Steel with excellent nitriding performance for high-strength aluminum-coated plate strip substrate and production method thereof

By optimizing the chemical composition and adding alloy elements to the steel used for aluminum-clad plate and strip substrates, the problems of insufficient strength and bonding performance in the existing technology are solved, and an aluminum-clad plate and strip substrate with high strength and good steel-aluminum bonding properties is achieved. Meet the needs of high temperature nitriding treatment and cost reduction.

CN118726833AActive Publication Date: 2024-10-01BAOSHAN IRON & STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310328770.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

The existing steel used for aluminum-clad panels and substrates has low strength or poor steel-aluminum bonding properties, which cannot meet the high-strength requirements after nitriding treatment, and the production cost is high.

Method used

High-strength aluminum-clad plate and substrate steel with specific chemical composition, content range is C: 0.01~0.07%, Si≤0.005%, Mn: 0.4~1.2%, P: 0.008~0.020%, Cr: 0.03~0.60%, N: 0.003~0.010%, O: 0.011~0.05%, Cu: 0.01~0.15%, and select to add Ti, Nb, V and other alloying elements to improve the yield strength and tensile strength through solid solution strengthening and phase transformation strengthening, and optimize the steel Aluminum bonding properties.

Benefits of technology

It has achieved yield strength ≥280MPa, tensile strength ≥340MPa, and elongation ≥30%, meeting the high-strength requirements after high-temperature nitriding treatment, reducing production costs, and improving the steel-aluminum bonding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726833A_ABST
    Figure CN118726833A_ABST
Patent Text Reader

Abstract

The invention discloses steel with excellent nitriding performance for a high-strength aluminum-coated plate strip substrate and a production method of the steel. The steel comprises the following chemical components in percentage by weight: 0.01-0.07% of C, 0 < Si < = 0.005%, 0.4-1.2% of Mn, 0.008-0.020% of P, < = 0.008% of S, 0 < Al < = 0.005%, 0.03-0.60% of Cr, 0.003-0.010% of N, 0.01-0.05% of O, 0.01-0.15% of Cu, 0.001-0.004% of Ca, one or more of 0.01-0.06% of Ti, 0.01-0.03% of Nb and 0.01-0.03% of V, and the balance of Fe and inevitable impurities. Meanwhile, the condition that 0.5 C + 6.86 N + O + 0.05 Cu + 0.047 Cr-0. 89 Al-1.15 Si is larger than or equal to 0.085 is met; 150 (C-0.01) + 60P + 300N + 5Mn + 3Cr is greater than or equal to 7.0. The yield strength is larger than or equal to 280 MPa, the tensile strength is larger than or equal to 340 MPa, the ductility is larger than or equal to 30%, high strength and excellent plasticity and aluminum coating performance are achieved, an aluminum-coated plate strip produced through the base plate has excellent surface quality and high strength, the subsequent high-temperature nitriding treatment process requirement can be met, and the base plate is mainly used for production of frying pans or other aluminum-coated plate strips with the high-strength requirement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ultra-low carbon steel manufacturing, and specifically relates to a high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance and a production method thereof. Background Art

[0002] Aluminum-clad strip is a composite strip formed by rolling and deforming the aluminum layer on the surface of the strip at room temperature. It has both steel-aluminum structure and steel-aluminum-steel or aluminum-steel-aluminum structure. Aluminum-clad strip has the strength of steel and the characteristics of aluminum such as good heat dissipation, corrosion resistance, light weight and beautiful appearance. Compared with pure aluminum materials, it greatly reduces the cost, so it is widely used in radiators, corrosion-resistant pipes, home appliance panels and other fields, and gradually expanded to automobile engine protective covers, new energy vehicle parts, atmospheric corrosion resistance, cookers, construction and other fields.

[0003] Aluminum-clad substrates are not only required to have good steel-aluminum bonding properties, but also to have high surface and high strength. In the field of kitchenware, new frying pans with a steel-aluminum-steel structure have both the strength of steel and the good heat dissipation of Al, thus avoiding the defects of uneven heat dissipation and easy sticking of iron frying pans, and are more lightweight. In order to extend the service life, the surface of the material is usually nitrided to increase the hardness, which requires the substrate to adapt to nitriding and form a high-hardness nitriding layer on the surface. At the same time, the matrix still maintains high strength after high-temperature treatment.

[0004] With the development of aluminum-clad substrates and the application of aluminum-clad strips, numerous patents for composite strips and steel for substrates have been developed.

[0005] Chinese patent CN102019727 discloses "aluminum-clad steel strip for cooler and its preparation method and steel strip and aluminum alloy strip used therein". The patent introduces the method and process for producing composite strips. Although the substrate used is mentioned, it is mainly used to produce aluminum-clad strips with a thickness of about 1.5 mm, which have a low yield strength and do not meet the requirements of nitriding processing.

[0006] The substrate used in the production of aluminum-clad steel strips deforms together with the aluminum layer during the production of the composite strips, so it is required to have strength and plasticity comparable to aluminum, especially excellent plasticity, and good steel-aluminum bonding performance, and has specific requirements on composition. Therefore, existing conventional low-strength steel is difficult to use in the production of aluminum-clad strips.

[0007] Japanese patent JP2005281806 discloses "Low yield point steel with excellent toughness and its production method". The steel disclosed belongs to low alloy structural steel with low yield strength and high elongation, and the yield strength is generally around 200MPa. The resulting product is generally a thick plate product. In terms of composition design, one or more components of alloys such as chromium (Cr), molybdenum (Mo), nickel (Ni), copper (Cu), and boron (B) are added based on low carbon (C)-silicon (Si)-manganese (Mn). The strength of the resulting steel is low, and there is no mention of aluminum coating performance. It is mainly used for the production of seismic dampers.

[0008] The Chinese patent CN111349869A discloses "a high-strength steel for aluminum-clad substrate and its production method", and the obtained steel has a yield strength of 210-290MPa, a tensile strength ≥320MPa, and an elongation ≥40%, and its strength is lower than that of the present invention. By adding a higher content of P element, the diffusion of Al is inhibited, thereby improving the steel-aluminum bonding performance. However, the steel involved is used for the production of aluminum-clad materials, and there is still an iron-aluminum compound layer with a thickness of no more than 5μm at the steel-aluminum interface. In addition, too high P content can easily lead to cold brittleness problems, which is not conducive to the forming and welding performance of the steel plate. Moreover, the patent does not mention nitriding treatment, and does not have the characteristic of maintaining high strength after nitriding treatment.

[0009] Chinese patent CN107881426A discloses "a high-strength aluminum-clad strip and its manufacturing method", which ensures the steel-aluminum bonding performance by controlling N, O and Si, and has a yield strength of 280-400MPa. It is mainly used in the production of radiators, home appliance panels, etc. However, the application has no nitriding characteristics, and the performance after high-temperature nitriding is unknown.

[0010] Chinese patent CN114250411A discloses "a steel with aluminum-clad plate with base plate for kitchenware and its production method". Although the steel plate involves nitriding process, its yield and tensile strengths do not exceed 280MPa and 380MPa respectively. At the same time, the patent requires that the carbon content be controlled below 0.005%, and the P and S contents are limited to no more than 0.012% and 0.006% respectively, which increases the difficulty of steelmaking and production costs. The patent mainly improves the strength during nitriding through the precipitation strengthening of V and Mo, and does not mention the nitriding adaptability of the base plate. In terms of function, the steel is limited to the processing of aluminum-clad materials for frying pans, and is not suitable for the production of other aluminum-clad materials with high strength requirements.

[0011] From the comparison with the existing patents, it can be found that the steel used for the existing aluminum-clad plate strip substrate has either low strength, or poor steel-aluminum bonding performance, or does not meet the nitriding treatment requirements. Summary of the invention

[0012] The purpose of the present invention is to provide a high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance and a production method thereof, wherein the steel has a yield strength of ≥280MPa, a tensile strength of ≥340MPa, and an elongation of ≥30%, and has high strength and excellent plasticity and aluminum-clad performance. The aluminum-clad plate strip produced using the substrate has excellent surface quality and high strength, can meet the subsequent high-temperature nitriding treatment process requirements, and is mainly used for the production of frying pans or other aluminum-clad plates with high strength requirements.

[0013] To achieve the above object, the technical solution of the present invention is:

[0014] A high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance, the chemical composition weight percentage of which is: C: 0.01-0.07%, 0<Si≤0.005%, Mn: 0.4-1.2%, P: 0.008-0.020%, S≤0.008%, 0<Al≤0.005%, Cr: 0.03-0.60%, N: 0.003-0.010%, O: 0.011-0.05%, Cu: 0.01-0.15%, Ca: 0.001-0.004%, and one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, and V: 0.01-0.03% are selectively added, and the balance contains Fe and other inevitable impurities; and at the same time,

[0015] 0.5C+6.86N+O+0.05Cu+0.047Cr-0.89Al-1.15Si≥0.085;

[0016] 150(C-0.01)+60P+300N+5Mn+3Cr≥7.0.

[0017] Furthermore, the balance is Fe and other inevitable impurities.

[0018] The microstructure of the steel for the aluminum-clad plate strip substrate of the present invention is a uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.

[0019] The steel used for the aluminum-clad plate substrate of the present invention has a yield strength of ≥280MPa, a tensile strength of ≥340MPa, and an elongation of ≥30%.

[0020] The steel for the high-strength aluminum-clad plate with excellent nitriding performance described in the present invention requires a yield strength and a tensile strength of more than 280MPa and 340MPa respectively, an elongation of more than 30%, and good steel-aluminum bonding performance. The aluminum-clad material prepared therefrom still has high strength requirements after high-temperature heat treatment such as nitriding. For this purpose, the content of specific alloy elements must be limited as much as possible.

[0021] In the chemical composition design of the steel for the aluminum-clad plate strip substrate of the present invention:

[0022] C improves yield strength through solid solution strengthening and phase transformation strengthening, while inhibiting the diffusion of Al in steel and the formation of iron-aluminum compounds. Too high C content is not good for the subsequent processing properties of the material such as stamping and drawing; however, higher C is prone to segregation at defect locations such as dislocations, which is not good for surface quality. According to the actual steelmaking process, the C content is controlled to be 0.01-0.07%.

[0023] Si is a deoxidizing element and also a solid solution strengthening element, which increases the yield strength and reduces the elongation. Although an appropriate amount of Si is beneficial to improving the bonding performance of the steel-aluminum interface, it will also weaken the inhibitory effect of O (oxygen) on the formation of a brittle compound layer at the steel-aluminum interface, so 0<Si≤0.005% is controlled.

[0024] Mn is also a common strengthening element in steel. It increases yield strength and reduces elongation through solid solution strengthening. An appropriate amount of Mn can combine with S in steel to form MnS, reducing the hot brittleness of steel. However, excessive Mn solid solution hinders the recovery of the structure and inhibits the growth of recrystallized grains, reducing the γ texture (ND∥ <111> ) strength, which is very unfavorable for the stamping forming of steel plates and will also increase costs, so its content is controlled at 0.40-1.20%.

[0025] P is generally controlled as an impurity element in steel, and is only allowed to be added in a few special-purpose steels. For example, adding no more than 0.15% P to sulfur-containing free-cutting steel makes it solid-dissolved in ferrite, causing strengthening and embrittlement to improve its cutting performance. In addition, P is the main corrosion-resistant element in traditional atmospheric corrosion-resistant steel. P in steel can accelerate the uniform dissolution of steel and Fe 2+ The oxidation rate is high, which helps to form a uniform FeOOH rust layer on the steel surface and promotes the formation of amorphous iron oxyhydroxide FeO x (OH) 3-2x Dense protective film effectively improves the atmospheric corrosion resistance of steel. Generally, the corrosion resistance is best when the P content is 0.08% to 0.15%, so P is added as a corrosion-resistant element in some early atmospheric corrosion-resistant steels. However, too much P causes "cold brittleness" of steel, reduces plasticity and impact toughness, and deteriorates the welding performance and cold bending performance of steel, so the amount of addition is clearly limited for steel types with requirements for low-temperature impact toughness or high forming performance. In recent years, some atmospheric corrosion-resistant steels have also reduced the P content and selected other alternative corrosion-resistant elements to ensure corrosion resistance, and even controlled it as an impurity element, requiring the content to be ≤0.015%, but controlling the P content at such a low level will increase the difficulty of steelmaking and increase manufacturing costs. The present invention considers that P improves the strength of the substrate for aluminum-clad plates and strips and the strength after nitriding by solid solution strengthening, phase transformation strengthening, etc., and uses it to improve the steel-aluminum bonding performance. Therefore, 0.008 to 0.020% of P is added in the present invention.

[0026] S is detrimental to the performance of steel, and can easily cause "hot brittleness" of steel, reduce the low-temperature toughness of steel, and deteriorate the steel-aluminum interface bonding performance. The addition of Mn can form MnS with S, and increasing the Mn / S ratio can improve hot ductility. It is required to control its content at a minimum level. Considering that too low a controlled content increases the difficulty of steelmaking and production costs, it is required to control the S content below 0.008%.

[0027] Al is an important deoxidizing element in steel, but higher Al content is easy to diffuse into the steel-aluminum bonding interface, deteriorating the interface bonding strength. Therefore, its content must be controlled within a certain range, so 0<Al≤0.005%.

[0028] Cr forms a continuous solid solution with Fe in steel, which has a solid solution strengthening effect, and forms various types of carbides with C, such as M3C, M7C3 and M 23 C6, etc., produce a secondary strengthening effect. At the same time, the addition of Cr is beneficial to inhibit the diffusion of Al and improve the steel-aluminum bonding performance. In addition, Cr is also an effective nitriding element, which can simultaneously increase the surface hardness and the depth of the nitriding layer. Conventional nitriding steels usually add up to 3% Cr. Higher Cr is not good for toughness and increases welding difficulty. Cr is a precious alloy element, so its content is controlled to 0.03-0.6%.

[0029] Cu has the effects of solid solution and precipitation strengthening. When the content is high, tempering at an appropriate temperature has a secondary hardening effect, thereby improving the strength, which is beneficial to the strength retention during high-temperature nitriding treatment. At the same time, the addition of Cu is also beneficial to improving the steel-aluminum bonding performance. Too high Cu causes cracks in the steel billet during heating and hot rolling, deteriorating the surface properties, so its content is controlled to 0.01-0.15%.

[0030] N can form AlN particles with Al in steel, thereby binding Al and limiting the diffusion of Al in steel. At the same time, N, like C, is prone to form Koch gas clusters at dislocations, resulting in strain concentration, which causes uneven strain in the aluminum-clad material during processing, affecting the surface quality. Excessive N also deteriorates impact toughness, so its content is controlled to 0.003-0.010%.

[0031] Oxygen (O) can inhibit the adverse effect of Al in steel on aluminum coating performance, so it is required to add a certain amount of O. However, too much oxygen will produce subcutaneous bubbles, looseness and other defects, and aggravate the thermal brittleness of sulfur. During the solidification process of steel, oxygen will precipitate in large quantities in the form of oxides, reducing the plasticity and impact toughness of steel. Therefore, its content is limited to 0.011-0.05%.

[0032] Adding Ca to steel can change the shape of sulfides, inhibit the hot brittleness of S, and improve toughness. Moreover, when there is excessive Ti in steel, it can form titanium sulfide or titanium carbide sulfide with sulfides. The effect is not obvious when the Ca content is too low. When the content exceeds 0.005%, the size of Ca(O,S) formed is too large, and the brittleness is also increased, which can become the starting point of fracture cracks, while reducing the purity of steel and worsening the toughness of the welding heat affected zone. Therefore, its content is limited to 0.001-0.004%.

[0033] In addition to the above elements, the present invention also requires the addition of one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, V: 0.01-0.03%, so as to further improve the room temperature strength and the strength after heat treatment.

[0034] Nb is a strong nitrogen carbide forming element. During the cooling process after rolling, it can combine with carbon and nitrogen in steel to form intermediate phases such as NbC, Nb(CN) and NbN. The fine carbide particles formed can refine the structure, produce fine grain strengthening and precipitation strengthening, and significantly improve the strength of the steel plate. When the Nb content is high, coarse carbonitride particles are formed at the grain boundary, which deteriorates the impact toughness. It can be added optionally, and its content needs to be controlled to 0.01-0.03%.

[0035] V is a strong carbonitride-forming element and can precipitate during the phase change process. The precipitation temperature of the carbonitride V4C3 formed by V is lower than that of Ti carbonitride, which has the effect of hindering dislocation movement, inhibiting grain boundary movement and grain growth. V works together with C, N and other micro-alloying elements of steel, and has a good precipitation strengthening effect during medium and low temperature heat treatment. In particular, the precipitation temperature of V (C, N) generally does not exceed 700℃, and the lower the temperature, the finer the precipitation, and the better the strengthening effect. The nitriding treatment temperature is generally 550-580℃. At this temperature, a large amount of V carbonitrides are precipitated, thereby ensuring that the aluminum-clad strip still has good strength after nitriding treatment. N preferentially forms BN and AlN with B and Al in steel. The addition of V forms VN with the remaining N in the steel, and at the same time utilizes the precipitation strengthening of V C and N compounds, thereby ensuring that it still has high strength during nitriding treatment. At the same time, the addition of V can significantly improve the hardness of the nitrided layer, deepen the depth of the nitrided layer, and has a good combination of strength and toughness, and good impact resistance. When the V content is high, coarse carbonitride particles are formed, which significantly deteriorates the impact toughness of the heat affected zone of the weld. Therefore, the content is limited to 0.01-0.03%.

[0036] Ti has high chemical activity and is easy to form compounds with C, N, O, S, etc. and precipitate during rolling and cooling to increase strength; at the same time, fine precipitates can pin the grain boundaries, thereby refining the austenite grains and preventing the grain growth in the welding heat affected zone, improving the welding performance of the steel plate. Ti has a strong affinity with N, which can increase the surface hardness and the depth of the permeation layer, increase the nitriding temperature, and play a great role in shortening the nitriding time. It is an important element added to fast nitriding steel. When the Ti content is too high, the titanium nitride particles tend to grow and agglomerate at high temperatures, which damages the plasticity and toughness of the steel. Therefore, it needs to be controlled at 0.01-0.06%.

[0037] The steel plate of the present invention requires high strength, is suitable for nitriding and has good steel-aluminum bonding performance to meet the use requirements of more application fields, and requires the steel plate to have a yield strength of ≥280MPa and a tensile strength of ≥340MPa. In order to meet the above performance requirements, the present invention strictly designs the composition according to the influence of different alloy elements on the above performance, and achieves the performance requirements through the comprehensive effect of multiple elements. The addition of C has solid solution strengthening and phase transformation strengthening effects. The existing aluminum-clad steel (such as Chinese patent CN114250411A) generally controls C≤0.005% to ensure plasticity, which greatly increases the difficulty of steelmaking. In order to ensure high strength after nitriding treatment, the present invention requires the yield strength of the substrate to be above 280MPa, so 0.01-0.07% C is used. On the one hand, it plays a role of solid solution strengthening, and at the same time, in the process of strip production, a ferrite + a small amount of bainite structure is formed in the matrix by controlling rolling and controlling post-rolling cooling, which plays a phase transformation strengthening role and improves strength.

[0038] Since the aluminum-clad substrate undergoes annealing heat treatment during the production process, and the steel of the present invention also undergoes subsequent nitriding heat treatment, conventional fine grain strengthening means have little effect after heat treatment, while solid solution strengthening is not limited by heat treatment. Therefore, the higher the strength of the substrate, the higher the strength of the finished aluminum-clad material. For this reason, the present invention adds 0.4-1.2% Mn, and the strength of the substrate is ensured by solid solution strengthening of Mn, and this strengthening effect still exists even after heat treatment.

[0039] In the present invention, the P content is controlled at 0.008-0.020%. P is usually controlled as an impurity element in steel, so it is hoped that its content is as low as possible, and is generally required to be controlled below 0.015% or even lower. However, the lower the P content, the higher the steelmaking cost and the greater the difficulty. Since P is an element of the same family as N, appropriate P is beneficial to the steel-aluminum bonding performance, but the research of the present invention has found that its improvement effect on the steel-aluminum bonding performance is not linear. When the P content exceeds 0.020%, the steel-aluminum bonding performance begins to deteriorate. Therefore, considering the difficulty, cost and performance requirements of steelmaking, the upper limit of P control is relaxed to 0.020%, which ensures the steel-aluminum bonding performance on the one hand, while improving the strength and reducing the steelmaking cost.

[0040] The steel of the present invention is required to have nitriding properties, and it is hoped that the steel is easy to form a nitriding layer during the nitriding process. In addition to solid solution strengthening, Cr in steel also has a secondary strengthening effect. However, in the present invention, the addition of 0.03-0.6% Cr can improve the nitriding performance of steel in addition to improving strength. Current nitriding steels such as 35MoCrAl and 42CrMo generally have a Cr content of more than 3%. Cr is a precious alloying element, and such a high content obviously increases the cost. The research of the present invention shows that Cr can promote the diffusion of N in the matrix and quickly form a nitriding layer, so that the substrate has good nitriding properties. The steel of the present invention also adds an appropriate amount of N to improve the steel-aluminum bonding performance. The N in the steel cooperates with Cr to further promote the formation of the nitriding layer and strengthen the matrix, thereby improving the strength of the steel plate. Since the aluminum-clad substrate only requires the nitriding layer hardness of about 500Hv, and the thickness of the nitriding layer does not exceed 100μm, the required nitriding layer thickness and hardness requirements are obtained by adding 0.03-0.6% Cr to the aluminum-clad substrate. Higher Cr has redundant effects and increases costs.

[0041] Although Cu also has a solid solution strengthening effect in steel and can precipitate and strengthen to improve strength during heat treatment. However, the present invention mainly uses the addition of Cu to further improve the steel-aluminum bonding performance. Because the steel type of the present invention undergoes annealing heat treatment and nitriding treatment during production and use, the high temperature during the heat treatment process easily promotes the formation of brittle iron-aluminum compounds, which deteriorates the steel-aluminum bonding performance. Therefore, the steel type of the present invention has higher requirements for steel-aluminum bonding performance than the existing aluminum-clad substrate, and adding an appropriate amount of Cu is conducive to improving the steel-aluminum bonding performance and improving the strength after nitriding treatment.

[0042] According to the strengthening effect of the above elements on the matrix, it is required to control the contents of C, P, N, Mn and Cr in the steel to satisfy the relationship 1: 150(C-0.01)+60P+300N+5Mn+3Cr≥7.0. If the value of the relationship is lower than 7.0, the problem of low strength is likely to occur.

[0043] The formation of iron-aluminum compounds is very sensitive to temperature. The high temperature during nitriding treatment provides a driving force for the formation of iron-aluminum compounds, which is more likely to induce the formation of iron-aluminum compounds, resulting in iron-aluminum stratification. Therefore, the steel plate of the present invention has higher requirements for steel-aluminum bonding performance than the existing aluminum-clad substrates. The key to the steel-aluminum bonding performance lies in controlling the formation of brittle iron-aluminum compounds at the steel-aluminum interface in the aluminum-clad material. The research of the present invention shows that the formation of iron-aluminum compounds is closely related to the diffusion of Al in steel. Controlling the diffusion of Al can unify the formation of iron-aluminum compounds within a certain temperature range. Therefore, the addition of C, Cr and Cu has a certain improvement effect on the steel-aluminum bonding performance, while O (oxygen) and N can inhibit the diffusion of Al, reduce the formation of brittle iron-aluminum compounds, and thus improve the steel-aluminum bonding performance. Si and Al, as deoxidizing elements, hinder the improvement of O on the steel-aluminum bonding performance, so their content should be limited.

[0044] The present invention obtains good steel-aluminum bonding performance through the synergistic effect of multiple elements such as C, Cr, Cu, O, N, etc. According to the strength of the effect of C, N, O, Cu, Cr, Al, and Si on the steel-aluminum bonding performance, their contents are required to satisfy the relationship 2: 0.5C+6.86N+O+0.05Cu+0.047Cr-0.89Al-1.15Si≥0.085, so as to ensure that the steel plate has excellent steel-aluminum bonding performance. If the value of the relationship is lower than 0.085, the aluminum-clad plate strip prepared from the steel plate is prone to steel-aluminum delamination during the subsequent nitriding treatment.

[0045] In general, the above-mentioned component system is adopted, the steel-aluminum bonding performance, strength and nitriding characteristics are comprehensively considered, and through the joint action of various elements, an invented steel grade that meets the performance requirements can be obtained.

[0046] The method for producing high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance of the present invention comprises the following steps:

[0047] 1) Smelting

[0048] According to the above composition, the molten iron is pretreated, blown in a converter, refined outside the furnace, and cast into a slab;

[0049] 2) Reheating and controlled rolling

[0050] The thickness of the steel strip after rolling is greater than 2.5mm, the heating temperature is ≥1230℃, the rough rolling end temperature is above 1050℃; the finishing rolling start temperature is above 980℃, and the finishing rolling end temperature is 870~910℃;

[0051] The thickness of the steel strip after rolling is ≤2.5mm, the heating temperature is ≥1100℃, the rough rolling end temperature is above 900℃, the cumulative deformation in the rough rolling stage is ≥80%; the finishing rolling start temperature is 810~870℃, and the finishing rolling end temperature is 710~770℃;

[0052] 3) Control cooling, cooling rate above 20℃ / s;

[0053] 4) Coiling: coiling temperature 550~610℃.

[0054] Preferably, in step 1), the obtained slab is machine cleaned.

[0055] Preferably, in step 2) controlled rolling, the side pressure in the rough rolling stage is controlled within 50 mm.

[0056] In the production process of the present invention:

[0057] Pretreatment of molten iron to remove P and S to ensure low P and S content in steel; top and bottom composite blowing in converter to control C content.

[0058] The function of machine cleaning after continuous casting is to eliminate surface defects of the ingot, reduce slag inclusions, warping, pits, scars and other defects on the strip surface, improve the surface quality of the strip, and reduce surface defects of the finished aluminum-clad materials.

[0059] The present invention formulates a rolling process according to the phase change temperature curve of the steel grade and combines the target performance to determine the temperature control parameters of the steel rolling process. The present invention relates to a steel grade with a low alloy content and a continuous cooling curve such as Figure 1 As shown in the figure, it can be seen that the starting temperature of the ferrite phase transformation of the steel is 870℃, pearlite begins to form after the temperature drops to 714℃, and the starting temperature of the bainite phase transformation is 663℃. When the cooling rate is above 5℃ / s, only ferrite and bainite are formed.

[0060] According to different thickness specifications, the present invention designs two rolling processes for the steel. For steel strips with a thickness greater than 2.5 mm, a conventional austenite rolling process is used; and for steel strips with a thickness less than 2.5 mm, a ferrite rolling process is selected to obtain a good plate shape and higher strength.

[0061] According to the composition calculation of the steel grade of the present invention, the Ar3 temperature of the steel grade is 871°C, so during the austenite rolling process, it is required to control the finishing temperature of the finishing rolling to be above 870°C. If the finishing temperature of the finishing rolling is too high, a higher heating temperature is required, which increases energy consumption and oxidation of the steel strip, so the upper limit of the finishing temperature is set to not exceed 910°C. Correspondingly, the finishing inlet temperature is required to be 980°C, and the rough rolling end temperature is required to be above 1050°C. In order to ensure the rough rolling end temperature, and considering the dissolution behavior of micro-alloying element carbonitrides in austenite and the growth behavior of austenite grains during heating, it is required to control the heating temperature to be above 1230°C.

[0062] When the thickness of the steel strip is below 2.5 mm, the deformation resistance of the steel strip is low at a high temperature of 870-910°C, and it is easy to break the strip, local stretching and lateral bending at the outlet of the finishing mill. For this reason, the present invention adopts a ferrite rolling process for production. On the one hand, the strength of the steel strip is higher at a lower temperature, and the steel strip is not easy to deform under the same coiling tension, thereby reducing the occurrence of narrowing and rolling breakage. At the same time, higher strength also allows higher coiling tension, thereby improving the plate shape and reducing the occurrence of lateral bending. Ferrite rolling requires that the entire finishing deformation is carried out in the ferrite zone, so the starting temperature of the finishing rolling is controlled not to be higher than 870°C, and the ending temperature is controlled not to be lower than 710°C. If the starting temperature of the finishing rolling is too low, the thermal deformation resistance is high, the rolling load of the final stand is increased, and the energy consumption is increased; if it is too high, it is easy to enter the austenite and ferrite two-phase region, and mixed crystals are easily formed in the matrix, causing rolling force fluctuations, which is not conducive to the thickness control and plate shape of the steel strip. Therefore, the start temperature of finishing rolling is set at 810-870℃ and the end temperature of finishing rolling is set at 710-770℃ during the ferrite rolling process. According to the start temperature of finishing rolling, considering the temperature drop of the intermediate billet on the roller, the end temperature of rough rolling is required to be above 900℃, and the corresponding billet heating temperature is controlled above 1100℃. In addition, in order to ensure the effect of recrystallization and grain refinement, the cumulative deformation in the rough rolling stage is required to be ≥80%.

[0063] The solid solubility of copper in steel is limited and decreases rapidly with decreasing temperature. At high temperature, C dissolved in austenite precipitates in the form of fine ε-Cu and is dispersed in the matrix. Its twin structure and pinning effect on dislocations increase the strength of steel. Studies have shown that Cu precipitates are formed at 650°C, and the lower the temperature, the smaller the size of the precipitates; the best precipitation strengthening effect is achieved at 500°C, so the lower limit of the coiling temperature cannot be lower than 500°C. Figure 2 According to the TTT curve, 580℃ is the temperature at which bainite transforms fastest. The steel matrix of the present invention is mainly equiaxed ferrite. In order to obtain higher strength, it is hoped that there is a certain amount of bainite structure in the matrix, so the coiling temperature is controlled at about 580℃. The selected added Nb, V and Ti carbonitrides also have a good precipitation strengthening effect near this temperature, so considering the precipitation strengthening and phase transformation strengthening effects, the coiling temperature is set at 550~610℃, and the cooling rate after rolling is controlled to be ≥5℃ / s.

[0064] In order to obtain the target performance, the steel matrix structure is controlled to be a uniform equiaxed ferrite structure, and a small amount of bainite structure is allowed to form. Figure 1 It can be seen that the ferrite + a small amount of bainite structure can be obtained when the cooling rate is above 5°C / s; considering that rapid cooling can refine the structure and increase the phase transformation rate, the post-rolling cooling rate of the steel type involved in the present invention is controlled to be above 20°C / s.

[0065] In order to obtain good strip surface quality, the side pressure in the rough rolling stage is controlled within 50mm. At the same time, it is required that there should be no defects such as pores and scars at the corners of the billet, or the surface should be cleaned.

[0066] In order to suppress the abnormal growth of ferrite grains in the strip after final rolling and ensure that the strip structure is a uniform equiaxed ferrite + bainite structure, the post-rolling cooling is required to adopt a front cooling method. That is, the strip is immediately intensively cooled after leaving the hot rolling unit. The process of the present invention can obtain a uniform ferrite + a small amount of bainite structure, and the specific requirement is that the bainite content is ≤20%. Too high a bainite content will lead to insufficient plasticity and increase the difficulty of aluminum cladding rolling.

[0067] The present invention has the following advantages:

[0068] 1. According to the characteristics that the solid solution strengthening and phase transformation strengthening effects are not affected by the subsequent annealing and nitriding heat treatment of the steel plate, the present invention adopts a simple C-Mn design in the composition design, and controls the contents of C, P, N, Mn, and Cr to satisfy the relationship: 150(C-0.01)+60P+300N+5Mn+3Cr≥7.0, thereby obtaining higher strength. The yield strength of the steel plate is ≥280MPa, and the tensile strength is ≥340MPa. At the same time, the selective addition of Cu, Nb, V, and Ti ensures the high strength after nitriding heat treatment to meet the use requirements of more application fields.

[0069] 2. The steel of the present invention must meet the requirements of subsequent nitriding treatment, so the steel-aluminum bonding performance is required to be higher. In the composition design, according to the effects of C, N, O, Cu, Cr and Al, Si on the steel-aluminum bonding performance, the content is required to meet the relationship: 0.5C+6.86N+O+0.05Cu+0.047Cr-0.89Al-1.15Si≥0.085, which inhibits the formation of brittle iron-aluminum compounds at the steel-aluminum interface, thereby ensuring that the steel plate obtains good steel-aluminum bonding performance. The interface of the finished aluminum-clad material is clean during the subsequent high-temperature nitriding treatment and processing and use, and no iron-aluminum compounds are formed.

[0070] 3. In the present invention, according to the influence of Cr on nitriding and the requirements of the nitriding layer of the aluminum-clad substrate, a small amount of Cr (0.03-0.6%) is added to promote the diffusion of N in the matrix and quickly form a nitriding layer, so that the substrate has good nitriding properties and the strength of the steel plate is improved. The performance of the steel plate meets the requirements of subsequent processing and use. Compared with the existing nitriding steel, the use of precious alloy elements is saved, the cost is reduced, and good nitriding properties are obtained.

[0071] 4. The present invention controls the P content to 0.008-0.020%, utilizes the solid solution strengthening effect of P and its influence on the steel-aluminum bonding performance, further improves the steel-aluminum bonding performance, and at the same time reduces the difficulty and cost of steelmaking, and has higher production efficiency.

[0072] 5. In terms of process control, the present invention adopts austenite rolling and ferrite rolling processes respectively for different ingot thicknesses obtained after rolling, so that the steel plate can obtain high strength while significantly improving the shape of thin-gauge steel strips, reducing the occurrence of problems such as strip narrowing, strip breaking and side bending during rolling. The production process is simple, the cost is low, and it is suitable for large-scale production of enterprises.

[0073] 6. The process of the present invention adopts different controlled rolling processes, combined with a coiling temperature of 550-610°C and a cooling rate after rolling ≥20°C / s, so that the obtained steel plate structure is uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%. The obtained steel plate has good deformation ability and can meet the deformation requirements of more than 80% of aluminum cladding rolling, as well as the stamping and drawing deformation in the subsequent processing process. No annealing is required in the middle, which reduces the production process and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 It is a schematic diagram of the static CCT curve (calculation) of the steel grade of the present invention.

[0075] Figure 2 It is a schematic diagram of the static TTT curve (calculation) of the steel grade of the present invention.

[0076] Figure 3 This is a typical matrix structure photo of the steel in Example 1 of the present invention. DETAILED DESCRIPTION

[0077] The present invention will be further described below in conjunction with the accompanying drawings.

[0078] The embodiment of the present invention adopts steelmaking in a 500kg vacuum induction furnace. The chemical composition of the embodiment steel is shown in Table 1, the specific process parameters are shown in Table 2, and the mechanical properties of the embodiment steel are shown in Table 3.

[0079] Depend on Figure 3 It can be seen that the microstructure of the steel plate obtained by using the composition and process of the present invention is a uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.

[0080] The composition, production process and performance of similar steel grades were compared.

[0081] Comparative steel 1 is Chinese patent CN101514426A "Low yield point steel for earthquake resistance of buildings with yield strength of 100 MPa and its production method", which has high Si and Al contents and does not contain O.

[0082] Comparative steel 2 is Chinese patent CN101525720 "A new type of special substrate for preparing aluminum-clad steel strip", and the alloy composition is too high.

[0083] Comparative steel 3 is Chinese patent CN111349869A "A high-strength steel for aluminum-clad substrate and its production method", with 0.018-0.03% P added to the composition. An iron-aluminum compound layer with a thickness of no more than 5μm appeared at the steel-aluminum interface, the steel-aluminum bonding performance was reduced, and the strength was low.

[0084] Comparative steel 4 is Chinese patent CN107881426A “A high-strength aluminum-clad strip and its manufacturing method”, which does not consider the nitriding characteristics and the strength reduction problem during nitriding.

[0085] The steel of the present invention has obvious differences in composition from the four comparative steels. In order to ensure good steel-aluminum bonding performance and high-temperature strength after nitriding treatment, the steel of the present invention has a specially designed composition system.

[0086] Among the above four comparative steels, comparative steels 1 and 2 contain relatively high Al and extremely high P, S, N, etc., without considering the steel-aluminum bonding performance; comparative steel 3 explicitly adds P, which is unfavorable to the steel-aluminum bonding performance and has low strength; comparative steel 4 involves an aluminum-clad plate and strip, but does not consider the strength reduction problem during nitriding, so like comparative steel 3, high-temperature strength is not considered in the composition. Therefore, the comparative steels are significantly different from the steels of the present invention in composition.

[0087] As can be seen from Table 3, the steel of the present invention has a stable yield strength. Under different rolling processes, the yield and tensile strengths of various specifications of steel plates are above 280MPa and 340MPa, and have a very high elongation. It is superior to the comparative steel in terms of composition design and function, so that the aluminum-clad plate strip produced by the steel of the present invention has good stamping and deep drawing performance, and is suitable for processing components with high-temperature heat treatment requirements such as nitriding process requirements and high-strength requirements.

[0088] From the performance point of view, the comparative steels 1 and 2 are only required to have lower yield strength and higher elongation, while the steel of the present invention, in addition to the above requirements, also explicitly requires the steel to have good aluminum coating performance, suitable for the production of aluminum-coated strip steel, without the need for annealing in the middle, which is also not available in comparative steel 2. Although comparative steels 3 and 4 also require aluminum coating performance, they are mainly used for the production of aluminum-coated strips such as radiators and home appliance panels, and the thickness of the aluminum layer on the surface does not exceed 0.1mm; while the steel involved in the present invention has a wider application field, and comparative steels 3 and 4 do not meet the requirements of nitriding treatment. Therefore, there are significant differences in performance between the steel of the present invention and the comparative steel.

[0089] In summary, the steel of the present invention adopts C-Mn design, supplemented by appropriate C, N, V, O and Cu, Cr and other components, and designs an aluminum-clad substrate with yield and tensile strength of 280MPa and 340MPa or more, respectively, which meets the requirements of aluminum-clad substrates with high elongation, good aluminum-clad performance, strong deformation ability and suitable for nitriding treatment, and can also be used for the production of other aluminum-clad materials with high strength requirements. In addition, the production cycle is short, the process is simple, and the performance also meets or exceeds the requirements of the comparative steel grades.

[0090] In addition, the embodiments are only for illustration, and the thickness of the steel type described in the present invention is not limited thereto, and thinner or thicker strip steel can be produced within the range allowed by the equipment.

[0091]

[0092]

[0093]

Claims

1. A high-strength aluminum-clad steel with excellent nitriding performance, the chemical composition weight percentage of which is: C: 0.01-0.07%, 0 < Si ≤ 0.005%, Mn: 0.4-1.2%, P: 0.008-0.020%, S ≤ 0.008%, 0 < Al ≤ 0.005%, Cr: 0.03-0.60%, N: 0.003-0.010%, O: 0.011-0.05%, Cu: 0.01-0.15%, Ca: 0.001-0.004%, and one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, V: 0.01-0.03% are selectively added, and the balance contains Fe and other unavoidable impurities; and at the same time, 0.5C+6.86N+O+0.05Cu+0.047Cr-0.89Al-1.15Si≥0.085; 150(C-0.01)+60P+300N+5Mn+3Cr≥7.

0.

2. The high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance according to claim 1, characterized in that: The balance is Fe and other inevitable impurities.

3. The high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance according to claim 1 or 2, characterized in that: The microstructure of the steel for the aluminum-clad plate strip substrate is uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.

4. The high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance as claimed in claim 1, 2 or 3, characterized in that: The steel used for the aluminum-clad plate substrate has a yield strength of ≥280MPa, a tensile strength of ≥340MPa, and an elongation of ≥30%.

5. The method for producing high-strength aluminum-clad strip substrate steel with excellent nitriding performance according to any one of claims 1 to 4, characterized in that: The steps include: 1) Smelting The composition according to claim 1 or 2 is subjected to molten iron pretreatment, converter blowing, external refining, and casting into slabs; 2) Reheating and controlled rolling The thickness of the steel strip after rolling is greater than 2.5mm, the heating temperature is ≥1230℃, the rough rolling end temperature is above 1050℃; the finishing rolling start temperature is above 980℃, and the finishing rolling end temperature is 870~910℃; The thickness of the steel strip after rolling is ≤2.5mm, the heating temperature is ≥1100℃, the rough rolling end temperature is above 900℃, the cumulative deformation in the rough rolling stage is ≥80%; the finishing rolling start temperature is 810~870℃, and the finishing rolling end temperature is 710~770℃; 3) Control cooling, the cooling rate is above 20℃ / s; 4) Coiling: coiling temperature 550~610℃.

6. The method for producing high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance as claimed in claim 5, characterized in that: In step 1), the obtained slab is machine cleaned.

7. The method for producing high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance as claimed in claim 5, characterized in that: Step 2) During the controlled rolling, the side pressure in the rough rolling stage is controlled within 50 mm.

8. The method for producing high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance as claimed in claim 5, characterized in that: The microstructure of the steel for the aluminum-clad plate strip substrate is uniform ferrite + a small amount of bainite structure, wherein the bainite content is ≤20%.

9. The method for producing high-strength aluminum-clad plate strip substrate steel with excellent nitriding performance as claimed in claim 5 or 8, characterized in that: The yield strength of the steel used for the aluminum-clad plate strip substrate is ≥280MPa, the tensile strength is ≥340MPa, and the elongation is ≥30%.

Citation Information

Patent Citations

  • Novel special base metal strip for preparing feran

    CN101525720A

  • Steel-aluminum composite board and preparation method thereof

    CN102734625A

  • Steel for aluminum-coated substrate and production method of steel

    CN107881422A

  • Method and device for preparing steel / aluminum laminated composite plate by hot continuous rolling with small rolling reduction

    CN111014294A

  • Corrosion-inhibiting high-strength aluminum-coated substrate steel and manufacturing method thereof

    CN111349848A