Modified coal tar and modification separation method thereof

By carrying out ring-enhancing modification treatment on coal tar, the single-ring and double-ring structures are modified to three or more rings, which solves the limitations of these structures in coal tar on the production of high-density fuel, significantly improves the density and calorific value of the fuel, and achieves High value-added utilization of coal tar and production of high-density fuel.

CN118725890APending Publication Date: 2024-10-01XI'AN PETROLEUM UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093441.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Coal tar contains single-ring and double-ring structures, which is not conducive to the production of high-density fuel and limits its utilization value.

Method used

2,5-Dimethylfuran is used as a modifier to perform a ring-enhancing modification reaction with coal tar, and a Lewis acid catalyst and dichloromethane solvent are used to modify the monocyclic and bicyclic structures to more than three rings through the Diels-Alder reaction. structure, and separate impurities through extraction and rotary evaporation to obtain modified coal tar.

Benefits of technology

It significantly increases the content of three-ring or higher components in modified coal tar, increases the density and volume calorific value, produces high-density fuel with excellent performance, and realizes the high value-added utilization of coal tar, with simple process and high safety. , low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987206090000051
    Figure BDA0004987206090000051
  • Figure BDA0004987206090000081
    Figure BDA0004987206090000081
  • Figure BDA0004987206090000082
    Figure BDA0004987206090000082
Patent Text Reader

Abstract

The invention discloses modified coal tar and a modification separation method thereof, and the method comprises the following steps: mixing coal tar, a modifier, a solvent and a catalyst, and carrying out a ring-increasing modification reaction to obtain a first crude product, the modifier adopts 2, 5-dimethylfuran, the mass ratio of the coal tar to the modifier is 1: (1-2), and the solvent is 1: (1-2); the ring increasing modification reaction of the first crude product is terminated to obtain a second crude product, the second crude product is subjected to extraction and rotary evaporation to separate impurities, and the modified coal tar is obtained, and the impurities comprise a catalyst and a solvent. According to the method, the coal tar distillate oil is subjected to ring-increasing modification treatment by using the modifier for the first time, the content of components with more than three rings in the coal tar distillate oil is increased by about 20%, the density and the volume calorific value are remarkably increased, and the problem of density reduction caused by hydrotreatment can be remarkably relieved, so that the high-density fuel with excellent performance is produced; meanwhile, the yield of high-density fuel can be greatly improved, and high-added-value utilization of coal tar is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coal tar, and in particular relates to a modified coal tar and a modification and separation method thereof. Background Art

[0002] Coal tar is a by-product of the coal coking process. It is a black or dark brown viscous liquid with a pungent odor at room temperature. It can be divided into low-temperature coal tar, medium-temperature coal tar and high-temperature coal tar according to the distillation temperature. At present, coal tar is mainly used to separate basic chemical raw materials or used as fuel through processing. With the continuous advancement of technology and people's increasing attention to environmental issues, coal tar is no longer used directly as fuel, but is produced through hydrogenation to produce gasoline and diesel. However, this method cannot give full play to the utilization value of coal tar.

[0003] From the composition point of view, the biggest difference between coal tar and crude oil is that it contains a large number of polycyclic and condensed ring compounds, so its density and volume calorific value are significantly greater than crude oil. This special composition is very consistent with the performance requirements of high-density aviation fuel; and with the rapid development of the aerospace industry, the market demand for high-density fuel is also increasing. Therefore, the use of coal tar to prepare high-density fuel not only meets market demand, but also can achieve high added value utilization of coal tar. However, coal tar also contains a certain amount of single-ring and double-ring structures, which is not conducive to the production of high-density fuel and restricts the utilization of coal tar to a certain extent. Therefore, it is necessary to process coal tar and modify single-ring and double-ring structures into polycyclic structures to remove these unfavorable factors. Summary of the invention

[0004] In order to overcome the problem that coal tar contains single-ring and double-ring structures which are not conducive to the production of high-density fuel, the present invention provides a modified coal tar and a modification and separation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] A modification and separation method for modified coal tar comprises the following steps: coal tar, a modifier, a solvent and a catalyst are mixed to carry out a ring-increasing modification reaction to obtain a first crude product, the modifier is 2,5-dimethylfuran, the mass ratio of coal tar to the modifier is 1:(1-2), the ring-increasing modification reaction of the first crude product is terminated to obtain a second crude product, and the second crude product is separated from impurities by extraction and rotary evaporation to obtain modified coal tar, the impurities include a catalyst and a solvent.

[0007] Furthermore, the catalyst is Lewis acid, the amount of the catalyst is 5% to 10% of the mass of the coal tar, the solvent is dichloromethane, and the volume ratio of the coal tar to the solvent is 1: (1 to 2).

[0008] Furthermore, the reaction temperature for the mixed ring-addition modification reaction is 20 to 120°C.

[0009] Furthermore, the extraction is specifically as follows: the second crude product is mixed with an extractant for extraction, the extractant is dichloromethane, the volume ratio of the second crude product to the extractant is 1:1, and the extraction time is 5 to 30 minutes.

[0010] Furthermore, the first crude product is mixed with a hydrochloric acid solution to obtain a second crude product, and the mass percentage concentration of the hydrochloric acid solution is 10%.

[0011] Furthermore, coal tar is composed of 12% to 20% straight-chain alkanes, 20% to 26% monocyclic, 40% to 50% bicyclic and 10% to 20% tricyclic and above compounds.

[0012] Furthermore, the solvent is dichloromethane, and the catalyst is anhydrous aluminum chloride, anhydrous ferric chloride, anhydrous tin tetrachloride or anhydrous boron trifluoride.

[0013] Furthermore, the reaction pressure of the mixing is 101.325 kPa, the reaction time of the mixing is 6 to 24 h, and the stirring rate of the mixing is 200 to 300 rpm / min.

[0014] Furthermore, the temperature of the rotary evaporation is 30-40° C., the speed of the rotary evaporation is set to 50-80 rpm / min, and the rotary evaporation is stopped after no bubbles are generated.

[0015] A modified coal tar is prepared by adopting the modified separation method of the modified coal tar.

[0016] Compared with the prior art, the present invention has the following beneficial technical effects:

[0017] The present invention proposes a modified separation method for modified coal tar, which uses a modifier to perform ring-increasing modification on coal tar fraction oil for the first time, thereby increasing the content of components with three rings or more in the coal tar fraction oil by about 20%, significantly increasing the density and volume calorific value, and significantly alleviating the problem of density reduction caused by hydrogenation treatment, thereby producing high-density fuel with excellent performance; at the same time, it can greatly improve the yield of high-density fuel and realize high added value utilization of coal tar.

[0018] The invention provides a modified separation method of modified coal tar, using coal tar as raw material, which has a wide source, low production cost, high product added value, good economic benefits, simple process, easy to meet process conditions, low risk factor in the operation process, and high safety. DETAILED DESCRIPTION

[0019] The present invention is described in further detail below:

[0020] A modified separation method for modified coal tar comprises the following steps:

[0021] Step 1: coal tar, a modifier, a solvent and a catalyst are put into a reactor and mixed evenly, wherein the modifier is 2,5-dimethylfuran, and a Diels-Alder reaction is performed under the action of the catalyst to perform ring-addition modification;

[0022] The Diels-Alder reaction, also known as the Diels-Alder reaction or diene synthesis reaction, is a very important cycloaddition reaction in organic chemistry.

[0023] Step 2: extract and purify the crude product after ring addition and modification to separate impurities such as catalyst and solvent.

[0024] The composition of coal tar should be 12% to 20% straight-chain alkanes, 20% to 26% monocyclic, 40% to 50% bicyclic and 10% to 20% tricyclic and above compounds; the mass ratio of coal tar to modifier is 1:1 to 2.

[0025] The reaction pressure of the ring-addition modification reaction in step 1 is 101.325 kPa, the reaction temperature is 20-120° C., the reaction time is 6-24 h, and the magnetic stirring rate during the reaction is 200-300 rpm / min.

[0026] The reaction catalyst is a Lewis acid catalyst, and the preferred catalyst is AlCl 3 The amount of catalyst used is 5 to 10% of the mass of coal tar.

[0027] The reaction solvent is dichloromethane, and the volume ratio of coal tar to the solvent is 1:1-2.

[0028] Before separation and purification of the product, the reaction needs to be terminated with 10% hydrochloric acid solution. This step is carried out in a pear-shaped flask and lasts for 10 minutes.

[0029] The extraction process is carried out in a separatory funnel, the extractant is dichloromethane, the volume ratio of the extractant to the product in the pear-shaped bottle is 1:1, and the extraction time is 5 to 30 minutes.

[0030] The rotary evaporation process was carried out in a rotary evaporator at a temperature of 30-40°C and a rotation speed of 50-80 rpm / min. The experiment was stopped when no bubbles were generated.

[0031] The present invention is further described in detail below in conjunction with embodiments:

[0032] Example 1

[0033] In this embodiment, methylnaphthalene simulated coal tar fraction oil was used for reaction, and the implementation process is as follows:

[0034] Weigh 10g of methylnaphthalene, 10g of 2,5-dimethylfuran and 20ml of dichloromethane into a 100ml Schlenk tube (reaction tube), add 0.5g of anhydrous aluminum chloride catalyst and seal it. Fix the Schlenk tube with an iron stand and place it in a DF-101S heat-collecting constant temperature heating magnetic stirrer. Set the reaction temperature to 20°C and the stirring speed to 250rpm / min. After 24 hours, the modification reaction is terminated.

[0035] After the modification reaction is completed, the reaction product is transferred to a 250ml pear-shaped bottle, 20ml of 10% hydrochloric acid solution is added dropwise and wait for 10min to terminate the reaction. All substances are transferred to a separatory funnel, and dichloromethane extractant is added three times, 20ml each time, and then the solution is allowed to stand for 10min to separate, and the crude product after removing the catalyst is collected. The collected crude product is placed in a rotary evaporator for rotary evaporation, the rotary temperature is 39°C, and the speed is set to 50rpm / min. The experiment is terminated after no bubbles are generated.

[0036] The reaction that occurs during the modification process is shown below:

[0037]

[0038] Example 2

[0039] Different from Example 1, the modification reaction temperature was set to 80°C, the timing was started when the temperature reached 80°C, the experiment was stopped after 24 hours, and subsequent operations were performed after cooling for 1 hour.

[0040] Example 3

[0041] Different from Example 1, the DF-101S heat-collecting constant temperature heating magnetic stirrer was turned on, the modification reaction temperature was set to 100°C, the timing was started when the temperature reached 100°C, the experiment was stopped after 24 hours, and subsequent operations were performed after cooling for 1 hour.

[0042] Example 4

[0043] Different from Example 1, the DF-101S heat-collecting constant temperature heating magnetic stirrer was turned on, the modification reaction temperature was set to 120°C, the timing was started when the temperature reached 120°C, the experiment was stopped after 24 hours, and subsequent operations were performed after cooling for 1 hour.

[0044] The experimental results of the yield changes at different modification reaction temperatures in Examples 1 to 4 are shown in Table 1.

[0045] Table 1 Yield changes at different modified reaction temperatures

[0046] Example Modification reaction temperature ℃ Yield % Example 1 20 33.15 Example 2 80 46.23 Example 3 100 57.91 Example 4 120 60.29

[0047] Example 5

[0048] The difference from Example 1 is that the catalyst for the modification reaction is anhydrous ferric chloride.

[0049] Example 6

[0050] The difference from Example 1 is that the catalyst for the modification reaction is anhydrous tin tetrachloride.

[0051] Example 7

[0052] The difference from Example 1 is that the catalyst for the modification reaction is anhydrous boron trifluoride.

[0053] The reaction results of Examples 1 and 5 to 7 under different catalyst conditions are shown in Table 2.

[0054] Table 2 Yield changes under different modified reaction catalysts

[0055] Example catalyst Yield % Example 1 <![CDATA[AlCl 3 ]]> 33.15 Example 5 <![CDATA[FeCl 3 ]]> 26.81 Example 6 <![CDATA[SnCl 4 ]]> 25.02 Example 7 <![CDATA[BF 3 ]]> 19.11

[0056] Example 8

[0057] The difference from Example 1 is that the amount of modifier used is 15 ml, and 22 ml of extractant is added each time.

[0058] Example 9

[0059] The difference from Example 1 is that the amount of modifier used is 20 ml, and the amount of extractant added is 23 ml each time. The experimental results of Examples 1, 8, and 9 under different agent-oil ratios are shown in Table 3.

[0060] Table 3 Yield changes under different agent-oil ratios

[0061] Example Agent-oil ratio Yield % Example 1 1:1 33.15 Example 8 1:1.5 33.31 Example 9 1:2 33.34

[0062] Example 10

[0063] The difference from Example 1 is that the amount of catalyst used is 0.8 g.

[0064] Embodiment 11

[0065] The difference from Example 1 is that the amount of catalyst used is 1.0 g.

[0066] The experimental results of Examples 1, 10 and 11 under different catalyst ratios are shown in Table 4.

[0067] Table 4 Yield changes under different catalyst dosages

[0068] Example Catalyst dosage Yield % Example 1 0.5 33.15 Example 10 0.8 33.18 Embodiment 11 1.0 33.18

[0069] Example 12

[0070] The difference from Example 1 is that the amount of dichloromethane used as the reaction solvent is 10 ml, and 17 ml of the extractant is added each time.

[0071] Embodiment 13

[0072] The difference from Example 1 is that the amount of dichloromethane used as the reaction solvent is 15 ml, and 18 ml of the extractant is added each time.

[0073] The experimental results of Examples 1, 12 and 13 under different reaction solvent dosage conditions are shown in Table 5.

[0074] Table 5 Yield changes under different reaction solvent dosages

[0075] Example Dichloromethane dosage Yield % Example 1 20ml 33.15 Example 12 10ml 32.93 Embodiment 13 15ml 33.06

[0076] Embodiment 14

[0077] Since the side chain on the benzene ring in coal tar has not only alkyl groups but also some hydroxyl groups, naphthol is used as the raw material in this embodiment, and the remaining reaction conditions and reaction steps are the same as those in Example 1. The reaction that occurs is shown in the following formula:

[0078]

[0079] Embodiment 15

[0080] Different from Example 14, the modification reaction temperature was set to 80°C, the timing started when the temperature reached 80°C, the experiment was stopped after 24 hours, and subsequent operations were performed after cooling for 1 hour.

[0081] Example 16

[0082] Different from Example 14, the DF-101S heat-collecting constant temperature heating magnetic stirrer was turned on, the modification reaction temperature was set to 100°C, the timing was started when the temperature reached 100°C, the experiment was stopped after 24 hours, and subsequent operations were carried out after cooling for 1 hour.

[0083] Embodiment 17

[0084] Different from Example 14, the DF-101S heat-collecting constant temperature heating magnetic stirrer was turned on, the modification reaction temperature was set to 120°C, the timing was started when the temperature reached 120°C, the experiment was stopped after 24 hours, and subsequent operations were carried out after cooling for 1 hour.

[0085] The experimental results of the yield changes at different reaction temperatures in Examples 14 to 17 are shown in Table 6.

[0086] Table 6 Yield changes at different reaction temperatures

[0087]

[0088]

[0089] Embodiment 18

[0090] The difference from Example 14 is that the catalyst for the modification reaction is anhydrous ferric chloride.

[0091] Embodiment 19

[0092] The difference from Example 14 is that the modification reaction catalyst is anhydrous tin tetrachloride.

[0093] Embodiment 20

[0094] The difference from Example 14 is that the catalyst for the modification reaction is anhydrous boron trifluoride.

[0095] The experimental results of yield changes under different catalysts in Examples 14, 18-20 are shown in Table 7.

[0096] Table 7 Yield changes under different catalysts

[0097] Example catalyst Yield % Embodiment 14 <![CDATA[AlCl 3 ]]> 26.34 Embodiment 18 <![CDATA[FeCl 3 ]]> 19.63 Embodiment 19 <![CDATA[SnCl 4 ]]> 16.24 Embodiment 20 <![CDATA[BF 3 ]]> 10.53

[0098] Embodiment 21

[0099] The difference from Example 14 is that the amount of modifier used is 15 ml and 22 ml of extractant is added each time.

[0100] Embodiment 22

[0101] The difference from Example 14 is that the amount of modifier used is 20 ml, and the amount of extractant added each time is 23 ml. The experimental results of the yield changes under different agent-to-oil ratios of Examples 14, 21, and 22 are shown in Table 8.

[0102] Table 8 Yield changes under different agent-oil ratios

[0103]

[0104]

[0105] Embodiment 23

[0106] The difference from Example 14 is that the amount of catalyst used is 0.8 g.

[0107] Embodiment 24

[0108] The difference from Example 14 is that the amount of catalyst used is 1.0 g.

[0109] The experimental results of yield changes under different catalyst dosage conditions of Examples 14, 23 and 24 are shown in Table 9.

[0110] Table 9 Yield changes under different catalyst dosages

[0111] Example Catalyst dosage g Yield % Embodiment 14 0.5 26.34 Embodiment 23 0.8 26.55 Embodiment 24 1.0 26.60

[0112] Embodiment 25

[0113] The difference from Example 14 is that the amount of dichloromethane used as the reaction solvent is 10 ml, and 17 ml of the extractant is added each time.

[0114] Embodiment 26

[0115] The difference from Example 14 is that the amount of dichloromethane used as the reaction solvent is 15 ml, and 18 ml of the extractant is added each time.

[0116] The experimental results of the yield changes under different solvent dosage conditions of Examples 14, 25 and 26 are shown in Table 10.

[0117] Table 10 Yield changes under different solvent dosages

[0118] Example Dichloromethane dosage Yield % Embodiment 14 20 26.34 Embodiment 25 10 25.78 Embodiment 26 15 26.04

[0119] Embodiment 27

[0120] Different from the above-mentioned embodiment, the raw material used in this embodiment is the distillate oil of 220-340° C. in medium-low temperature coal tar. The specific raw material properties are shown in Table 11 and Table 12.

[0121] Table 11 Coal tar components

[0122] project content% Straight chain alkanes 14.74 Monocyclic compounds 24.13 Bicyclic compounds 46.22 Tricyclic and above compounds 14.91

[0123] Table 12 Coal tar carbon number distribution

[0124]

[0125]

[0126] The specific experimental steps include:

[0127] Weigh 10g coal tar, 10g 2,5-dimethylfuran and 20ml dichloromethane into a 100ml Schlenk tube, add 0.5g anhydrous aluminum chloride catalyst and seal. Fix the Schlenk tube with an iron stand, place it in a DF-101S thermal collector constant temperature heating magnetic stirrer, and heat it in an oil bath. Set the temperature of the DF-101S thermal collector constant temperature heating magnetic stirrer to 100℃, and the stirring speed to 250rpm / min. After the temperature reaches 80℃, react for 6h, and then react at 100℃ for 18h. After the reaction is completed, place the Schlenk tube above the DF-101S thermal collector constant temperature heating magnetic stirrer and cool it naturally for 1h.

[0128] Transfer the reaction product to a 250ml pear-shaped bottle, add 20ml 10% hydrochloric acid solution and wait for 10min to terminate the reaction. Transfer all the substances to a separatory funnel, add dichloromethane extractant three times, add 20ml each time, then let it stand for 10min to separate the solution, and collect the crude product after removing the catalyst. Place the collected crude product in a rotary evaporator for rotary evaporation, the rotary temperature is 39℃, the speed is set to 50rpm / min, and the experiment is terminated when no bubbles are generated.

[0129] During the process of coal tar ring-increasing modification, the reaction that occurs is shown in the following formula:

[0130]

[0131] Wherein: R represents hydroxyl and various alkyl substituent groups, and the number of R on the same benzene ring is between 0 and 6.

[0132] Coal tar contains a variety of substances, and different substances undergo different reactions. The above four reactions represent the reactions occurring among the different types of substances.

[0133] After the products were collected and analyzed by GC-MS, it can be seen that the composition of coal tar has changed significantly after the ring-addition modification. The specific composition and carbon number distribution of the modified coal tar products are shown in Tables 13 and 14.

[0134] Table 13 Composition of modified coal tar products

[0135]

[0136]

[0137] Table 14 Carbon number distribution of modified coal tar products

[0138] project content% C7 11.26 C8 2.97 C9 3.87 C10 4.33 C11 6.26 C12 6.82 C13 9.42 C14 4.95 C15 2.81 C16+ 47.31

[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit its protection scope. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the field should understand that after reading the present invention, those skilled in the art can still make various changes, modifications or equivalent substitutions to the specific implementation methods of the invention, but these changes, modifications or equivalent substitutions are all within the protection scope of the pending claims of the invention.

Claims

1. A modified separation method for modified coal tar, characterized in that: The method comprises the following steps: coal tar, a modifier, a solvent and a catalyst are mixed to carry out a ring-addition modification reaction to obtain a first crude product, the modifier is 2,5-dimethylfuran, the mass ratio of coal tar to the modifier is 1:(1-2), the ring-addition modification reaction of the first crude product is terminated to obtain a second crude product, and the second crude product is separated from impurities by extraction and rotary evaporation to obtain modified coal tar, wherein the impurities include a catalyst and a solvent.

2. The modified separation method of modified coal tar according to claim 1, characterized in that: The catalyst adopts Lewis acid, the dosage of the catalyst is 5% to 10% of the mass of the coal tar, the solvent adopts dichloromethane, and the volume ratio of the coal tar to the solvent is 1: (1 to 2).

3. The modification and separation method of modified coal tar according to claim 1, characterized in that: The reaction temperature for the mixed ring-addition modification reaction is 20 to 120°C.

4. The modification and separation method of modified coal tar according to claim 7, characterized in that: The extraction is specifically as follows: the second crude product is mixed with an extractant for extraction, the extractant is dichloromethane, the volume ratio of the second crude product to the extractant is 1:1, and the extraction time is 5 to 30 minutes.

5. The modification and separation method of modified coal tar according to claim 1, characterized in that: The first crude product is mixed with a hydrochloric acid solution to obtain a second crude product, wherein the mass percentage concentration of the hydrochloric acid solution is 10%.

6. The modification and separation method of modified coal tar according to claim 1, characterized in that: Coal tar is composed of 12% to 20% straight-chain alkanes, 20% to 26% monocyclic, 40% to 50% bicyclic and 10% to 20% tricyclic and above compounds.

7. The modified separation method of modified coal tar according to claim 6, characterized in that: The solvent is dichloromethane, and the catalyst is anhydrous aluminum chloride, anhydrous ferric chloride, anhydrous tin tetrachloride or anhydrous boron trifluoride.

8. The modification and separation method of modified coal tar according to claim 1, characterized in that: The reaction pressure of the mixture is 101.325 kPa, the reaction time of the mixture is 6 to 24 hours, and the stirring rate of the mixture is 200 to 300 rpm / min.

9. The modification and separation method of modified coal tar according to claim 1, characterized in that: The temperature of the rotary evaporation is 30-40° C., the speed of the rotary evaporation is set to 50-80 rpm / min, and the rotary evaporation is stopped when no bubbles are generated.

10. A modified coal tar, characterized in that: The modified coal tar is prepared by the modified separation method of any one of claims 1 to 9.