, 10 minutes, 12 minutes, 14 minutes, 16 minutes, 18 minutes or 20 minutes, etc., but it is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0121] In the present invention, a damping material polishing pad can be optionally used in conjunction with mechanical chemical grinding to perform SiC fine polishing operations, which greatly prolongs the life of the polishing pad while improving the polishing removal rate and substrate surface quality, improves the polishing efficiency, and can better meet mass production needs.

[0122] Further, in order to illustrate the good polishing effect that can be achieved by the abrasive particles for the polishing liquid provided by the present invention, a detailed description is given by way of actual examples, as follows:

[0123] Example 1

[0124] This embodiment provides a substrate polishing method, specifically for polishing a SiC substrate, the process is as follows:

[0125] Mechanical chemical grinding with polishing fluid;

[0126] The polishing liquid comprises, by weight percentage:

[0127] The polishing liquid contains 15% abrasive, 0.2% oxidant, 1.2% second surfactant, 0.25% thickener, and the balance is solvent water;

[0128] The particle size of the abrasive particles used in the polishing liquid is 40-60 nm;

[0129] The preparation process of abrasive particles for polishing liquid is as follows:

[0130] Glucose nanoparticles and silica sol are mixed, and then gelation and precipitation operations are performed to obtain silica-coated glucose nanoparticles; the silica sol is obtained by mixing a silicon agent, a first surfactant and solvent water; the mass percentage of the silicon agent in the silica sol is 10%; the mass percentage of the first surfactant in the silica sol is 0.2%; the particle size of the glucose nanoparticles is 35-50nm; the solid-liquid ratio of the glucose nanoparticles and the silica sol in the mixing is 1:6 g / mL; ultrasound is performed during the mixing (ultrasound power is 180W); the mixing time is 8min; acid or alkali is added during the gelation; the amount of acid or alkali added in the gelation is 0.2% of the total mass of the glucose nanoparticles and the silica sol; the pH of the precipitation operation is 8; the temperature of the precipitation operation is 30°C;

[0131] The oxidant is hydrogen peroxide; the thickener is sodium carboxymethyl cellulose; the second surfactant is sodium octanoate; the pH value adjuster is sodium hydroxide and / or potassium hydroxide;

[0132] The mechanochemical polishing is assisted by ultraviolet light irradiation; the wavelength of the ultraviolet light used in the mechanochemical polishing is 350nm; the power of the ultraviolet light used in the mechanochemical polishing is 20mW; the pressure applied in the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 8psi; the pressure applied in the mechanochemical polishing when polishing the SiC-C surface of the substrate is 3psi; the rotation speed of the polishing head in the mechanochemical polishing is 70r / min; the flow rate of the polishing liquid in the mechanochemical polishing is 120mL / min.

[0133] Example 2

[0134] This embodiment provides a substrate polishing method, specifically for polishing a SiC substrate, the process is as follows:

[0135] Mechanical chemical grinding with polishing fluid;

[0136] The polishing liquid comprises, by weight percentage:

[0137] The polishing liquid contains 25% abrasive, 0.3% oxidant, 1.5% second surfactant, 0.3% thickener, and the balance is solvent water;

[0138] The particle size of the abrasive particles used in the polishing liquid is 55-80nm;

[0139] The preparation process of abrasive particles for polishing liquid is as follows:

[0140] Glucose nanoparticles and silica sol are mixed, and then gelation and precipitation are performed to obtain glucose nanoparticles coated with silica; the silica sol is obtained by mixing a silicon agent, a first surfactant and solvent water; the mass percentage of the silicon agent in the silica sol is 15%; the mass percentage of the first surfactant in the silica sol is 0.15%; the particle size of the glucose nanoparticles is 40-60nm; the solid-liquid ratio of the glucose nanoparticles and the silica sol in the mixing is 1:7 g / mL; stirring is performed during the mixing (stirring rate is 200r / min); the mixing time is 8min; acid or alkali is added during the gelation; the amount of acid or alkali added in the gelation is 0.3% of the total mass of the glucose nanoparticles and the silica sol; the pH of the precipitation operation is 9; the temperature of the precipitation operation is 40°C;

[0141] The oxidant is hydrogen peroxide; the thickener is hydroxypropyl methylcellulose; the second surfactant is sodium octanoate; the pH adjuster is sodium hydroxide;

[0142] The mechanochemical polishing is assisted by ultraviolet light irradiation; the wavelength of the ultraviolet light used in the mechanochemical polishing is 380nm; the power of the ultraviolet light used in the mechanochemical polishing is 50mW; the pressure applied in the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 8.5psi; the pressure applied in the mechanochemical polishing when polishing the SiC-C surface of the substrate is 4psi; the rotation speed of the polishing head in the mechanochemical polishing is 90r / min; the flow rate of the polishing liquid in the mechanochemical polishing is 80mL / min.

[0143] Example 3

[0144] This embodiment provides a substrate polishing method, specifically for polishing a SiC substrate, the process is as follows:

[0145] Mechanical chemical grinding with polishing fluid;

[0146] The polishing liquid comprises, by weight percentage:

[0147] The polishing liquid contains 1% abrasive, 0.1% oxidant, 2% second surfactant, 0.15% thickener, and the balance is solvent water;

[0148] The particle size of the abrasive particles used in the polishing liquid is 50-80 nm;

[0149] The preparation process of abrasive particles for polishing liquid is as follows:

[0150] Glucose nanoparticles and silica sol are mixed, and then gelation and precipitation operations are performed to obtain silica-coated glucose nanoparticles; the silica sol is obtained by mixing a silicon agent, a first surfactant and solvent water; the mass percentage of the silicon agent in the silica sol is 5%; the mass percentage of the first surfactant in the silica sol is 0.1%; the particle size of the glucose nanoparticles is 20-40nm; the solid-liquid ratio of the glucose nanoparticles and the silica sol in the mixing is 1:5 g / mL; ultrasound is performed during the mixing (ultrasound power is 180W); the mixing time is 8min; acid or alkali is added during the gelation; the amount of acid or alkali added in the gelation is 0.1% of the total mass of the glucose nanoparticles and the silica sol; the pH of the precipitation operation is 10; the temperature of the precipitation operation is 60°C;

[0151] The oxidant includes hydrogen peroxide; the thickener includes polyacrylamide; the second surfactant is potassium octanoate; the pH adjuster is potassium hydroxide;

[0152] The mechanochemical polishing is assisted by ultraviolet light irradiation; the wavelength of the ultraviolet light used in the mechanochemical polishing is 300nm; the power of the ultraviolet light used in the mechanochemical polishing is 10mW; the pressure applied in the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 7psi; the pressure applied in the mechanochemical polishing when polishing the SiC-C surface of the substrate is 5psi; the rotation speed of the polishing head in the mechanochemical polishing is 60r / min; the flow rate of the polishing liquid in the mechanochemical polishing is 300mL / min.

[0153] Example 4

[0154] This embodiment provides a substrate polishing method, specifically for polishing a SiC substrate, the process is as follows:

[0155] Mechanical chemical grinding with polishing fluid;

[0156] The polishing liquid comprises, by weight percentage:

[0157] The polishing liquid comprises 40% abrasive, 0.5% oxidant, 0.5% second surfactant, 0.4% thickener, and the balance is solvent water;

[0158] The particle size of the abrasive particles used in the polishing liquid is 80-100 nm;

[0159] The preparation process of abrasive particles for polishing liquid is as follows:

[0160] Glucose nanoparticles and silica sol are mixed, and then gelation and precipitation are performed to obtain glucose nanoparticles coated with silica; the silica sol is obtained by mixing a silicon agent, a first surfactant and solvent water; the mass percentage of the silicon agent in the silica sol is 20%; the mass percentage of the first surfactant in the silica sol is 0.25%; the particle size of the glucose nanoparticles is 70-80nm; the solid-liquid ratio of the glucose nanoparticles and the silica sol in the mixing is 1:10 g / mL; stirring is performed during the mixing (stirring rate is 200r / min); the mixing time is 10min; acid or alkali is added during the gelation; the amount of acid or alkali added in the gelation is 5% of the total mass of the glucose nanoparticles and the silica sol; the pH of the precipitation operation is 7; the temperature of the precipitation operation is 10°C;

[0161] The oxidant is hydrogen peroxide; the thickener is hydroxypropyl methylcellulose; the second surfactant is potassium octanoate; the pH adjuster is potassium hydroxide;

[0162] The mechanochemical polishing is assisted by ultraviolet light irradiation; the wavelength of the ultraviolet light used in the mechanochemical polishing is 400nm; the power of the ultraviolet light used in the mechanochemical polishing is 100mW; the pressure applied in the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 9psi; the pressure applied in the mechanochemical polishing when polishing the SiC-C surface of the substrate is 2psi; the rotation speed of the polishing head in the mechanochemical polishing is 120r / min; the flow rate of the polishing liquid in the mechanochemical polishing is 50mL / min.

[0163] Example 5

[0164] The only difference from Example 1 is that glucose nanoparticles are directly used as the abrasive particles.

[0165] Example 6

[0166] The only difference from Example 1 is that the mass percentage of the silicon agent in the silica sol is 25%.

[0167] Example 7

[0168] The only difference from Example 1 is that the mass percentage of the silicon agent in the silica sol is 2%.

[0169] Example 8

[0170] The only difference from Example 1 is that the mass percentage of the first surfactant in the silica sol is 0.05%.

[0171] Example 9

[0172] The only difference from Example 1 is that the mass percentage of the first surfactant in the silica sol is 0.3%.

[0173] Example 10

[0174] The only difference from Example 1 is that the pH value of the precipitation operation is 5.

[0175] Embodiment 11

[0176] The only difference from Example 1 is that the pH value of the precipitation operation is 13.

[0177] Example 12

[0178] The only difference from Example 1 is that the ultraviolet light power used is 5 mW.

[0179] Example 13

[0180] The only difference from Example 1 is that the ultraviolet light power used is 110 mW, photodegradation occurs, and the photocatalytic efficiency is reduced, thereby reducing the polishing rate of SiC.

[0181] In the above embodiment, the preparation process of the glucose nanoparticles used is as follows:

[0182] 1. Dissolve 1000 mg of glucose in 10 mL of water to form a 10% glucose solution.

[0183] 2. The glucose solution was mixed with an equal volume of chloroform, and 0.5% PVA was added as a surfactant, and then the mixture was emulsified for 8 minutes using an ultrasonic processor to form a stable emulsion, wherein the ultrasonic power was 200 W and the processing time was 8 minutes.

[0184] 3. Place the emulsion in a 37°C incubator to allow the chloroform to evaporate for 24 h, leaving the glucose nanoparticles.

[0185] 4. The ultrasonically treated solution was centrifuged at a speed of 5000 r / min for 30 minutes, and then washed with deionized water to remove residual surfactant and solvent.

[0186] 5. The separated glucose nanoparticles were vacuum dried at 60°C for 4 h.

[0187] Table 1

[0188]

[0189]

[0190] Combined with Table 1, comparing Example 1 with Example 5, the abrasive particles are directly selected as glucose nanoparticles without silicon oxide coating. Since the hardness of glucose nanoparticles is extremely low, and when directly mixed with hydrogen peroxide, a redox reaction will occur, which affects the photocatalytic effect of the particles, thereby greatly reducing the polishing rate of SiC.

[0191] By comparing Example 1 with Examples 6 and 7, when the mass percentage of the silicon agent in the silica sol is too high, the sol may be too thick, resulting in uneven or too thick coating layer, which may lower the polishing rate to a certain extent; and when the mass percentage of the silicon agent in the silica sol is too low, the sol may not be fully formed and cannot be effectively coated on the particle surface, resulting in unstable coating layer quality, causing some glucose nanoparticles to be exposed, thereby reducing the SiC polishing rate.

[0192] By comparing Example 1 with Examples 8 and 9, when the mass percentage of the first surfactant in the silica sol is too high, the sol may be too stable, making it difficult to form a coating layer, affecting the properties or stability of the particles after coating, the polishing rate is low, and the roughness is higher than that of Example 1; when the mass percentage of the first surfactant in the silica sol is too high, the interaction between the particles may be weakened, making it impossible for the sol to be effectively coated on the surface of the particles, so that some glucose nanoparticles are exposed to the outside, reducing the SiC polishing rate.

[0193] By comparing Example 1 with Examples 10 and 11, when the pH value of the precipitation operation is higher than the pH in the optimal range, the solution is too alkaline, which will cause excessive precipitation or aggregation of silica, thereby forming an uneven and too thick coating layer. If the coating layer is too thick, the UV photocatalytic effect will be weakened, the polishing rate will be reduced, the coating layer will be uneven, and the polishing uniformity and roughness will be high. When the pH value of the precipitation operation is lower than the pH in the optimal range, the solution is too acidic, and the interaction between the glucose nanoparticles and silica is weakened. When the pH is less than 7, the precipitation reaction will be slow or even unable to proceed, and a complete silica coating layer cannot be formed, so that part of the glucose nanoparticles are exposed to the outside, reducing the SiC polishing rate.

[0194] By comparing Example 1 with Examples 12 and 13, when the ultraviolet light power is too high, it will cause over-excitation of glucose nanoparticles, trigger photodegradation or thermal effect, reduce photocatalytic efficiency, and thus cause the SiC polishing rate to become lower; when the ultraviolet light power is too low, the light excitation effect is insufficient, and hydroxyl radicals cannot be generated, which is consistent with the operating effect of the current alkaline silicon oxide abrasive polishing liquid, and the SiC polishing rate is low.

[0195] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0196] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0197] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0198] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A polishing liquid abrasive grain, characterized in that: The abrasive particles for the polishing liquid include glucose nanoparticles coated with silicon dioxide; The particle size of the abrasive particles used in the polishing liquid is 30-100 nm.

2. A method for preparing abrasive particles for polishing liquid as claimed in claim 1, characterized in that: The preparation method comprises: Glucose nanoparticles and silica sol are mixed, and then subjected to gelation and precipitation operations to obtain silica-coated glucose nanoparticles.

3. The preparation method according to claim 2, characterized in that: The silica sol is obtained by mixing a silicon agent, a first surfactant and a first solvent; Preferably, the mass percentage of the silicon agent in the silica sol is 5-20%; Preferably, the mass percentage of the first surfactant in the silica sol is 0.1-0.25%; Preferably, the particle size of the glucose nanoparticles is 20-80 nm, preferably 35-60 nm; Preferably, the solid-liquid ratio of glucose nanoparticles to silica sol in the mixture is 1:(5-10) g / mL, preferably 1:(6-8).

4. The preparation method according to any one of claims 2 to 4, characterized in that: Performing ultrasound or stirring during the mixing; Preferably, the mixing time is 5-10 min; Preferably, an acid or a base is added during the gelation; Preferably, the amount of acid or base added in the gelation is 0.1-5%, preferably 0.2-0.3%, of the total mass of the glucose nanoparticles and the silica sol; Preferably, the pH of the precipitation operation is 7-10; Preferably, the temperature of the precipitation operation is 10-60°C.

5. A polishing liquid, characterized in that: The polishing liquid comprises: the abrasive for polishing liquid as claimed in claim 1, an oxidizing agent, a second surfactant, a thickener, a pH adjuster and a second solvent.

6. The polishing liquid according to claim 5, characterized in that: The polishing liquid comprises, by weight percentage: The polishing liquid contains 1-40% abrasive grains, 0.1-0.5% oxidant, 0.5-2% second surfactant, 0.15-0.4% thickener, and the balance is the second solvent.

7. The polishing liquid according to claim 5 or 6, characterized in that: The oxidant includes hydrogen peroxide; Preferably, the thickener comprises one or a combination of at least two of hydroxypropyl methylcellulose, sodium carboxymethyl cellulose or polyacrylamide; Preferably, the second surfactant comprises one or a combination of at least two of sodium octanoate, potassium octanoate, hexadecyltrimethylammonium bromide or TritonX-100; Preferably, the pH adjuster comprises sodium hydroxide and / or potassium hydroxide.

8. A substrate polishing method, characterized in that: The substrate polishing method comprises: Mechanochemical polishing is performed using the polishing liquid as described in any one of claims 5 to 7.

9. The substrate polishing method according to claim 8, characterized in that: The mechanochemical grinding is supplemented by ultraviolet light irradiation; Preferably, the wavelength of the ultraviolet light used in the mechanochemical grinding is 300-400 nm; Preferably, the power of the ultraviolet light used in the mechanochemical polishing is 10-100 mW.

10. The substrate polishing method according to claim 8 or 9, characterized in that: The pressure applied during the mechanochemical grinding is 3-10 psi; Preferably, the pressure applied during the mechanochemical polishing when polishing the SiC-Si surface of the substrate is 7-9 psi; Preferably, the pressure applied in the mechanochemical polishing when polishing the SiC-C surface of the substrate is 2-5 psi; Preferably, the rotation speed of the polishing head in the mechanochemical polishing is 30-120 r / min; Preferably, the flow rate of the polishing liquid in the mechanochemical polishing is 50-300 mL / min.