5-series aluminum alloy for nuclear industry and manufacturing method of 5-series aluminum alloy
By controlling impurity elements and precisely controlling Mg, Cr, and Zr elements during the aluminum alloy smelting process, combined with thermal processing, the problem of performance deterioration of 5-series aluminum alloys in a neutron irradiation environment has been solved, and good mechanical properties and Neutron transmittance extends the service life of the structure.
Patent Information
- Application Number
- CN202411022499.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
AI Technical Summary
In a neutron irradiation environment, some impurity elements in 5 series aluminum alloys are prone to transmutation and produce gases, resulting in deterioration of alloy properties. It is difficult to ensure both neutron transmittance and mechanical properties with existing technology.
By controlling the content of impurity elements during the aluminum alloy smelting process, a protective layer mixed with pure water, water glass and oxides is used to precisely control the elemental composition of Mg, Cr and Zr, and perform thermal processing to reduce the content of impurity elements and improve the quality of the aluminum alloy. purity to achieve grain refinement.
It effectively reduces the generation of transmutation gas in a neutron irradiation environment, improves the mechanical properties, welding performance and neutron transmittance of aluminum alloys, and extends the service life of the structure.
Smart Images

Figure CN118726780A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aluminum alloys, and in particular relates to a 5 series aluminum alloy for nuclear industry and a manufacturing method thereof. Background Art
[0002] With the rapid development of civil nuclear power technology, aluminum alloys with high specific strength, specific stiffness and excellent hot and cold forming properties have been widely used in the nuclear industry. In application scenarios such as neutron reactors, in addition to requiring aluminum alloys as structural materials to have good mechanical properties, they also need to have good forming properties, welding properties and neutron permeability, and be able to maintain good structural stability in a neutron irradiation environment for a long time. Among various series of aluminum alloys, 1 series aluminum alloys and 5 series aluminum alloys have good neutron permeability, but the strength of 1 series aluminum alloys in the O state is relatively low, so neutron reactors generally use 5 series aluminum alloys as the main structural material. Under long-term neutron irradiation, some impurity elements in the alloy are prone to transmutation and produce gas, resulting in serious deterioration of alloy performance. Therefore, a method for manufacturing 5 series aluminum alloys is provided to reduce the generation of transmutation gas while ensuring neutron transmittance, which has positive significance for improving the service life and reliability of neutron reactor structures. Summary of the invention
[0003] The object of the present invention is to provide a method for manufacturing a 5 series aluminum alloy for nuclear industry, which can reduce the generation of transmutation gas of the 5 series aluminum alloy under neutron irradiation environment. The present invention also provides a 5 series aluminum alloy for nuclear industry.
[0004] According to an embodiment of one aspect of the present invention, a method for manufacturing a 5 series aluminum alloy for nuclear industry is provided, the method comprising the following steps:
[0005] Step a): providing a smelting device, the smelting device comprising a smelting crucible and a smelting tool; mixing pure water, water glass, aluminum oxide, and magnesium oxide in a weight ratio of pure water: water glass: aluminum oxide: magnesium oxide = (3-4): (0.8-1.0): (0.5-0.8): (0.5-0.8) to obtain a coating material; applying the coating material on the surface of the smelting crucible and the smelting tool and drying;
[0006] Step b): using pure aluminum, pure magnesium, Al-Cr master alloy, Al-Ti master alloy and Al-Zr master alloy as smelting raw materials to smelt in the smelting crucible to obtain an alloy ingot; the alloy ingot comprises, by weight, 2.4%-2.8% Mg, 0.15%-0.35% Cr, 0.02%-0.05% Zr, 0.02%-0.04% Ti, and the balance is Al and inevitable impurities; among the inevitable impurities, by weight, Si does not exceed 0.1%, Fe does not exceed 0.12%, Mn does not exceed 0.1%, Zn does not exceed 0.1%, Cu does not exceed 0.1%, Ga does not exceed 0.04%, Cd does not exceed 0.003%, B does not exceed 0.001%, Li does not exceed 0.008%, Co does not exceed 0.001%, other single weight impurities do not exceed 0.05%, and the total amount of the inevitable impurities does not exceed 0.15%;
[0007] Step c): homogenizing the alloy ingot and performing hot working and deformation treatment to obtain a finished aluminum material.
[0008] In the aluminum alloy for nuclear industry, on the one hand, it is necessary to strictly control the elements such as Li, Ga, Cd, Co, B that will undergo transmutation under neutron irradiation environment, otherwise helium bubbles will appear in the aluminum alloy structure, causing serious deterioration of the performance of aluminum-based structure; on the other hand, it is necessary to reduce the content of elements such as Cu, Mn, Zn, Fe, etc. to improve the neutron transmittance. This makes the selection of alloy components of 5 series aluminum alloy for nuclear industry restricted to a great extent, and it is impossible to improve the mechanical properties of aluminum alloy structure through existing strengthening technology routes such as Al-Ti-B, resulting in coarse alloy structure, low mechanical properties and fracture toughness. The manufacturing method provided by the above embodiment can effectively reduce the content of impurity elements introduced during the smelting process and improve the purity of aluminum alloy components; and by accurately controlling the composition range of Mg and Cr elements and adding a small amount of Zr elements, it is possible to achieve grain refinement in the aluminum alloy structure, and obtain a 5 series aluminum alloy for nuclear industry with good forming performance, welding performance, fracture toughness and good neutron irradiation tolerance.
[0009] Furthermore, in some embodiments, in the step a), the coating material is applied by heating the smelting crucible and the smelting tool to 150°C-180°C, uniformly coating the coating material, and drying the mixture at 180°C-300°C; the coating material thickness on the surface of the smelting crucible is 1mm-2mm, and the coating material thickness on the surface of the smelting tool is 0.5mm-1mm.
[0010] Furthermore, in some embodiments, in the step b), the smelting step includes a melting step, a mixing and refining step and a vacuum refining step, wherein in the melting step, the pure aluminum and all of the Al-Zr master alloy, the Al-Cr master alloy and the Al-Ti master alloy providing 60%-90% of the total Ti amount are added, heated and stirred evenly, and then the pure magnesium is added, and the surface scum is removed after it is fully melted; in the mixing and refining step, 95% of argon and 5% of chlorine are introduced for refining; in the vacuum refining step, the refining vacuum degree is controlled to be 800Pa-1800Pa, and after the vacuum refining step is completed, the remaining amount of the Al-Ti master alloy is added to melt and mix evenly.
[0011] Furthermore, in some embodiments, in the melting step, the Al-Zr master alloy, the Al-Cr master alloy and the Al-Ti master alloy are added and then heated to a temperature of 800°C-840°C, cooled to 730°C-750°C and then the pure magnesium is added; the mixed refining temperature is 720°C-740°C, and the refining time is 10min-30min; the vacuum refining temperature is 720°C-740°C, and the refining time is 10min-20min.
[0012] Furthermore, in some embodiments, after completing the vacuum refining step, a composition adjustment step is also included when adding the remaining amount of the Al-Ti master alloy, and the composition adjustment step supplements the burned alloy elements according to the composition of the sample before the furnace, followed by argon refining.
[0013] Furthermore, in some embodiments, the argon refining temperature is 700° C.-720° C., and the time is 10 min-15 min.
[0014] Furthermore, in some embodiments, in the step c), the homogenization treatment includes a first-stage treatment and a second-stage treatment, the first-stage treatment temperature is 390°C-430°C, and the second-stage treatment temperature is 510°C-530°C.
[0015] Furthermore, in some embodiments, the thermal processing includes hot rolling, hot extrusion or hot forging, and the heating temperature is 480°C-510°C.
[0016] According to an embodiment of another aspect of the present invention, there is provided a 5 series aluminum alloy for nuclear industry, which comprises, by weight, 2.4%-2.8% Mg, 0.15%-0.35% Cr, 0.02%-0.05% Zr, 0.02%-0.04% Ti, and the balance being Al and inevitable impurities; among the inevitable impurities, by weight, Si does not exceed 0.1%, Fe does not exceed 0.12%, Mn does not exceed 0.1%, Zn does not exceed 0.1%, Cu does not exceed 0.1%, Ga does not exceed 0.04%, Cd does not exceed 0.003%, B does not exceed 0.001%, Li does not exceed 0.008%, Co does not exceed 0.001%, other single weight impurities do not exceed 0.05%, and the total amount of the inevitable impurities does not exceed 0.15%.
[0017] Furthermore, in some embodiments, the 5 series aluminum alloy for nuclear industry is manufactured by the manufacturing method of the 5 series aluminum alloy for nuclear industry provided in any of the aforementioned embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a metallographic photograph of the surface structure of the alloy ingot in one embodiment;
[0019] Figure 2 This is a metallographic photograph of the alloy ingot T / 2 thickness structure in one embodiment;
[0020] Figure 3 This is a metallographic photograph of the surface structure of the finished aluminum material O-state plate in an embodiment;
[0021] Figure 4 This is a metallographic photograph of the structure of a finished aluminum material O-state plate T / 2 thickness in an embodiment;
[0022] Figure 5 This is a metallographic photograph of the structure at position D / 4 of the alloy ingot in another embodiment;
[0023] Figure 6 This is a metallographic photograph of the structure at position D / 2 of the alloy ingot in another embodiment;
[0024] Figure 7 This is a metallographic photograph of a cross section of a finished aluminum forging at T / 2 thickness in another embodiment;
[0025] Figure 8 This is a metallographic photograph of the longitudinal section structure of a finished aluminum forging with a thickness of T / 2 in another embodiment.
[0026] The purpose of the above embodiments is to explain the invention in detail so that those skilled in the art can understand the technical concept of the present invention, but it is not intended to limit the present invention. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings.
[0028] Mentioning "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present invention. The phrase appearing in various locations in the specification does not necessarily refer to the same embodiment, nor is it limited to mutually exclusive independent or alternative embodiments. It should be understood by those skilled in the art that the embodiments herein can be combined with other embodiments without structural conflicts. In the description herein, terms such as "first" and "second" are only used to distinguish different objects, and cannot be understood as indicating relative importance or limiting the number, specific order or primary and secondary relationship of the described technical features. In the description herein, the meaning of "multiple" is at least two.
[0029] With the rapid development of civil nuclear power technology, the nuclear industry has put forward higher and higher requirements for the comprehensive performance of metal materials, such as mechanical properties, reliability and economy. Due to the advantages of low cost, high specific strength and specific stiffness, and excellent cold and hot forming performance, various aluminum alloys have been widely used in the nuclear industry. In nuclear power facilities, as structural parts, in addition to the strength performance requirements, structural materials also need to have good neutron irradiation resistance, and it is not easy to transmute and produce gas inside after neutron irradiation; at the same time, as non-shielding materials, they should also have good neutron permeability. Among conventional aluminum alloy grades, 1 series aluminum alloys and 5 series aluminum alloys have better neutron permeability, but the steady-state (O state) strength of 1 series aluminum alloys is low, which is difficult to meet the structural strength requirements of nuclear power facilities. Therefore, 5 series aluminum alloys have better application prospects.
[0030] Due to the neutron irradiation effect, if there are elements such as Li, Ga, Cd, Co, and B in the aluminum alloy matrix, they are prone to transmutation under long-term service conditions and produce helium bubbles. The accumulation of helium bubbles in the aluminum alloy matrix will seriously damage the organizational strength. On the other hand, elements such as Cu, Mn, Zn, and Fe will hinder neutron penetration, resulting in reduced neutron transmittance. Therefore, when using 5-series aluminum alloys to manufacture the main structure of a neutron reactor, the content of the above elements needs to be controlled.
[0031] However, elements such as Cu, Li, and B are commonly used strengthening elements in aluminum alloys. For example, in some 5-series aluminum alloys, Al-Ti-B wires are introduced to refine the cast grains to achieve strengthening effects. The lack of the above elements results in coarse structure of 5-series aluminum alloys, reduced forming performance and fracture toughness, which restricts the application scope of 5-series aluminum alloys. On the other hand, in the existing aluminum alloy manufacturing process, some of the above impurity elements can easily be mixed into the aluminum alloy structure through smelting furnace refractory bricks and other channels, resulting in a decrease in the neutron irradiation performance of the aluminum alloy.
[0032] In order to solve the above problems, an embodiment of one aspect of the present invention provides a method for manufacturing a 5-series aluminum alloy for the nuclear industry, which can reduce the content of unfavorable elements in the aluminum alloy while improving the mechanical properties of the aluminum alloy. The method comprises the following steps:
[0033] Step a): Prepare a protective layer for smelting equipment. In order to avoid the seepage of impurities in refractory bricks and the influence of residual impurities in the gaps of traditional aluminum alloy smelting furnaces on the control of impurity elements, a smelting crucible is used for aluminum alloy smelting, and a protective layer is applied to the surface of the smelting crucible and the surface of the smelting tool in contact with the aluminum alloy melt before smelting. Pure water, water glass, aluminum oxide, and magnesium oxide are mixed in a weight ratio of pure water: water glass: aluminum oxide: magnesium oxide = (3-4): (0.8-1.0): (0.5-0.8): (0.5-0.8) to obtain a coating material; the coating material is then applied to the surface of the smelting crucible and the smelting tool and dried to form a protective layer. In a preferred embodiment, during the coating process, the melting crucible and the melting tool are first heated to 150°C-180°C and dried, and then the coating material is evenly sprayed on the surface, and after the coating material completely covers the surface, it is dried in a drying furnace at 180°C-300°C, and the coating is applied once or multiple times until the coating material thickness on the surface of the melting crucible is 1mm-2mm, and the coating material thickness on the surface of the melting tool is 0.5mm-1mm. The protective layer can effectively prevent impurities from mixing into the aluminum alloy melt and improve the purity of the finished aluminum alloy.
[0034] Step b): smelting aluminum alloy. Pure aluminum ingot, pure magnesium ingot and Al-Cr master alloy, Al-Ti master alloy and Al-Zr master alloy are used as raw materials for smelting in a crucible to obtain alloy ingot. The alloy ingot includes 2.4%-2.8% Mg, 0.15%-0.35% Cr, 0.02%-0.05% Zr, 0.02%-0.04% Ti by weight, and the balance is Al and inevitable impurities. Among them, the content of impurity elements needs to be strictly controlled, and the inevitable impurities should meet the following requirements by weight: Si does not exceed 0.1%, Fe does not exceed 0.12%, Mn does not exceed 0.1%, Zn does not exceed 0.1%, Cu does not exceed 0.1%, Ga does not exceed 0.04%, Cd does not exceed 0.003%, B does not exceed 0.001%, Li does not exceed 0.008%, Co does not exceed 0.001%, other single weight impurities do not exceed 0.05%, and the total amount of inevitable impurities does not exceed 0.15%.
[0035] In a preferred embodiment, smelting includes a melting step, a mixing refining step and a vacuum refining step.
[0036] In the melting step, firstly, pure aluminum ingots and all Al-Zr master alloys, Al-Cr master alloys and Al-Ti master alloys providing 60%-90% of the total amount of Ti are added, and after being fully melted, they are evenly stirred by electromagnetic stirring, and then pure magnesium ingots are added and fully melted, and then surface scum is removed. In a further preferred embodiment, the heating temperature after adding Al-Zr alloy and Al-Cr alloy is 800℃-840℃, and the electromagnetic stirring state is kept for 15min-45min; then the temperature is lowered to 730℃-750℃ and pure magnesium is added.
[0037] During the mixed refining process, 95% argon and 5% chlorine are introduced. In a further preferred embodiment, the refining temperature is controlled at 720° C.-740° C., and the refining time is 10 min-30 min.
[0038] The vacuum degree during vacuum refining is 800Pa-1800Pa. After vacuum refining is completed, the remaining Al-Ti master alloy is added to melt and mix evenly. In a further preferred embodiment, the vacuum refining temperature is controlled at 720℃-740℃, the refining time is 10min-20min, and the burned alloy elements are supplemented according to the composition of the sample before the furnace when the remaining Al-Ti alloy is added to adjust the alloy composition to the target range, and then argon refining is performed at 700℃-720℃ for 10min-20min. The staged addition of different components during the smelting process helps to reduce the loss of volatile alloy components during high-temperature smelting and improve the control accuracy of alloy components.
[0039] During the refining process, the composition is adjusted and slag is removed, and the alloy ingot is obtained by semi-continuous casting.
[0040] Step c): Finished product processing. The alloy ingot is subjected to homogenization heat treatment, and then hot processed to obtain finished aluminum material. In a preferred embodiment, the homogenization treatment adopts a two-stage heating process, the first stage heat treatment temperature is 390℃-430℃, and the second stage heat treatment temperature is 510℃-530℃. After the alloy ingot after homogenization treatment is peeled or milled, it is processed and formed by hot rolling, hot extrusion or hot forging, and the heating temperature is 480℃-510℃ to obtain a finished aluminum material. The finished aluminum material is annealed and subjected to 4%-15% cold deformation processing to obtain an aluminum alloy product. Cold deformation processing can adopt different processes such as pre-stretching, cold pressing, cold rolling, etc.
[0041] An embodiment of another aspect of the present invention provides a 5 series aluminum alloy for nuclear industry, which comprises, by weight: 2.4%-2.8% Mg, 0.15%-0.35% Cr, 0.02%-0.05% Zr, 0.02%-0.04% Ti, and the balance is Al and inevitable impurities; among the inevitable impurities, by weight, Si does not exceed 0.1%, Fe does not exceed 0.12%, Mn does not exceed 0.1%, Zn does not exceed 0.1%, Cu does not exceed 0.1%, Ga does not exceed 0.04%, Cd does not exceed 0.003%, B does not exceed 0.001%, Li does not exceed 0.008%, Co does not exceed 0.001%, other single weight impurities do not exceed 0.05%, and the total amount of inevitable impurities does not exceed 0.15%.
[0042] The aluminum alloy achieves grain refinement through the addition of Ti element, and produces precipitation hardening effect through Al3Ti precipitation; Zr element can inhibit the growth of recrystallized grains during annealing, and can achieve precipitation strengthening by forming Al3Zr precipitation; further, Mg element can produce solid solution strengthening effect, and the addition of Cr element can achieve microalloying of alloy structure, thereby improving the overall mechanical properties of aluminum alloy. The aluminum alloy has extremely strict requirements on the content of impurity elements such as Cd, B, Li, and Co. It is difficult for traditional refractory brick gas furnaces to effectively control impurity elements, and a manufacturing method with more precise control of impurity components should be adopted. In a preferred embodiment, the aluminum alloy is manufactured using the manufacturing method of the 5 series aluminum alloy for nuclear industry provided in any of the aforementioned embodiments.
[0043] In a preferred embodiment, the manufacturing process of the aluminum alloy is as follows.
[0044] The target composition ratio of the aluminum alloy is: Mg 2.4%, Cr 0.18%, Zr 0.03%, Ti 0.03%, Si 0.07%, Fe 0.10%, and the balance is Al.
[0045] First, high-purity aluminum ingots, high-purity magnesium ingots, Al5Zr alloys, Al2Cr alloys and Al5Ti alloys are selected according to the chemical composition. 60kg of pure water, 20kg of water glass, 10kg of high-purity alumina powder and 10kg of high-purity magnesium oxide powder are mixed and uniformly configured as coating materials. The stainless steel crucible and iron smelting tool are heated to 180℃ and dried, and the coating material is evenly sprayed, and then dried at 200℃. The process is repeated several times until the protective layer thickness of the inner surface of the crucible reaches 1.5mm and the protective layer thickness of the smelting tool surface reaches 0.6mm.
[0046] According to the composition ratio, pure aluminum ingots, Al5Zr alloy, Al2Cr alloy and Al5Ti alloy accounting for 2 / 3 of the total Ti are placed in a crucible and heated until fully melted. The temperature is controlled at 820°C and kept warm for 20 minutes under electromagnetic stirring; then the temperature is lowered to 730°C, and the magnesium ingot is added to fully melt and the slag is removed. Next, the temperature is maintained at 730°C, and high-purity argon + 5% high-purity chlorine is used for 10 minutes of mixed refining; after the slag is removed, vacuum refining is carried out, the vacuum degree is controlled at 1100Pa, and the refining time is 15 minutes. Take the sample before the furnace to test the composition, and supplement the remaining burned alloy elements while adding the remaining Al5Ti alloy, and finally carry out argon refining in high-purity argon for 10 minutes.
[0047] After refining, the temperature of the aluminum liquid is controlled to 710°C, and the alloy melt is introduced into a crystallizer and cast into a flat ingot with a specification of δ420×1320mm.
[0048] The ingot was homogenized in an annealing furnace with air circulation. A two-stage homogenization treatment was adopted, with the first stage treatment temperature at 400°C for 8 hours and the second stage treatment temperature at 510°C for 24 hours.
[0049] The aluminum ingot after homogenization treatment is milled, heated at 480°C for 10 hours, and hot-rolled into 40mm plates. The plate slices are heated to 360°C in an annealing furnace for 1 hour, and air-cooled to room temperature to obtain finished aluminum plates.
[0050] The chemical composition of the aluminum plate was tested, and the results are shown in Table 1. It can be seen that the aluminum alloy manufacturing method used in the embodiment achieves accurate control of the alloying elements and impurity components of the aluminum alloy.
[0051] element Fe Cu Mn Mg Zn Ti Cr Content wt% 0.01 0.01 0.01 2.38 0.02 0.03 0.18 element Cd Ga B Li Co Si Zr Content wt% 0.0003 0.001 0.00001 0.001 0.0008 0.06 0.028
[0052] Table 1 Chemical composition of aluminum alloy plate
[0053] The aluminum plate was tested for mechanical properties, bending properties, corrosion properties and mechanical properties of welded joints. The results are shown in Table 2.
[0054]
[0055]
[0056] Table 2 Aluminum alloy plate performance test results
[0057] Metallographic analysis of the alloy ingot surface Figure 1 As shown, metallographic analysis was performed at T / 2 (T is the total thickness of the alloy ingot) of the ingot. Figure 2 As shown. It can be seen that the alloy structure is uniform, without inclusions or impurities. The metallographic analysis of the surface of the O-state plate is as follows Figure 3As shown in the figure, the metallographic analysis of the thickness position of the O-state plate T / 2 (T is the plate thickness) is as follows Figure 4 As shown in Figure 2, it can be seen that the rolled plate has a uniform and fine structure, and sufficient recrystallization has occurred.
[0058] Without adding elements that may cause the production of transmutation gas and elements that are not conducive to neutron permeability, the O-state plate has good mechanical properties and welding properties, as well as good corrosion resistance, meeting the performance requirements of structural materials for nuclear power facilities and being suitable for the manufacture of nuclear power equipment in a neutron irradiation environment.
[0059] In another preferred embodiment, the manufacturing process of the aluminum alloy is as follows:
[0060] The target composition ratio of the aluminum alloy is: Mg 2.8%, Cr 0.20%, Zr 0.03%, Ti 0.02%, Si 0.08%, Fe 0.12%, and the balance is Al.
[0061] First, high-purity aluminum ingots, high-purity magnesium ingots, Al5Zr alloys, Al2Cr alloys and Al5Ti alloys are selected according to the chemical composition. 60kg of pure water, 16kg of water glass, 12kg of high-purity alumina powder and 12kg of high-purity magnesium oxide powder are mixed and uniformly configured as coating materials. The stainless steel crucible and iron smelting tool are heated to 180℃ and dried, and the coating material is evenly sprayed, and then dried at 210℃. Repeat several times until the protective layer thickness of the inner surface of the crucible reaches 2mm and the protective layer thickness of the smelting tool surface reaches 1mm.
[0062] According to the composition ratio, pure aluminum ingots, Al5Zr alloy, Al2Cr alloy and Al5Ti alloy accounting for 1 / 2 of the total amount are placed in a crucible and heated until fully melted. The temperature is controlled at 810℃ and kept warm for 30 minutes under electromagnetic stirring; then the temperature is lowered to 730℃, and magnesium ingots are added to fully melt and the slag is removed. Next, the temperature is maintained at 730℃, and high-purity argon + 5% high-purity chlorine is used for mixed refining for 15 minutes; after the slag is removed, vacuum refining is carried out, the vacuum degree is controlled at 800Pa, and the refining time is 18 minutes. Take the sample before the furnace to test the composition, and supplement the remaining burned alloy elements while adding the remaining Al5Ti alloy, and finally carry out argon refining in high-purity argon for 10 minutes.
[0063] After refining, the temperature of the aluminum liquid is controlled to 710°C, and the alloy melt is introduced into the crystallizer and cast into a round ingot with a specification of Φ500mm.
[0064] The ingot was homogenized in an annealing furnace with air circulation. A two-stage homogenization treatment was adopted, with the first stage treatment temperature at 430°C for 7 hours and the second stage treatment temperature at 520°C for 20 hours.
[0065] The aluminum ingot after homogenization treatment is peeled, heated at 490℃ for 6h, taken out of the furnace for two upsetting, two drawing and square repair to form a free forging with a thickness of 100mm, the annealing furnace is heated to 360℃, the free forging is loaded, and the free forging is heated to 370℃ and kept for 1.5h before being taken out of the furnace and air-cooled to room temperature to obtain the finished forging. The finished forging is cold-pressed on a press, and the cold-pressing deformation is 7%.
[0066] The chemical composition of the aluminum plate was tested, and the results are shown in Table 3. It can be seen that the aluminum alloy manufacturing method adopted in the embodiment achieves accurate control of the alloying elements and impurity components in the aluminum alloy.
[0067] element Fe Cu Mn Mg Zn Ti Cr Content wt% 0.07 0.02 0.02 2.77 0.03 0.02 0.21 element Cd Ga B Li Co Si Zr Content wt% 0.0001 0.008 0.00001 0.001 0.0006 0.05 0.03
[0068] Table 3 Chemical composition of aluminum alloy forgings
[0069] The mechanical properties, corrosion properties and mechanical properties of the welded joints of the aluminum plate were tested, and the results are shown in Table 4.
[0070]
[0071]
[0072] Table 4 Performance test results of aluminum alloy forgings
[0073] Metallographic analysis was performed on the alloy ingot at D / 4 (D is the diameter of the alloy ingot). Figure 5 As shown, metallographic analysis was performed at D / 2 of the ingot. Figure 6 As shown. It can be seen that the alloy structure is uniform, without inclusions or impurities. Metallographic analysis of the cross section of the forging T / 2 (T is the thickness of the forging) is as follows Figure 7 As shown in the figure, metallographic analysis was performed on the longitudinal section of the forging T / 2 thickness. Figure 8 As shown in the figure, it can be seen that the forging structure is uniform and fine, and sufficient recrystallization has occurred. The cross-sectional and longitudinal sectional structures have similar morphologies without obvious anisotropy.
[0074] Without adding elements that may cause the production of transmutation gas and elements that are not conducive to neutron permeability, this forging has good mechanical properties and welding properties, as well as good corrosion resistance, meeting the performance requirements of structural materials for nuclear power facilities and being suitable for the manufacture of nuclear power equipment in a neutron irradiation environment.
[0075] The purpose of the above embodiments is to further explain the present invention in detail in conjunction with the accompanying drawings so that those skilled in the art can understand the technical concept of the present invention. Within the scope of the present invention, the optimization or equivalent replacement of the method steps involved, and the combination of the implementation methods in different embodiments without conflict of structure and principle, all fall within the protection scope of the present invention.
Claims
1. A method for producing a 5 series aluminum alloy for nuclear industry, characterized in that: The following steps are involved: Step a): providing a smelting device, wherein the smelting device comprises a smelting crucible and a smelting tool; Pure water, water glass, aluminum oxide, and magnesium oxide are mixed in a weight ratio of pure water: water glass: aluminum oxide: magnesium oxide = (3-4): (0.8-1.0): (0.5-0.8): (0.5-0.8) to obtain a coating material; Applying the coating material to the surface of the smelting crucible and the smelting tool and drying them; Step b): using pure aluminum, pure magnesium, Al-Cr master alloy, Al-Ti master alloy, Al-Zr master alloy as smelting raw materials and smelting in the smelting crucible to obtain an alloy ingot; The alloy ingot comprises, by weight, 2.4%-2.8% Mg, 0.15%-0.35% Cr, 0.02%-0.05% Zr, 0.02%-0.04% Ti, and the balance is Al and unavoidable impurities; Among the inevitable impurities, by weight, Si does not exceed 0.1%, Fe does not exceed 0.12%, Mn does not exceed 0.1%, Zn does not exceed 0.1%, Cu does not exceed 0.1%, Ga does not exceed 0.04%, Cd does not exceed 0.003%, B does not exceed 0.001%, Li does not exceed 0.008%, Co does not exceed 0.001%, other single weight impurities do not exceed 0.05%, and the total amount of the inevitable impurities does not exceed 0.15%; Step c): homogenizing the alloy ingot and performing hot working and deformation treatment to obtain a finished aluminum material.
2. The method for producing a 5 series aluminum alloy for nuclear industry according to claim 1, characterized in that: In the step a), the coating material is applied by heating the smelting crucible and the smelting tool to 150°C-180°C and then evenly applying the coating material, and drying at 180°C-300°C; the coating material thickness on the surface of the smelting crucible is 1mm-2mm, and the coating material thickness on the surface of the smelting tool is 0.5mm-1mm.
3. The method for producing a 5 series aluminum alloy for nuclear industry according to claim 1, characterized in that: In the step b), the smelting step includes a melting step, a mixing refining step and a vacuum refining step. Wherein, in the melting step, the pure aluminum and all of the Al-Zr master alloy, the Al-Cr master alloy and the Al-Ti master alloy providing 60%-90% of the total Ti content are added, heated and stirred evenly, and then the pure magnesium is added, and the surface scum is removed after being fully melted; In the mixed refining step, 95% argon and 5% chlorine are introduced for refining; In the vacuum refining step, the refining vacuum degree is controlled to be 800Pa-1800Pa. After the vacuum refining step is completed, the remaining amount of the Al-Ti master alloy is added to be melted and mixed evenly.
4. The method for producing a 5-series aluminum alloy for nuclear industry according to claim 3, characterized in that: In the melting step, the Al-Zr master alloy, the Al-Cr master alloy and the Al-Ti master alloy are added and heated to a temperature of 800° C.-840° C., and then cooled to 730° C.-750° C. before adding the pure magnesium; The mixing and refining temperature is 720°C-740°C, and the refining time is 10min-30min; The vacuum refining temperature is 720° C.-740° C., and the refining time is 10 min-20 min.
5. The method for producing a 5-series aluminum alloy for nuclear industry according to claim 3 or 4, characterized in that: After the vacuum refining step is completed, a composition adjustment step is also included when adding the remaining amount of the Al-Ti master alloy, wherein the burned alloy elements are supplemented according to the composition of the sample before the furnace, and then argon refining is performed.
6. The method for producing 5 series aluminum alloy for nuclear industry according to claim 5, characterized in that: The argon refining temperature is 700° C.-720° C., and the time is 10 min-15 min.
7. The method for producing 5 series aluminum alloy for nuclear industry according to claim 1, characterized in that: In the step c), the homogenization treatment includes a first-stage treatment and a second-stage treatment, the first-stage treatment temperature is 390°C-430°C, and the second-stage treatment temperature is 510°C-530°C.
8. The method for producing a 5-series aluminum alloy for nuclear industry according to claim 1 or 7, characterized in that: The thermal processing includes hot rolling, hot extrusion or hot forging, and the heating temperature is 480°C-510°C.
9. A 5 series aluminum alloy for nuclear industry, characterized in that: The composition includes, by weight, 2.4%-2.8% Mg, 0.15%-0.35% Cr, 0.02%-0.05% Zr, 0.02%-0.04% Ti, and the balance is Al and inevitable impurities; among the inevitable impurities, by weight, Si does not exceed 0.1%, Fe does not exceed 0.12%, Mn does not exceed 0.1%, Zn does not exceed 0.1%, Cu does not exceed 0.1%, Ga does not exceed 0.04%, Cd does not exceed 0.003%, B does not exceed 0.001%, Li does not exceed 0.008%, Co does not exceed 0.001%, other single weight impurities do not exceed 0.05%, and the total amount of the inevitable impurities does not exceed 0.15%.
10. The 5 series aluminum alloy for nuclear industry according to claim 9, characterized in that: The 5-series aluminum alloy for the nuclear industry is manufactured by the method for manufacturing the 5-series aluminum alloy for the nuclear industry according to any one of claims 1 to 8.
Citation Information
Cited By
Aluminum alloy for simulating neutron irradiation transmutation silicon effect and manufacturing method thereof
CN120099335A
An aluminum alloy simulating the effect of neutron irradiation-induced transmutation of silicon and a manufacturing method thereof
CN120099335B