Selective reduction chromium-silicon co-removal method for sodium modified vanadium liquid
By adjusting the pH value of the sodium vanadium solution and adding a silicon removal agent, the selective precipitation of chromium and silicon in the sodium vanadium solution is achieved, which solves the problem of coexistence of chromium and silicon in the existing vanadium extraction process and improves efficiency. Vanadium product quality and reduced vanadium losses.
Patent Information
- Application Number
- CN202410917163.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing vanadium extraction process, the coexistence of chromium and silicon in the sodium vanadium solution leads to a decline in the quality of the vanadium product. The existing chromium removal method has a large amount of wastewater, high costs and high vanadium losses, making it difficult to meet the diverse market needs.
By adjusting the pH value of the sodium vanadium solution to perform a reduction reaction within a specific range, adding a silicon removal agent to promote the selective precipitation of chromium and silicon, and using oxidation purification treatment to obtain a low chromium and low silicon vanadium intermediate precipitate. , reduce vanadium loss.
It achieves high-efficiency chromium and silicon removal, with small vanadium loss and short process. It can significantly reduce the chromium and silicon content in the vanadium liquid and improve the quality of vanadium products.
Smart Images

Figure CN118726770A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vanadium extraction technology, in particular to a method for selectively reducing chromium and silicon with sodium vanadium solution. Background Art
[0002] Vanadium is a very rare metal element, mainly used in the steel industry to improve the strength, toughness and other properties of steel products. In recent years, the application of vanadium in non-steel fields has become more and more extensive, such as the hot energy storage field, vanadium-based positive electrode materials, and the research and application of all-vanadium liquid flow batteries have become more and more mature. There are also many applications in chemical catalysis, medicine, metal vanadium, vanadium alloys, titanium alloys and other fields. The application characteristics of vanadium in non-steel fields determine that the quality requirements of vanadium oxide are very high. The sodium roasting of vanadium slag-water leaching vanadium extraction process is still the most widely used vanadium extraction process. Due to the chromium characteristics of vanadium, the sodium leached vanadium liquid generally contains a certain amount of chromium. In the process of vanadium precipitation in vanadium liquid, chromium will more or less enter the vanadium product, thereby reducing the quality of vanadium products. Therefore, it is necessary to reduce the chromium content in the vanadium liquid, and then reduce the chromium entering the vanadium product, so as to improve the quality of vanadium products and meet the needs of multiple markets. The industry generally adopts the re-dissolution of vanadium intermediate precipitates APV, AMV, and SAV for secondary vanadium precipitation to achieve chromium removal of vanadium products, or adopts weak acid or weak alkaline reduction of vanadium liquid to remove chromium. Such methods generally produce large amounts of wastewater, high vanadium losses, and high costs.
[0003] For example, in the literature: "Study on the Removal of Chromium Impurities in Vanadium Solution by Sodium Sulfide Reduction", Na2S was used as the reducing agent and NaOH as the precipitating agent to study the effects of reducing agent dosage, temperature, reaction time, precipitation time and solution pH value on the removal of chromium impurities and vanadium loss rate. The experiment showed that the optimal reaction conditions were Na2S addition amount 4 times the theoretical dosage, reaction temperature 60℃, reaction time 2h, precipitation time 2h, and solution pH=11 during the reaction. At this time, the chromium removal rate was as high as 94%, and the vanadium loss rate was also controlled at 14%.
[0004] Based on this, the existing technology still needs to be improved. Summary of the invention
[0005] In order to solve the above technical problems, the embodiment of the present invention proposes a method for selectively reducing chromium and silicon with sodium vanadium solution to solve the technical problems existing in the sodium vanadium chromium and silicon co-removal in the prior art.
[0006] In order to solve the above technical problems, some embodiments of the present invention disclose a method for selectively reducing chromium and silicon by sodium vanadium solution, comprising: Step 1, adjusting the pH value of the sodium vanadium solution so that the pH value of the system solution is 10.5-11.5 at 60° C., or the pH value of the system solution is 11.3-12.7 at 20° C.-25° C., to obtain a pretreated sodium vanadium solution; Step 2, adding a predetermined amount of reducing agent to the pretreated sodium vanadium solution at one time to carry out a reduction reaction; Step 3: adding a silicon remover to the reaction system at the end of the reduction reaction to react and obtain a first intermediate reaction solution; Step 4: performing solid-liquid separation on the first intermediate reaction liquid, washing the solid phase with water and then adding it into the filtrate to obtain a decontamination liquid; Step 5: subjecting the impurity removal liquid to an oxidation purification treatment to obtain a purified liquid.
[0007] In some embodiments, it also includes: Step 6: dilute the purified solution to a vanadium content of 25 g / L-35 g / L, adjust the pH value to 5.0-6.0, the temperature to 20-70° C., and then add ammonium salt; Step 7: Adjust the pH value to 2.0-2.3 and then heat to 90-100°C for heat preservation and reaction, and then perform solid-liquid separation to obtain APV.
[0008] In some embodiments, in step six, the amount of ammonium salt added is TV / ammonium sulfate = 1.2 to 2.0 by mass ratio.
[0009] In some embodiments, it also includes: Step 6, adjusting the pH value of the purified liquid to 9.0-9.5 and the temperature to 20-40° C., and then adding ammonium salt; Step 7: After the reaction is carried out at 10-40°C, solid-liquid separation is performed to obtain AMV.
[0010] In some embodiments, in step six, the amount of ammonium salt added is TV / ammonium sulfate = 2.5 to 5.0 by mass ratio.
[0011] In some embodiments, in step 1, If the pH value of the system solution is greater than 11.5 at 60°C, sulfuric acid is added to the system solution to adjust the pH value; If the pH value of the system solution is less than 10.5 at 60°C, add sodium hydroxide to the system solution to adjust the pH value, and the reaction must last for 10 to 60 minutes after the addition of sodium hydroxide; Preferably, the pH value of the system solution at 60° C. is 10.6-11.0.
[0012] In some embodiments, in step 2, the reducing agent is sodium hydrosulfide or sodium sulfide, and the amount of the reducing agent added is Cr / S=0.75-1.3 in terms of the molar ratio, the pH value of the reaction system at 60° C. is 10.5-11.5, the reaction temperature is 60° C.-95° C., and the reaction time is 30 min-90 min; Preferably, in step 2, the amount of reducing agent sodium hydrosulfide or sodium sulfide added is Cr / S=0.85-1.0, the reaction temperature is 60° C.-85° C., and the reaction time is 30 min-60 min.
[0013] In some embodiments, in step three, the desiliconizing agent is aluminum sulfate, and the amount of the desiliconizing agent added is Al / Si=0.4-0.8 in terms of the molar ratio, the reaction temperature is 60-95° C., and the reaction time is 30-40 min.
[0014] In some embodiments, in step 4, the impurity removal residue obtained after solid-liquid separation is washed once with clean water at 20° C. to 60° C., and the washing filtrate is added to the impurity removal liquid. The amount of washing water is the amount of water taken away by the impurity removal residue, and the volume of the impurity removal liquid is ensured to be equal to the volume of the sodium vanadium solution; Preferably, in step 4, the first intermediate reaction liquid obtained after the reaction is completed is subjected to solid-liquid separation without standing.
[0015] In some embodiments, in step 5, the oxidant for the oxidation purification treatment is hydrogen peroxide with a mass concentration of 25% to 50%, and the amount added is H2O2 / Cr=1 to 2.5 in terms of the molar ratio of substances, the pH value of the reaction system is 10.8 to 12.0 at 60°C, the reaction temperature is 30°C to 95°C, and the reaction time is 10min to 60min; Preferably, in step five, the pH value of the reaction system at 60° C. is 10.8 to 11.5, the temperature range is 60° C. to 85° C., and the reaction time is 20 min to 30 min.
[0016] By adopting the above technical solution, the present invention has at least the following beneficial effects: The present invention provides a method for selectively reducing chromium and silicon removal by sodium-containing vanadium liquid. Under specific concentration and pH conditions, vanadium mainly exists in the form of pyrovanadate in sodium-containing solution. The vanadium has low oxidizability, stable properties, and is not easily reduced. Even if a small part of it is reduced, the vanadium still remains in the solution in the form of vanadate, while the chromate is selectively reduced to generate chromium hydroxide, and the vanadium and chromium separation is completed in the form of chromium hydroxide precipitation. At the end of the selective reduction reaction, aluminum salt is added to the reduction system to react with silicon in the vanadium liquid to generate aluminum silicate. The aluminum silicate and chromium hydroxide are mutually adsorbed, flocculated and co-precipitated, which can greatly promote the chromium removal effect and silicon removal effect of the system. After the impurity removal liquid is purified, low-chromium and low-silicon vanadium intermediate precipitates APV and AMV can be precipitated. The present invention has the characteristics of high chromium removal rate, high silicon removal rate, small vanadium loss and short process. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 A diagram showing the pH and potential range for selective reduction and chromium removal of a method for selective reduction and co-removal of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Figure 2 A diagram showing the pH and potential range for selective reduction and chromium removal of a method for selective reduction and co-removal of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Figure 3 A graph showing the relationship between the redox potential and time during the reduction of chromium and silicon in a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Figure 4 A graph showing the relationship between pH and time during the reduction of chromium and silicon in a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Figure 5 A graph showing the relationship between the oxidation potential of a vanadium solution and pH in a method for selectively reducing chromium and silicon by using a sodium vanadium solution disclosed in some embodiments of the present invention; Figure 6 A graph showing the relationship between the oxidation potential of a vanadium solution and the temperature in a method for selectively reducing chromium and silicon by using a sodium vanadium solution disclosed in some embodiments of the present invention; Figure 7 A diagram showing the effect of temperature on the chromium and silicon removal efficiency and vanadium loss in a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Figure 8 A diagram showing the effect of time on the chromium and silicon removal efficiency and vanadium loss in a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Fig. 9 A diagram showing the effect of pH on chromium removal efficiency and vanadium loss in a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Fig.10 A graph showing the effect of the reducing agent addition coefficient on the chromium and silicon removal efficiency in the selective reduction of chromium and silicon removal process in a method for selective reduction of chromium and silicon removal with sodium vanadium solution disclosed in some embodiments of the present invention; Fig.11A diagram showing the influence of the aluminum addition coefficient on the silicon removal efficiency and vanadium loss in the selective reduction of chromium and silicon by a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Fig.12 A diagram showing the influence of the aluminum addition coefficient on the sedimentation effect of impurity removal slag in a method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Fig.13 A diagram showing the oxidation effect of the impurity removal liquid in a method for selectively reducing chromium and silicon by sodium vanadium solution disclosed in some embodiments of the present invention; Fig.14 The present invention discloses a flow chart of a method for selectively reducing chromium and silicon by sodium vanadium solution according to some embodiments of the present invention. DETAILED DESCRIPTION
[0019] The following is a further detailed description of the embodiments of the present disclosure in conjunction with the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to exemplarily illustrate the principles of the present disclosure, but cannot be used to limit the scope of the present disclosure. The present disclosure can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
[0020] The present disclosure provides these embodiments to make the present disclosure thorough and complete, and to fully express the scope of the present disclosure to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of the materials, the numerical expressions and the numerical values set forth in these embodiments should be interpreted as being merely exemplary, and not as limiting.
[0021] It should be noted that, in the description of the present disclosure, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present disclosure. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0022] In addition, the words "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different parts. "Vertical" does not mean vertical in the strict sense, but is within the tolerance range. "Parallel" does not mean parallel in the strict sense, but is within the tolerance range. "Include" or "comprising" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.
[0023] It should also be noted that in the description of the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.
[0024] All terms used in the present disclosure have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined as such herein.
[0025] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.
[0026] like Fig.14 As shown, some embodiments of the present invention disclose a method for selective reduction of sodium vanadium liquid to remove chromium and silicon. Under specific concentration and pH conditions, vanadium mainly exists in the form of pyrovanadate in sodium solution, which has low oxidizability, stable properties, and is not easy to be reduced. Even if a small part is reduced, vanadium still remains in the solution in the form of vanadate, and chromate will be selectively reduced to form chromium hydroxide, and vanadium and chromium separation is completed in the form of chromium hydroxide precipitation. At the end of the selective reduction reaction, aluminum salt is added to the reduction system to react with silicon in the vanadium liquid to form aluminum silicate. Aluminum silicate and chromium hydroxide are mutually adsorbed, flocculated and co-precipitated, which can greatly promote the chromium removal effect and silicon removal effect of the system. The present invention can easily reduce Cr in vanadium liquid from 3000mg / L to 1mg / L, Si<20mg / L, and vanadium loss rate can be <2%. After purification, the impurity removal liquid can precipitate low-chromium and low-silicon vanadium intermediate precipitates APV and AMV.
[0027] The method comprises the following steps: a. Pretreatment of sodium leaching solution (sodium vanadium solution); b. Adding a reducing agent to the pretreatment solution for selective reduction and chromium removal; c. Add silicon removal agent to the reduction system to carry out silicon-chromium co-precipitation; d. Purifying the impurity removal liquid to obtain a vanadium precipitation purified liquid; e. Purify the liquid to prepare vanadium intermediate precipitate APV or AMV.
[0028] The composition requirements of the sodium vanadium solution are shown in Table 1.
[0029] Table 1
[0030] In the above embodiment, the vanadium concentration of the sodium vanadium solution in step a should be controlled at 30 g / L to 60 g / L, preferably in the range of 35 g / L to 50 g / L, and the pH of the sodium vanadium solution is controlled at 10.5 to 11.5 (the pH is measured at 60°C. If it is at 20°C to 25°C, it must be increased by 0.8 to 1.2 in the range of 10.5 to 11.5. The main reason is that the higher the temperature of the sodium vanadium solution system, the lower the detected pH, and it changes nonlinearly), preferably in the pH range of 10.6 to 11.0. Experiments have found that a pH higher than the above range will cause the chromium-containing solid particles in the chromium removal solution to become smaller, which is not conducive to sedimentation and filtration. Further increase in pH will cause part of the Cr(OH)3 to dissolve, and vanadium and chromium separation cannot be efficiently achieved, which is not conducive to the chromium removal process. If the pH of the sodium vanadium solution in step a is less than 10.5 at 60° C., sodium hydroxide needs to be added to adjust the pH to ≥ 10.5. After adding the sodium hydroxide, the reaction must be carried out for 10 min to 60 min, preferably 20 min to 40 min, so that the vanadium is fully polymerized in the solution, so that the vanadium exists mainly in the form of pyrovanadate in the solution. If the pH of the sodium vanadium solution in step a is greater than 11.5 at 60° C., sulfuric acid needs to be added to adjust the pH to ≤ 11.5. If the pH is too high, the solubility of chromium hydroxide will increase, and the vanadium-chromium separation cannot be effectively completed.
[0031] In step b, the reducing agent is sodium hydrosulfide and sodium sulfide, preferably sodium hydrosulfide, the reducing agent addition coefficient Cr / S=0.75-1.3 (molar ratio), preferably Cr / S=0.85-1.0, the reaction pH is 10.5-11.5 (measured at 60° C.), the reduction temperature is 60° C.-95° C., preferably 60° C.-85° C., and the reduction time is 30 min-90 min, preferably 30 min-60 min; the reducing agent in step b is added all at once, and after the reducing agent is added, the pH of the solution system will increase rapidly, further improving the selective reduction and chromium removal ability of the entire system.
[0032] The silicon removal agent in step c is aluminum sulfate, and the silicon removal agent addition coefficient is Al / Si=0.4-0.8 (substance molar ratio). Because part of the silicon will be taken away during the reduction and chromium removal process, and the addition of too much aluminum sulfate will greatly reduce the pH of the system, which is not conducive to the selective reduction and chromium removal. Appropriately lowering the pH of the system at the end of the reduction and chromium removal can enhance the vanadium-chromium separation effect; the reaction temperature of the silicon removal agent in step c is 60°C-95°C, the reaction time is 10min-60min, preferably 30min-40min, and the reaction is completed. The post-standing time is 0 to 48 hours, preferably 0 to 12 hours. In the mixed system of chromium hydroxide and aluminum silicate, the adverse effects of pH and standing time on the silicon removal effect will be weakened, that is, a better silicon removal effect can be achieved under high pH and no standing conditions, and the filterability of the impurity removal slag will be greatly increased; after the solid-liquid separation in step c, the impurity removal slag is washed once with 20°C to 60°C clean water, and the washing filtrate is merged into the impurity removal liquid. The amount of washing water is the amount of water taken away by the impurity removal slag, ensuring that the amount of impurity removal liquid is roughly equal to the volume of the vanadium liquid before impurity removal.
[0033] In step d, an oxidant is used for oxidation purification, the oxidant is 25% to 50% hydrogen peroxide, the addition amount is H2O2 / Cr=1 to 2.5 (molar ratio), the reaction pH is 10.8 to 12.0 (at 60°C), preferably the pH range is 10.8 to 11.5, the reaction temperature is 30°C to 95°C, preferably the temperature range is 60°C to 85°C, the reaction time is 10min to 60min, preferably the time range is 20min to 30min.
[0034] If APV is precipitated in step e, the solution needs to be diluted to V of 25g / L~35g / L, the pH is adjusted to 5.0~6.0 for the first time, the pH temperature is adjusted to 20℃~70℃ for the first time, and ammonium salt is added after the pH is adjusted. The amount of ammonium salt added is TV / ammonium sulfate = 1.2~2.0 (mass ratio), and the preferred amount of ammonium salt added is TV / ammonium sulfate = 1.2~1.6 (mass ratio). Then, the acid is adjusted for the second time, and the pH is adjusted to 2.0~2.3 for the second time. Then, the temperature is raised to 90℃~100℃ and kept for 45min~90min. After solid-liquid separation, high-quality APV is obtained.
[0035] If AMV is precipitated in step e, there is no need to dilute the purified liquid, adjust the pH to 9.0-9.5, adjust the pH temperature to 20°C-40°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 2.5-5.0 (mass ratio), keep warm at 10°C-40°C for 120min-240min, and obtain high-quality AMV after solid-liquid separation.
[0036] Experiments have shown that the method for selective reduction of chromium and silicon by sodium vanadium solution disclosed in the embodiment of the present invention can reduce 3.2g / L Cr in the solution to 0.002g / L, a reduction of more than 1000 times, and reduce 0.8g / L Si to 0.03g / L under high pH conditions, with a chromium removal rate of more than 99.5% and a silicon removal rate of more than 93.3%. The vanadium loss is about 2.41%-2.55%.
[0037] In the process of reducing chromium, it is necessary to control the pH and redox potential. Figure 1 In the wireframe area A, vanadium is ensured to exist in the solution in ionic form, while chromium in the system will precipitate out as Cr(OH)3 (e.g. Figure 2 Wire frame B), thereby achieving vanadium-chromium separation in the solution system. Figure 3 This is the relationship between the redox potential and time in the process of selective reduction of chromium and silicon by sodium vanadium solution. Figure 1 , reflecting that the redox potential in the actual operation process is consistent with the theoretical range value. Figure 4 This is the relationship between pH and time in the process of selective reduction of chromium and silicon by sodium vanadium solution. Figure 1 , reflecting that the pH value in the actual operation process is consistent with the theoretical range value; combined Figure 1 , Figure 2 , Figure 3 , Figure 4 This indicates that the actual potential and pH value of the sodium vanadium solution in the process of selective reduction of chromium and silicon are consistent with the theory, and the chromium removal agent has excellent performance. Figure 5 is the relationship between the oxidation potential of the solution system and pH, Figure 5 It can be seen that the oxidation potential of vanadium in the solution decreases with the increase of pH value, which means that the higher the pH value of the solution, the lower the oxidizability of vanadium, the more stable the existence form of vanadium, the less likely V is to be reduced during chromium removal, the better the V-Cr selectivity, and the lower the vanadium loss. Figure 6 is the relationship between the oxidation potential of the solution system and temperature. Figure 6 It can be seen that the oxidation potential of vanadium in the solution decreases with increasing temperature, which means that the higher the solution temperature, the lower the oxidizability of vanadium, the more stable the existence form of vanadium, the less likely V is to be reduced during chromium removal, the better the V-Cr selectivity, and the lower the vanadium loss. Figure 7 The effect of temperature on the removal efficiency of chromium and silicon and vanadium loss in the process of selective reduction of chromium and silicon is shown in Figure 2. Figure 7 It can be seen that when the water bath temperature is ≥70℃ (solution temperature is 60℃), the chromium removal effect is good and the vanadium loss is low. Figure 8 The figure is the effect of time on the removal efficiency of chromium and silicon and vanadium loss in the process of selective reduction of chromium and silicon; Figure 8 It can be seen that when the reaction time is 30 minutes, the Cr in the purified liquid can be reduced to 0.006 g / L, and the vanadium loss begins to increase after 60 minutes. Fig. 9The effect of pH on chromium removal efficiency and vanadium loss in the process of selective reduction of chromium and silicon is shown in Figure 2. Fig. 9 It can be seen that the selective reduction and removal of chromium by sodium vanadium solution requires a higher pH. If the pH is lower, the chromium removal rate is low and the vanadium loss is large. Fig.10 The effect of the reducing agent addition coefficient on the removal efficiency of chromium and silicon in the process of selective reduction of chromium and silicon is shown in the figure. Fig.10 It can be seen that when the chromium removal agent dosage coefficient increases from 0.7 to 1.0, the chromium concentration in the purified liquid can be reduced from about 1g / L to less than 0.1g / L, and silicon and chromium show synergistic changes. Fig.11 The figure is the effect of aluminum addition coefficient on silicon removal efficiency and vanadium loss in the process of selective reduction of chromium and silicon; Fig.11 It can be seen that as the aluminum addition coefficient increases, the Si content in the purification liquid decreases, and there is no obvious regularity in the effect of the aluminum addition coefficient on the vanadium loss. Fig.12 This is the effect of aluminum addition coefficient on the sedimentation effect of impurity removal during the selective reduction of chromium and silicon. Fig.13 This is a diagram showing the oxidation effect of the impurity removal liquid. Fig.12 , Fig.13 It can be seen that adding aluminum sulfate will reduce the pH value of the purified liquid, which is conducive to the precipitation of silicon and chromium. When aluminum sulfate is not added, there are more suspended solids in the purified liquid, which is difficult to clarify. When filtering, the suspended solids are seriously filtered (the number below the beaker is the aluminum addition coefficient). The impurity removal liquid is colorless after complete oxidation. The impurity removal liquid is yellow-brown mainly due to vanadic acid, and the sodium vanadium liquid is yellow mainly due to chromate. Under high pH conditions, vanadium is reduced to vanadic acid and exists in the solution in the form of ions, which will not increase vanadium loss.
[0038] Example 1 Use a measuring cylinder to measure 400mL of the above sodium vanadium solution. The composition is shown in Table 1.1. The vanadium concentration of the vanadium solution is 39.39g / L, the pH of the sodium vanadium solution is 10.5 (measured at 60°C), sodium hydrosulfide (containing 32% water) is used as the reducing agent, the reducing agent addition coefficient Cr / S=1.0 (molar ratio) is 1.56g, the reaction pH is 10.5 (measured at 60°C), the reduction temperature is 63°C, and the reduction time is 60min; the reducing agent is added all at once, aluminum sulfate is used as the desiliconizing agent, the desiliconizing agent addition coefficient is Al / Si=0.8 (molar ratio) is 2.97g, and the desiliconizing agent reaction is 1.50g. The reaction temperature is 60℃, the reaction time is 30min, the standing time after the reaction is 0h, the impurity removal residue after solid-liquid separation is washed once with 26℃ clean water, the washing filtrate is added into the impurity removal liquid, the washing water volume is 80mL, and it is ensured that the volume of the impurity removal liquid is roughly equal to the volume of the vanadium liquid before impurity removal; an oxidant is used for oxidation purification, the oxidant is 30% hydrogen peroxide, the addition amount is H2O2 / Cr=2 (molar ratio) of 4.24mL, the reaction pH is 10.8 (at 60℃), the reaction temperature is 60℃, the reaction time is 30min, Cr<1mg / L, Si=0.02g / L in the purified liquid, and the vanadium loss is 1.4%.
[0039] Take the purified liquid to precipitate APV, dilute the solution to V of 30g / L, a total of 200mL, adjust pH to 5.0 for the first time, and adjust the pH temperature to 60℃. After adjusting the pH, add ammonium salt, the amount of ammonium salt added is TV / ammonium sulfate = 1.2 (mass ratio), which is 7.2g. Then carry out the second acid adjustment, adjust pH to 2.0 for the second time, then raise the temperature to 95℃ and keep warm for 60min. After solid-liquid separation, high-quality APV is obtained. The composition is shown in Table 1.2 below.
[0040] Table 1.1 Element Na V Si Cr pH content 40g / L 39.39g / L 0.78g / L 2.43g / L 10.5(60℃) Table 1.2 Element V Cr Si Na K content / % 50.20 <0.01 <0.01 0.101 0.104 To precipitate AMV, there is no need to dilute the purified liquid, a total of 200 mL, adjust the pH to 9.0, adjust the pH temperature to 30°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 2.5 (mass ratio) is 19.41g, keep warm at 30°C for 180 minutes, and the high-quality AMV after solid-liquid separation, the composition is shown in Table 1.3.
[0041] Table 1.3 Element V Cr Si Na K content / % 43.46 <0.01 0.010 0.026 0.016 Example 2 Use a measuring cylinder to measure 400mL of the above sodium vanadium solution. The composition and content are shown in Table 2.1. The vanadium concentration of the vanadium solution is 49.04g / L, and the pH of the sodium vanadium solution is 10.1 (measured at 60°C). Sodium hydroxide needs to be added to adjust the pH to 10.8. After adding sodium hydroxide, the reaction must be carried out for 30 minutes. Sodium sulfide (sodium sulfide nonahydrate) is used as a reducing agent. The reducing agent addition coefficient Cr / S=0.85 (molar ratio) is 4.98g, the reaction pH is 10.8 (measured at 60°C), the reduction temperature is 85°C, and the reduction time is 30min; the reducing agent is added all at once, and aluminum sulfate is used as a desiliconizing agent. The desiliconizing agent addition coefficient is Al / Si=0.6 (molar ratio) is 2.21g, the reaction temperature of the silicon remover is 80℃, the reaction time is 30min, the standing time after the reaction is 12h, the impurity removal residue after solid-liquid separation is washed once with 20℃ clean water, the washing filtrate is added to the impurity removal liquid, the washing water volume is 90mL, and the impurity removal liquid volume is ensured to be roughly equal to the volume of the vanadium liquid before impurity removal; an oxidant is used for oxidation purification, the oxidant is 30% hydrogen peroxide, the addition amount is H2O2 / Cr=2.5 (molar ratio) is 5.88mL, the reaction pH is 11.1 (at 60℃), the reaction temperature is 60℃, the reaction time is 30min, Cr<1mg / L in the purified liquid, Si=0.01g / L, and the vanadium loss is 1.6%.
[0042] Take the purified liquid to precipitate APV, dilute the solution to V of 30g / L, a total of 200mL, adjust pH to 6.0 for the first time, and adjust the pH temperature to 70℃. After adjusting the pH, add ammonium salt, the amount of ammonium salt added is TV / ammonium sulfate = 1.6 (mass ratio), which is 9.6g. Then carry out the second acid adjustment, adjust pH to 2.3 for the second time, then raise the temperature to 90℃ and keep warm for 45min. After solid-liquid separation, high-quality APV is obtained. The composition is shown in Table 2.2.
[0043] Table 2.1 Element Na V Si Cr pH content 39.1g / L 49.04g / L 0.774g / L 2.7g / L 10.1(60℃) Table 2.2 Element V Cr Si Na K content / % 50.33 <0.01 <0.01 0.079 0.080 To precipitate AMV, there is no need to dilute the purified liquid, a total of 200 mL, adjust the pH to 9.5, adjust the pH temperature to 40°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 4 (mass ratio), which is 38.68 g, keep warm at 30°C for 120 minutes, and the high-quality AMV after solid-liquid separation is obtained. The composition is shown in Table 2.3.
[0044] Table 2.3 Element V Cr Si Na K content / % 43.21 <0.01 0.012 0.087 0.018 Example 3 Table 3.1 Element Na V Si Cr pH content 43.1g / L 52.0g / L 0.84g / L 3.2g / L 10.0(60℃) Use a measuring cylinder to measure 400mL of the above sodium vanadium solution. The composition and content are shown in Table 3.1. The vanadium concentration of the vanadium solution is 52g / L, and the pH of the sodium vanadium solution is 10.0 (measured at 60°C). Sodium hydroxide needs to be added to adjust the pH to 10.8. After adding sodium hydroxide, the reaction must be carried out for 30 minutes. Sodium hydrosulfide is used as a reducing agent (70% effective ingredient). The reducing agent addition coefficient Cr / S=1 (molar ratio) is 1.97g, the reaction pH is 10.8 (measured at 60°C), the reduction temperature is 85°C, and the reduction time is 30min; the reducing agent is added all at once, and aluminum sulfate is used as a desiliconizing agent. The desiliconizing agent addition coefficient is Al / Si=0.4 (molar ratio). The molar ratio) is 1.52g, the reaction temperature of the silicon remover is 80℃, the reaction time is 30min, the standing time after the reaction is 12h, and the impurity removal slag is washed once with 20℃ clean water after solid-liquid separation, and the washing filtrate is incorporated into the impurity removal liquid. The washing water volume is 100mL to ensure that the volume of the impurity removal liquid is roughly equal to the volume of the vanadium liquid before impurity removal; an oxidant is used for oxidation purification, the oxidant is 30% hydrogen peroxide, the addition amount is H2O2 / Cr=1 (molar ratio) is 2.79mL, the reaction pH is 11.4 (at 60℃), the reaction temperature is 60℃, the reaction time is 30min, Cr=0.002g / L, Si=0.01g / L in the purified liquid, and the vanadium loss is 2.2%.
[0045] Take the purified liquid to precipitate APV, dilute the solution to V of 30g / L, a total of 200mL, adjust pH to 6.0 for the first time, and adjust the pH temperature to 70℃. After adjusting the pH, add ammonium salt, the amount of ammonium salt added is TV / ammonium sulfate = 1.6 (mass ratio), which is 9.6g. Then carry out the second acid adjustment, adjust pH to 2.3 for the second time, then raise the temperature to 90℃ and keep warm for 45min. After solid-liquid separation, high-quality APV is obtained. The composition is shown in Table 3.2.
[0046] Table 3.2 Element V Cr Si Na K content / % 50.36 <0.01 <0.01 0.039 0.098 To precipitate AMV, there is no need to dilute the purified liquid, a total of 200 mL, adjust the pH to 9.5, adjust the pH temperature to 40°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 4 (mass ratio), which is 40.68 g, keep warm at 30°C for 120 minutes, and the high-quality AMV after solid-liquid separation is obtained. The composition is shown in Table 3.3.
[0047] Table 3.3 Element V Cr Si Na K content / % 43.31 <0.01 0.010 0.017 0.018 Example 4 Table 4.1 Element Na V Si Cr pH content 43.1g / L 52.0g / L 0.84g / L 3.2g / L 10.0(60℃) Use a measuring cylinder to measure 400mL of the above sodium vanadium solution. The composition and content are shown in Table 4.1. The vanadium concentration of the vanadium solution is 52g / L, and the pH of the sodium vanadium solution is 10.0 (measured at 60°C). Sodium hydroxide needs to be added to adjust the pH to 10.8. After adding sodium hydroxide, it must react for 30 minutes. Sodium hydrosulfide is used as a reducing agent (70% effective ingredient). The reducing agent addition coefficient Cr / S=1 (molar ratio) is 1.97g. The reducing agent is added in 5 times, with an interval of 2min between each addition. It takes 8min to complete the addition. The reaction pH is 10.8 (measured at 60°C), the reduction temperature is 85°C, and the reduction time is 30min. Aluminum sulfate is used as a desiliconizer, and the desiliconizer addition coefficient is Al / Si=0.4 (molar ratio) is 1.52g, the reaction temperature of the silicon remover is 80℃, the reaction time is 30min, the standing time after the reaction is 12h, the impurity removal slag after solid-liquid separation is washed once with 20℃ clean water, and the washing filtrate is added to the impurity removal liquid. The washing water volume is 100mL to ensure that the volume of the impurity removal liquid is roughly equal to the volume of the vanadium liquid before impurity removal; an oxidant is used for oxidation purification, the oxidant is 30% hydrogen peroxide, the addition amount is H2O2 / Cr=1 (molar ratio) is 2.79mL, the reaction pH is 11.4 (at 60℃), the reaction temperature is 60℃, the reaction time is 30min, Cr=0.03g / L and Si=0.01g / L in the purified liquid, and the vanadium loss is 3.2%.
[0048] Take the purified liquid to precipitate APV, dilute the solution to V of 30g / L, a total of 200mL, adjust pH to 6.0 for the first time, and adjust the pH temperature to 70℃. After adjusting the pH, add ammonium salt, the amount of ammonium salt added is TV / ammonium sulfate = 1.6 (mass ratio), which is 9.6g. Then carry out the second acid adjustment, adjust pH to 2.3 for the second time, then raise the temperature to 90℃ and keep warm for 45min. After solid-liquid separation, high-quality APV is obtained. The composition is shown in Table 4.2.
[0049] Table 4.2 Element V Cr Si Na K content / % 50.1 0.016 <0.01 0.060 0.138 To precipitate AMV, there is no need to dilute the purified liquid, a total of 200 mL, adjust the pH to 9.5, adjust the pH temperature to 40°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 4 (mass ratio), which is 40.68 g, keep warm at 30°C for 120 minutes, and the high-quality AMV after solid-liquid separation is obtained. The composition is shown in Table 4.3.
[0050] Table 4.3 Element V Cr Si Na K content / % 43.01 0.021 0.011 0.027 0.023 Example 5 Table 5.1 Element Na V Si Cr pH content 43.1g / L 52.0g / L 0.84g / L 3.2g / L 10.0(60℃) Use a measuring cylinder to measure 400mL of the above sodium vanadium solution. The composition and content are shown in Table 5.1. The vanadium concentration of the vanadium solution is 52g / L, the pH of the sodium vanadium solution is 10.0 (measured at 60°C), and the pH of the vanadium solution is not adjusted. Sodium hydrosulfide is used as a reducing agent (70% effective ingredient), the reducing agent addition coefficient Cr / S=1 (molar ratio) is 1.97g, the reaction pH is 10.0 (measured at 60°C), the reduction temperature is 85°C, and the reduction time is 30min; the reducing agent is added all at once, aluminum sulfate is used as a desiliconizing agent, the desiliconizing agent addition coefficient is Al / Si=0.4 (molar ratio) is 1.52g, and the desiliconizing agent The reaction temperature was 80°C, the reaction time was 30 min, and the reaction was allowed to stand for 12 h. After solid-liquid separation, the impurity removal residue was washed once with 20°C clean water, and the washing filtrate was added to the impurity removal liquid. The washing water volume was 100 mL, ensuring that the volume of the impurity removal liquid was roughly equal to the volume of the vanadium liquid before impurity removal. An oxidant was used for oxidation purification. The oxidant was 30% hydrogen peroxide, and the addition amount was H2O2 / Cr=1 (molar ratio) of 2.79 mL. The reaction pH was 11.4 (at 60°C), the reaction temperature was 60°C, the reaction time was 30 min, Cr=0.634 g / L, Si=0.02 g / L in the purified liquid, and the vanadium loss was 5.2%.
[0051] Take the purified liquid to precipitate APV, dilute the solution to V of 30g / L, a total of 200mL, adjust pH to 6.0 for the first time, and adjust the pH temperature to 70℃. After adjusting the pH, add ammonium salt, the amount of ammonium salt added is TV / ammonium sulfate = 1.6 (mass ratio), which is 9.6g. Then carry out the second acid adjustment, adjust pH to 2.3 for the second time, then raise the temperature to 90℃ and keep warm for 45min. After solid-liquid separation, high-quality APV is obtained. The composition is shown in Table 5.2.
[0052] Table 5.2 Element V Cr Si Na K content / % 49.11 0.219 0.012 0.139 0.113 To precipitate AMV, there is no need to dilute the purified liquid, a total of 200 mL, adjust the pH to 9.5, adjust the pH temperature to 40°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 4 (mass ratio), which is 40.68 g, keep warm at 30°C for 120 minutes, and the high-quality AMV after solid-liquid separation is obtained. The composition is shown in Table 5.3.
[0053] Table 5.3 Element V Cr Si Na K content / % 42.71 0.184 0.021 0.037 0.053 Example 6 Table 6.1 Element Na V Si Cr pH content 43.1g / L 52.0g / L 0.84g / L 3.2g / L 10.0(60℃) Use a measuring cylinder to measure 400mL of the above sodium vanadium solution. The composition and content are shown in Table 5.1. The vanadium concentration of the vanadium solution is 52g / L, the pH of the sodium vanadium solution is 10.0 (measured at 60°C), and sodium hydroxide is used to adjust the pH of the vanadium solution to 11.6. After adding sodium hydroxide, the reaction must be carried out for 30 minutes. Sodium hydrosulfide is used as a reducing agent (70% effective ingredient), the reducing agent addition coefficient Cr / S=1 (molar ratio) is 1.97g, the reaction pH is 10.0 (measured at 60°C), the reduction temperature is 85°C, and the reduction time is 30min; the reducing agent is added all at once, and aluminum sulfate is used as a desiliconizing agent, and the desiliconizing agent addition coefficient is Al / Si=0.4 (molar ratio). The molar ratio) is 1.52g, the reaction temperature of the silicon remover is 80℃, the reaction time is 30min, the standing time after the reaction is 12h, and the impurity removal residue is washed once with 20℃ clean water after solid-liquid separation. The washing filtrate is incorporated into the impurity removal liquid. The washing water volume is 100mL to ensure that the volume of the impurity removal liquid is roughly equal to the volume of the vanadium liquid before impurity removal; an oxidant is used for oxidation purification. The oxidant is 30% hydrogen peroxide, the addition amount is H2O2 / Cr=1 (molar ratio) is 2.79mL, the reaction pH is 12.4 (at 60℃), the reaction temperature is 60℃, the reaction time is 30min, Cr=0.14 / L, Si=0.08g / L in the purified liquid, and the vanadium loss is 2.6%.
[0054] Take the purified liquid to precipitate APV, dilute the solution to V of 30g / L, a total of 200mL, adjust pH to 6.0 for the first time, and adjust the pH temperature to 70℃. After adjusting the pH, add ammonium salt, the amount of ammonium salt added is TV / ammonium sulfate = 1.6 (mass ratio), which is 9.6g. Then carry out the second acid adjustment, adjust pH to 2.3 for the second time, then raise the temperature to 90℃ and keep warm for 45min. After solid-liquid separation, high-quality APV is obtained. The composition is shown in Table 6.2.
[0055] Table 6.2 Element V Cr Si Na K content / % 49.72 0.118 0.02 0.127 0.126 To precipitate AMV, there is no need to dilute the purified liquid, a total of 200 mL, adjust the pH to 9.5, adjust the pH temperature to 40°C, add ammonium salt after adjusting the pH, the amount of ammonium salt added is TV / ammonium sulfate = 4 (mass ratio), which is 40.68 g, keep warm at 30°C for 120 minutes, and the high-quality AMV after solid-liquid separation is obtained. The composition is shown in Table 6.3.
[0056] Table 6.3 Element V Cr Si Na K content / % 42.91 0.184 0.061 0.069 0.083 So far, various embodiments of the present disclosure have been described in detail. In order to avoid obscuring the concept of the present disclosure, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.
[0057] Although some specific embodiments of the present disclosure have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present disclosure. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present disclosure. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict.
Claims
1. A method for selectively reducing chromium and silicon with sodium vanadium solution, characterized in that: include: Step 1, adjusting the pH value of the sodium vanadium solution so that the pH value of the system solution is 10.5-11.5 at 60° C., or the pH value of the system solution is 11.3-12.7 at 20° C.-25° C., to obtain a pretreated sodium vanadium solution; Step 2, adding a predetermined amount of reducing agent to the pretreated sodium vanadium solution at one time to carry out a reduction reaction; Step 3: adding a silicon remover to the reaction system at the end of the reduction reaction to react and obtain a first intermediate reaction solution; Step 4: performing solid-liquid separation on the first intermediate reaction liquid, washing the solid phase with water and then adding it into the filtrate to obtain a decontamination liquid; Step 5: subjecting the impurity removal liquid to an oxidation purification treatment to obtain a purified liquid.
2. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: Also includes: Step 6: dilute the purified liquid to a vanadium content of 25 g / L-35 g / L, adjust the pH value to 5.0-6.0, the temperature to 20-70° C., and then add ammonium salt; Step 7: Adjust the pH value to 2.0-2.3 and then heat to 90-100°C for heat preservation and reaction, and then perform solid-liquid separation to obtain APV.
3. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 2, characterized in that: In step six, the amount of ammonium salt added is TV / ammonium sulfate = 1.2 to 2.0 by mass ratio.
4. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: Also includes: Step 6, adjusting the pH value of the purified liquid to 9.0-9.5 and the temperature to 20-40° C., and then adding ammonium salt; Step 7: After the reaction is carried out at 10-40°C, solid-liquid separation is performed to obtain AMV.
5. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 4, characterized in that: In step six, the amount of ammonium salt added is TV / ammonium sulfate = 2.5 to 5.0 by mass ratio.
6. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: In step one, If the pH value of the system solution is greater than 11.5 at 60°C, sulfuric acid is added to the system solution to adjust the pH value; If the pH value of the system solution is less than 10.5 at 60°C, add sodium hydroxide to the system solution to adjust the pH value, and the reaction must last for 10 to 60 minutes after the addition of sodium hydroxide; Preferably, the pH value of the system solution at 60° C. is 10.6-11.
0.
7. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: In step 2, the reducing agent is sodium hydrosulfide or sodium sulfide, and the amount of the reducing agent added is Cr / S=0.75-1.3 in terms of the molar ratio. The pH value of the reaction system at 60° C. is 10.5-11.5, the reaction temperature is 60° C.-95° C., and the reaction time is 30 min-90 min. Preferably, in step 2, the amount of reducing agent sodium hydrosulfide or sodium sulfide added is Cr / S=0.85-1.0, the reaction temperature is 60° C.-85° C., and the reaction time is 30 min-60 min.
8. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: In step three, the desiliconizing agent is aluminum sulfate. The amount of desiliconizing agent added is Al / Si=0.4-0.8 based on the molar ratio of substances. The reaction temperature is 60-95°C and the reaction time is 30-40min.
9. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: In step 4, the impurity removal residue obtained after solid-liquid separation is washed once with clean water at 20°C to 60°C, and the washing filtrate is added to the impurity removal liquid. The amount of washing water is the amount of water taken away by the impurity removal residue, and the volume of the impurity removal liquid is ensured to be equal to the volume of the sodium vanadium solution; Preferably, in step 4, the first intermediate reaction liquid obtained after the reaction is completed is subjected to solid-liquid separation without standing.
10. The method for selective reduction of chromium and silicon by sodium vanadium solution according to claim 1, characterized in that: In step 5, the oxidant for oxidation purification treatment is hydrogen peroxide with a mass concentration of 25% to 50%, and the amount added is H2O2 / Cr=1 to 2.5 in terms of the molar ratio. The pH value of the reaction system is 10.8 to 12.0 at 60°C, the reaction temperature is 30°C to 95°C, and the reaction time is 10min to 60min. Preferably, in step five, the pH value of the reaction system at 60° C. is 10.8 to 11.5, the temperature range is 60° C. to 85° C., and the reaction time is 20 min to 30 min.
Citation Information
Cited By
Method for preparing low-chromium low-potassium vanadium oxide from sodium vanadium oxide liquid
CN119660794A
Method for removing impurities phosphorus, chromium and silicon in sodium vanadium solution
CN120776142A
Sodium vanadium solution treatment method
CN120776143A
Method for co-removing chromium and silicon from sodium-containing vanadium solution by selective reduction
WO2026012038A1