High-hardness micro-diameter ball-end milling cutter coating and preparation method thereof

By depositing functional coatings of materials such as aluminum oxide, modified cubic boron nitride, modified silicon carbide and modified graphene on the surface of micro-diameter ball-end milling cutters, the poor machining performance of micro-diameter ball-end milling cutters is solved. solve the problem and achieve high hardness and improved wear resistance.

CN118726901AActive Publication Date: 2024-10-01ZHEJIANGSHENGANG SAIOU TECH CO LTD

Patent Information

Application Number
CN202411061133.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing micro-diameter ball-end milling cutters have poor machining performance and are difficult to meet the needs for high precision, high speed, and high efficiency.

Method used

A layer of functional coating is deposited on the surface of the micro-diameter ball end mill using vapor deposition technology. The coating is composed of aluminum oxide, modified cubic boron nitride, modified silicon carbide, modified graphene and titanium nitride. It is prepared by arc-enhanced glow discharge technology and magnetron sputtering technology to form a high-hardness coating with a thickness of 1-2μm.

Benefits of technology

Significantly improves the hardness and wear resistance of the coating, enhances the mechanical properties of the tool, and improves the machining performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726901A_ABST
    Figure CN118726901A_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of cutter coatings, and provides a high-hardness micro-diameter ball-end milling cutter coating and a preparation method thereof.The high-hardness micro-diameter ball-end milling cutter coating comprises at least one functional layer deposited on a micro-diameter ball-end milling cutter, the functional layer comprises the following raw materials: aluminum oxide, modified cubic boron nitride, modified silicon carbide, modified graphene and titanium nitride, and the aluminum oxide, the modified cubic boron nitride, the modified silicon carbide, the modified graphene and the titanium nitride are added into the raw materials of the functional layer; by adding the modified cubic boron nitride to be fully combined with other components, the hardness and other mechanical properties of the coating are improved, by adding the modified silicon carbide to improve the hardness and deposition efficiency, the formed coating is compact, high in hardness and good in wear resistance, and by adding the modified graphene, the coating is further high in hardness and good in wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tool coatings, and in particular relates to a high-hardness, small-diameter ball-end milling cutter coating and a preparation method thereof. Background Art

[0002] A ball end mill is a tool with a ball-like blade that is mounted on a milling machine and is used to mill various curved surfaces and arc grooves. A ball end mill is also called an R cutter.

[0003] Mechanical processing is constantly moving towards high precision, high speed and high efficiency. Precision machining tools such as small-diameter milling cutters and micro-diameter milling cutters have emerged. They are usually made of ultra-fine grain WC-Co cemented carbide and have poor rigidity.

[0004] In order to improve the machining performance of the micro-diameter tool, one or more layers of coatings with excellent comprehensive performance can be deposited on the surface of the micro-diameter tool through vapor deposition technology, so that it has high hardness and can protect the micro-diameter tool. Summary of the invention

[0005] The present invention provides a high-hardness and micro-diameter ball-end milling cutter coating, aiming to solve the above-mentioned problems.

[0006] The present invention is implemented as follows: a high-hardness micro-diameter ball end mill coating comprises at least one functional layer deposited on the micro-diameter ball end mill, the thickness of the functional layer is 1-2 μm, and the functional layer comprises the following raw materials in parts by weight: 2-4 parts of aluminum oxide, 2-3 parts of modified cubic boron nitride, 1-3 parts of modified silicon carbide, 1-2 parts of modified graphene, and 1-3 parts of titanium nitride.

[0007] Preferably, the functional layer comprises the following raw materials in parts by weight: 2.5-3.5 parts of aluminum oxide, 2.2-2.8 parts of modified cubic boron nitride, 1.5-2.5 parts of modified silicon carbide, 1.3-1.7 parts of modified graphene, and 1.5-2.5 parts of titanium nitride.

[0008] Preferably, the functional layer comprises the following raw materials in parts by weight: 3 parts of aluminum oxide, 2.5 parts of modified cubic boron nitride, 3 parts of modified silicon carbide, 1.5 parts of modified graphene, and 2 parts of titanium nitride.

[0009] Preferably, the preparation method of the modified cubic boron nitride is as follows: placing cubic boron nitride powder in nitric acid with a mass fraction of 10-30% by weight and 5-7 times the weight, heating to 80-90°C, stirring for 2-3h, centrifuging, washing and drying for use to obtain product A; dispersing product A in water with a mass fraction of 6-8 times the weight, and passing N 2 O or N 2The product B is obtained by filtration: the product B is dispersed in a siloxane solution with a weight of 4-7 times and a volume fraction of 1-3%, heated to 80-100°C, reacted for 3-5h, filtered, and vacuum dried to obtain modified cubic boron nitride. The modification improves the dispersibility, chemical activity and strength of the cubic boron nitride, and is fully combined with other components to improve the mechanical properties such as the hardness of the coating.

[0010] Preferably, the preparation method of the modified silicon carbide is as follows: by weight, 6-10 parts of nano-silicon carbide are added to 30-40 parts of a hydrochloric acid solution with a mass fraction of 30-40%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 20-30 parts of a sodium chromate solution with a concentration of 100-200 g / L, and then 10-20 parts of glucose with a concentration of 40-50 g / L, 4-6 parts of polyethylene glycol with a concentration of 5-10 g / L, and 5-10 parts of sodium hexametaphosphate with a concentration of 20-40 g / L are added; high pressure is continuously stirred and pumped into the solution; The method comprises the following steps: heating the autoclave to 150-160°C and reacting the nano-silicon carbide for 30-50 minutes; cooling the autoclave to below 90°C after the reaction, extracting the suspension, filtering, washing and drying the suspension, and sintering the dried powder at 800-1000°C for 3-4 hours to obtain modified silicon carbide; adding the nano-silicon carbide to a hydrochloric acid solution for pickling, using the hydrochloric acid solution to remove impurities on the surface of the nano-silicon carbide, thereby improving its purity, increasing the hydroxyl content on the surface of the nano-silicon carbide powder, and improving its activity; reducing the sodium chromate to form a chromium hydroxide layer wrapped on the surface of the silicon carbide, thereby improving the hardness and deposition efficiency, and forming a dense coating with high hardness and good wear resistance.

[0011] Preferably, the preparation method of the modified graphene is as follows: 4-6 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 0.5-1.5 parts of nano-Cr powder are added and ball milled for 30-50 minutes. The liquid after ball milling is stirred at a temperature of 120-160°C for 1-2 hours, and then freeze-dried at a temperature of -40 to -20°C for 3-5 hours to obtain modified graphene. The modified graphene has high hardness, good wear resistance, and excellent mechanical properties. The addition of nano-Cr powder forms a coating with strong interfacial bonding force, which can effectively adhere to the surface of the tool substrate.

[0012] The present invention also provides a method for preparing the high-hardness micro-diameter ball-end milling cutter coating, comprising the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate is pre-treated and placed in a vacuum chamber; Evacuate the vacuum chamber and preheat it to 350-450°C; The existing arc-enhanced glow discharge technology is used to ion clean and etch the tool substrate for 10-20 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, using existing magnetron sputtering technology to coat the tool substrate to form a functional layer; After coating, cool for 90-120 minutes.

[0013] Preferably, the N 2 The flow rate is 40-60sccm, the Ar flow rate is 80-120sccm, and the coating time is 60-80min.

[0014] Preferably, the pretreatment of the tool substrate comprises immersing the tool substrate in acetone for ultrasonic cleaning for 3-5 minutes, then immersing the tool substrate in ethanol for ultrasonic cleaning for 4-6 minutes and then blowing it dry.

[0015] Preferably, the pretreatment of the tool substrate also includes, after drying, immersing the to-be-coated portion of the tool substrate under the liquid surface of a mixed liquid in a container, wherein the mixed liquid includes nano-titanium powder and Acetobacter xylinum fermentation liquid in a mass ratio of 1:20-30, culturing at 30-35°C for 36-48 hours, taking out the tool substrate, washing it with distilled water 2-3 times and then drying it; during the fermentation process, bacterial cellulose grows, and the bacterial cellulose adsorbs the nano-titanium powder and adheres to the surface of the to-be-coated portion of the tool substrate, and is able to adsorb coating materials, thereby improving the adhesion tightness of the coating on the one hand, and improving the hardness of the coating on the other hand.

[0016] Compared with the prior art, the embodiments of the present application have the following beneficial effects: The high-hardness, small-diameter ball-end milling cutter coating provided by the present invention can improve the hardness and other properties of the coating by adding aluminum oxide, modified cubic boron nitride, modified silicon carbide, modified graphene, and titanium nitride to the functional layer raw materials. By adding modified cubic boron nitride and fully combining with other components, the mechanical properties such as the hardness of the coating are improved. By adding modified silicon carbide, the hardness and deposition efficiency are improved. The formed coating is dense, has high hardness, and good wear resistance. By adding modified graphene, the coating is further made to have high hardness and good wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a flow chart of a method for preparing a high-hardness, small-diameter ball-end milling cutter coating provided in Examples 1-5 of the present invention.

[0018] Figure 2 This is a flow chart of a method for preparing a high-hardness, small-diameter ball-end milling cutter coating provided in Example 6 of the present invention. DETAILED DESCRIPTION

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0020] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. Example 1

[0021] The embodiment of the present invention provides a high-hardness micro-diameter ball end milling cutter coating, such as Figure 1 As shown, it includes at least one functional layer deposited on the micro-diameter ball end milling cutter, the thickness of the functional layer is 1 μm, and the functional layer includes the following raw materials in parts by weight: 2 parts of aluminum oxide, 2 parts of modified cubic boron nitride, 1 part of modified silicon carbide, 1 part of modified graphene, and 1 part of titanium nitride. The method for preparing the high-hardness micro-diameter ball end milling cutter coating includes the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate was immersed in acetone for ultrasonic cleaning for 3 minutes, then immersed in ethanol for ultrasonic cleaning for 4 minutes, blown dry, and placed in a vacuum chamber; Evacuate the vacuum chamber and preheat it to 350°C; The existing arc-enhanced glow discharge technology was used to ion clean and etch the tool substrate for 10 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, the N 2 The flow rate is 40sccm, the Ar flow rate is 80sccm, and the existing magnetron sputtering technology is used to coat the tool substrate to form a functional layer. The coating time is 60min; After coating, cool for 90 minutes.

[0022] The preparation method of the modified cubic boron nitride is as follows: putting the cubic boron nitride powder into nitric acid with a mass fraction of 10% by weight, heating to 80°C, stirring for 2 hours, centrifuging, washing and drying for use to obtain product A; dispersing product A in water with a mass fraction of 6 times the weight of water, and passing N 2 O or N 2 The product B was obtained by filtration: the product B was dispersed in a siloxane solution with a weight of 4 times and a volume fraction of 1%, heated to 80°C, reacted for 3h, filtered, and vacuum dried to obtain modified cubic boron nitride.

[0023] In this embodiment, the preparation method of the modified silicon carbide is as follows: by weight, 6 parts of nano-silicon carbide are added to 30 parts of a hydrochloric acid solution with a mass fraction of 30%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 20 parts of a sodium chromate solution with a concentration of 100 g / L, and then 10 parts of glucose with a concentration of 40 g / L, 4 parts of polyethylene glycol with a concentration of 5 g / L, and 5 parts of sodium hexametaphosphate with a concentration of 20 g / L are added; the mixture is pumped into an autoclave under continuous stirring, heated to 150°C for reaction for 30 minutes; after the reaction is completed, the mixture is cooled to below 90°C, the suspension is extracted, filtered, washed, and dried, and the dried powder is sintered at 800°C for 3 hours to obtain modified silicon carbide.

[0024] In a specific implementation, the preparation method of the modified graphene is as follows: 4 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 0.5 parts of nano-Cr powder are added and ball-milled for 30 minutes. The ball-milled liquid is stirred at a temperature of 120°C for 1 hour, and then freeze-dried at a temperature of -40°C for 3 hours to obtain modified graphene. Example 2

[0025] The embodiment of the present invention provides a high-hardness micro-diameter ball end milling cutter coating, such as Figure 1 As shown, at least one functional layer is deposited on the micro-diameter ball end milling cutter, the thickness of the functional layer is 1 μm, and the functional layer includes the following raw materials in parts by weight: 2.5 parts of aluminum oxide, 2.2 parts of modified cubic boron nitride, 1.5 parts of modified silicon carbide, 1.3 parts of modified graphene, and 1.5 parts of titanium nitride. The method for preparing the high-hardness micro-diameter ball end milling cutter coating includes the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate was immersed in acetone for ultrasonic cleaning for 3 minutes, then immersed in ethanol for ultrasonic cleaning for 4 minutes, blown dry, and placed in a vacuum chamber; Evacuate the vacuum chamber and preheat it to 350°C; The existing arc-enhanced glow discharge technology was used to ion clean and etch the tool substrate for 10 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, the N 2 The flow rate is 40sccm, the Ar flow rate is 80sccm, and the existing magnetron sputtering technology is used to coat the tool substrate to form a functional layer. The coating time is 60min; After coating, cool for 90 minutes.

[0026] The preparation method of the modified cubic boron nitride is as follows: putting the cubic boron nitride powder into nitric acid with a mass fraction of 10% by weight, heating to 80°C, stirring for 2 hours, centrifuging, washing and drying for use to obtain product A; dispersing product A in water with a mass fraction of 6 times the weight of water, and passing N 2 O or N 2 The product B was obtained by filtration: the product B was dispersed in a siloxane solution with a weight of 4 times and a volume fraction of 1%, heated to 80°C, reacted for 3h, filtered, and vacuum dried to obtain modified cubic boron nitride.

[0027] In this embodiment, the preparation method of the modified silicon carbide is as follows: by weight, 6 parts of nano-silicon carbide are added to 30 parts of a hydrochloric acid solution with a mass fraction of 30%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 20 parts of a sodium chromate solution with a concentration of 100 g / L, and then 10 parts of glucose with a concentration of 40 g / L, 4 parts of polyethylene glycol with a concentration of 5 g / L, and 5 parts of sodium hexametaphosphate with a concentration of 20 g / L are added; the mixture is pumped into an autoclave under continuous stirring, heated to 150°C for reaction for 30 minutes; after the reaction is completed, the mixture is cooled to below 90°C, the suspension is extracted, filtered, washed, and dried, and the dried powder is sintered at 800°C for 3 hours to obtain modified silicon carbide.

[0028] In a specific implementation, the preparation method of the modified graphene is as follows: 4 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 0.5 parts of nano-Cr powder are added and ball-milled for 30 minutes. The ball-milled liquid is stirred at a temperature of 120°C for 1 hour, and then freeze-dried at a temperature of -40°C for 3 hours to obtain modified graphene. Example 3

[0029] The embodiment of the present invention provides a high-hardness micro-diameter ball end milling cutter coating, such as Figure 1As shown, it includes at least one functional layer deposited on the micro-diameter ball end milling cutter, the thickness of the functional layer is 1.5 μm, and the functional layer includes the following raw materials in parts by weight: 3 parts of aluminum oxide, 2.5 parts of modified cubic boron nitride, 3 parts of modified silicon carbide, 1.5 parts of modified graphene, and 2 parts of titanium nitride. The high-hardness micro-diameter ball end milling cutter coating preparation method includes the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate was immersed in acetone for ultrasonic cleaning for 4 minutes, then immersed in ethanol for ultrasonic cleaning for 5 minutes, blown dry, and placed in a vacuum chamber; Evacuate the vacuum chamber and preheat it to 400°C; The existing arc-enhanced glow discharge technology was used to ion clean and etch the tool substrate for 15 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, the N 2 The flow rate is 50sccm, the Ar flow rate is 100sccm, and the existing magnetron sputtering technology is used to coat the tool substrate to form a functional layer. The coating time is 70min; After coating, cool for 105 minutes.

[0030] The preparation method of the modified cubic boron nitride is as follows: putting cubic boron nitride powder into nitric acid with a mass fraction of 20% by weight, heating to 85°C, stirring for 2.5 hours, centrifuging, washing and drying for use to obtain product A; dispersing product A in water with a mass fraction of 7 times the weight of water, and passing N 2 O or N 2 The product B was obtained by filtration: the product B was dispersed in a siloxane solution with a weight of 6 times and a volume fraction of 2%, heated to 90°C, reacted for 4 hours, filtered, and vacuum dried to obtain modified cubic boron nitride.

[0031] In this embodiment, the preparation method of the modified silicon carbide is as follows: by weight, 8 parts of nano-silicon carbide are added to 35 parts of a hydrochloric acid solution with a mass fraction of 35%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 25 parts of a sodium chromate solution with a concentration of 150 g / L, and then 15 parts of glucose with a concentration of 45 g / L, 5 parts of polyethylene glycol with a concentration of 8 g / L, and 7 parts of sodium hexametaphosphate with a concentration of 30 g / L are added; the mixture is pumped into an autoclave under continuous stirring, heated to 155°C and reacted for 40 minutes; after the reaction is completed, the mixture is cooled to below 90°C, the suspension is extracted, filtered, washed, and dried, and the dried powder is sintered at 900°C for 3.5 hours to obtain modified silicon carbide.

[0032] In a specific implementation, the preparation method of the modified graphene is as follows: 5 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 1 part of nano-Cr powder is added and ball-milled for 40 minutes. The ball-milled liquid is stirred at a temperature of 140°C for 1.5 hours, and then freeze-dried at a temperature of -30°C for 4 hours to obtain modified graphene. Example 4

[0033] The embodiment of the present invention provides a high-hardness micro-diameter ball end milling cutter coating, such as Figure 1 As shown, at least one functional layer is deposited on the micro-diameter ball end milling cutter, the thickness of the functional layer is 2 μm, and the functional layer includes the following raw materials in parts by weight: 3.5 parts of aluminum oxide, 2.8 parts of modified cubic boron nitride, 2.5 parts of modified silicon carbide, 1.7 parts of modified graphene, and 2.5 parts of titanium nitride. The method for preparing the high-hardness micro-diameter ball end milling cutter coating includes the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate was immersed in acetone for ultrasonic cleaning for 5 minutes, then immersed in ethanol for ultrasonic cleaning for 6 minutes, blown dry, and placed in a vacuum chamber; The vacuum chamber is evacuated and preheated to 450°C; The existing arc-enhanced glow discharge technology was used to ion clean and etch the tool substrate for 20 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, the N 2 The flow rate is 60sccm, the Ar flow rate is 120sccm, and the existing magnetron sputtering technology is used to coat the tool substrate to form a functional layer. The coating time is 80min; After coating, cool for 120 minutes.

[0034] The preparation method of the modified cubic boron nitride is as follows: putting the cubic boron nitride powder into 7 times the weight of nitric acid with a mass fraction of 30%, heating to 90°C, stirring for 3 hours, centrifuging, washing and drying for use to obtain product A; dispersing product A in 8 times the weight of water, and passing N 2 O or N 2 The product B was obtained by filtration: the product B was dispersed in a siloxane solution with a weight of 7 times and a volume fraction of 3%, heated to 100°C, reacted for 5 hours, filtered, and vacuum dried to obtain modified cubic boron nitride.

[0035] In this embodiment, the preparation method of the modified silicon carbide is as follows: by weight, 10 parts of nano-silicon carbide are added to 40 parts of a hydrochloric acid solution with a mass fraction of 40%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 30 parts of a sodium chromate solution with a concentration of 200 g / L, and then 20 parts of glucose with a concentration of 50 g / L, 6 parts of polyethylene glycol with a concentration of 10 g / L, and 10 parts of sodium hexametaphosphate with a concentration of 40 g / L are added; the mixture is pumped into an autoclave under continuous stirring, heated to 160°C for reaction for 50 minutes; after the reaction is completed, the mixture is cooled to below 90°C, the suspension is extracted, filtered, washed, and dried, and the dried powder is sintered at 1000°C for 4 hours to obtain modified silicon carbide.

[0036] In a specific implementation, the preparation method of the modified graphene is as follows: 6 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 1.5 parts of nano-Cr powder are added and ball-milled for 50 minutes. The ball-milled liquid is stirred at a temperature of 160°C for 2 hours, and then freeze-dried at a temperature of -20°C for 5 hours to obtain modified graphene. Example 5

[0037] The embodiment of the present invention provides a high-hardness micro-diameter ball end milling cutter coating, such as Figure 1 As shown, at least one functional layer is deposited on the micro-diameter ball end milling cutter, the thickness of the functional layer is 2 μm, and the functional layer includes the following raw materials in parts by weight: 4 parts of aluminum oxide, 3 parts of modified cubic boron nitride, 3 parts of modified silicon carbide, 2 parts of modified graphene, and 3 parts of titanium nitride. The method for preparing the high-hardness micro-diameter ball end milling cutter coating includes the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate was immersed in acetone for ultrasonic cleaning for 5 minutes, then immersed in ethanol for ultrasonic cleaning for 6 minutes, blown dry, and placed in a vacuum chamber; The vacuum chamber is evacuated and preheated to 450°C; The existing arc-enhanced glow discharge technology was used to ion clean and etch the tool substrate for 20 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, the N 2 The flow rate is 60sccm, the Ar flow rate is 120sccm, and the existing magnetron sputtering technology is used to coat the tool substrate to form a functional layer. The coating time is 80min; After coating, cool for 120 minutes.

[0038] The preparation method of the modified cubic boron nitride is as follows: putting the cubic boron nitride powder into 7 times the weight of nitric acid with a mass fraction of 30%, heating to 90°C, stirring for 3 hours, centrifuging, washing and drying for use to obtain product A; dispersing product A in 8 times the weight of water, and passing N 2 O or N 2 The product B was obtained by filtration: the product B was dispersed in a siloxane solution with a weight of 7 times and a volume fraction of 3%, heated to 100°C, reacted for 5 hours, filtered, and vacuum dried to obtain modified cubic boron nitride.

[0039] In this embodiment, the preparation method of the modified silicon carbide is as follows: by weight, 10 parts of nano-silicon carbide are added to 40 parts of a hydrochloric acid solution with a mass fraction of 40%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 30 parts of a sodium chromate solution with a concentration of 200 g / L, and then 20 parts of glucose with a concentration of 50 g / L, 6 parts of polyethylene glycol with a concentration of 10 g / L, and 10 parts of sodium hexametaphosphate with a concentration of 40 g / L are added; the mixture is pumped into an autoclave under continuous stirring, heated to 160°C for reaction for 50 minutes; after the reaction is completed, the mixture is cooled to below 90°C, the suspension is extracted, filtered, washed, and dried, and the dried powder is sintered at 1000°C for 4 hours to obtain modified silicon carbide.

[0040] In a specific implementation, the preparation method of the modified graphene is as follows: 6 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 1.5 parts of nano-Cr powder are added and ball-milled for 50 minutes. The ball-milled liquid is stirred at a temperature of 160°C for 2 hours, and then freeze-dried at a temperature of -20°C for 5 hours to obtain modified graphene. Example 6

[0041] The embodiment of the present invention provides a high-hardness micro-diameter ball end milling cutter coating, such as Figure 2 As shown, it includes at least one functional layer deposited on the micro-diameter ball end milling cutter, the thickness of the functional layer is 1.5 μm, and the functional layer includes the following raw materials in parts by weight: 3 parts of aluminum oxide, 2.5 parts of modified cubic boron nitride, 3 parts of modified silicon carbide, 1.5 parts of modified graphene, and 2 parts of titanium nitride. The high-hardness micro-diameter ball end milling cutter coating preparation method includes the following steps: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate was immersed in acetone for ultrasonic cleaning for 4 minutes, and then immersed in ethanol for ultrasonic cleaning for 5 minutes and then blown dry. The part of the tool substrate to be coated was immersed under the liquid surface of the mixed liquid in the container, wherein the mixed liquid includes nano-titanium powder and Acetobacter xylinum fermentation liquid in a mass ratio of 1:25. After culturing at 30°C for 42 hours, the tool substrate was taken out, washed twice with distilled water, blown dry, and placed in a vacuum chamber; Evacuate the vacuum chamber and preheat it to 400°C; The existing arc-enhanced glow discharge technology was used to ion clean and etch the tool substrate for 15 minutes; N is continuously introduced into the vacuum chamber. 2 and Ar, the N 2 The flow rate is 50sccm, the Ar flow rate is 100sccm, and the existing magnetron sputtering technology is used to coat the tool substrate to form a functional layer. The coating time is 70min; After coating, cool for 105 minutes.

[0042] The preparation method of the modified cubic boron nitride is as follows: putting cubic boron nitride powder into nitric acid with a mass fraction of 20% by weight, heating to 85°C, stirring for 2.5 hours, centrifuging, washing and drying for use to obtain product A; dispersing product A in water with a mass fraction of 7 times the weight of water, and passing N 2 O or N 2 The product B was obtained by filtration: the product B was dispersed in a siloxane solution with a weight of 6 times and a volume fraction of 2%, heated to 90°C, reacted for 4 hours, filtered, and vacuum dried to obtain modified cubic boron nitride.

[0043] In this embodiment, the preparation method of the modified silicon carbide is as follows: by weight, 8 parts of nano-silicon carbide are added to 35 parts of a hydrochloric acid solution with a mass fraction of 35%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; the pretreated silicon carbide is added to 25 parts of a sodium chromate solution with a concentration of 150 g / L, and then 15 parts of glucose with a concentration of 45 g / L, 5 parts of polyethylene glycol with a concentration of 8 g / L, and 7 parts of sodium hexametaphosphate with a concentration of 30 g / L are added; the mixture is pumped into an autoclave under continuous stirring, heated to 155°C and reacted for 40 minutes; after the reaction is completed, the mixture is cooled to below 90°C, the suspension is extracted, filtered, washed, and dried, and the dried powder is sintered at 900°C for 3.5 hours to obtain modified silicon carbide.

[0044] In a specific implementation, the preparation method of the modified graphene is as follows: 5 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion, and then 1 part of nano-Cr powder is added and ball-milled for 40 minutes. The ball-milled liquid is stirred at a temperature of 140°C for 1.5 hours, and then freeze-dried at a temperature of -30°C for 4 hours to obtain modified graphene.

[0045] Comparative Example 1: Compared with Example 3, the modified cubic boron nitride is replaced by ordinary cubic boron nitride.

[0046] Comparative Example 2: Compared with Example 3, the modified silicon carbide is replaced by ordinary silicon carbide.

[0047] Comparative Example 3: Compared with Example 3, the modified graphene is replaced by ordinary graphene.

[0048] Comparative Example 4: Compared with Example 3, the modified cubic boron nitride is replaced by ordinary cubic boron nitride, the modified silicon carbide is replaced by ordinary silicon carbide, and the modified graphene is replaced by ordinary graphene.

[0049] Comparative Example 5: A commercially available coated micro-diameter ball end mill.

[0050] The microhardness of the coatings of Examples 1-6 and Comparative Examples 1-4 was measured using a nanoindenter. The test results are shown in the following table: Group Hardness (GPa) Example 1 42 Example 2 43 Example 3 45 Example 4 44 Example 5 43 Example 6 48 Comparative Example 1 31 Comparative Example 2 30 Comparative Example 3 32 Comparative Example 4 26 Comparative Example 5 25 It can be seen from the above results that the coating prepared by the present invention has high hardness, and by adding modified cubic boron nitride, modified silicon carbide and modified graphene, the three have a synergistic effect and can improve the hardness of the coating.

[0051] It should be noted that, for the above embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.

[0052] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. A high-hardness micro-diameter ball end mill coating, comprising at least one functional layer deposited on the micro-diameter ball end mill, characterized in that: The thickness of the functional layer is 1-2 μm, and the functional layer comprises the following raw materials in parts by weight: 2-4 parts of aluminum oxide, 2-3 parts of modified cubic boron nitride, 1-3 parts of modified silicon carbide, 1-2 parts of modified graphene, and 1-3 parts of titanium nitride.

2. The high-hardness micro-diameter ball end mill coating according to claim 1, characterized in that: The functional layer comprises the following raw materials in parts by weight: 2.5-3.5 parts of aluminum oxide, 2.2-2.8 parts of modified cubic boron nitride, 1.5-2.5 parts of modified silicon carbide, 1.3-1.7 parts of modified graphene, and 1.5-2.5 parts of titanium nitride.

3. The high-hardness micro-diameter ball end mill coating according to claim 2, characterized in that: The functional layer includes the following raw materials in parts by weight: 3 parts of aluminum oxide, 2.5 parts of modified cubic boron nitride, 3 parts of modified silicon carbide, 1.5 parts of modified graphene, and 2 parts of titanium nitride.

4. The high-hardness micro-diameter ball end mill coating according to claim 1, characterized in that: The preparation method of the modified cubic boron nitride is as follows: putting cubic boron nitride powder into nitric acid with a mass fraction of 10-30% by weight and heating to 80-90°C, stirring for 2-3h, centrifuging, washing and drying for standby use to obtain product A; dispersing product A in water with a weight of 6-8 times, irradiating under the condition of passing N2O or N2, the ventilation time is 20-30min, the dose rate of the irradiation treatment is 70-90Gy / min, the total dose is 90-100kGy, filtering to obtain product B: dispersing product B in a siloxane solution with a weight of 4-7 times and a volume fraction of 1-3%, heating to 80-100°C, reacting for 3-5h, filtering, and vacuum drying to obtain modified cubic boron nitride.

5. The high-hardness micro-diameter ball end mill coating according to claim 1, characterized in that: The preparation method of the modified silicon carbide is as follows: by weight, 6-10 parts of nano silicon carbide are added to 30-40 parts of a hydrochloric acid solution with a mass fraction of 30-40%, and after sufficient stirring, centrifugation, washing, and drying are performed in sequence to obtain pretreated silicon carbide; The pretreated silicon carbide is added to 20-30 parts of a sodium chromate solution with a concentration of 100-200 g / L, and then 10-20 parts of glucose with a concentration of 40-50 g / L, 4-6 parts of polyethylene glycol with a concentration of 5-10 g / L, and 5-10 parts of sodium hexametaphosphate with a concentration of 20-40 g / L are added; the solution is pumped into an autoclave under continuous stirring, heated to 150-160°C and reacted for 30-50 minutes; after the reaction is completed, the solution is cooled to below 90°C, the suspension is pumped out, filtered, washed, and dried, and the dried powder is sintered at 800-1000°C for 3-4 hours to obtain modified silicon carbide.

6. The high-hardness micro-diameter ball end mill coating according to claim 1, characterized in that: The preparation method of the modified graphene is as follows: 4-6 parts of graphene oxide are dispersed in anhydrous ethanol by weight and ultrasonically vibrated to prepare a graphene oxide dispersion liquid, and then 0.5-1.5 parts of nano Cr powder are added and ball milled for 30-50 minutes, and the ball-milled liquid is stirred at a temperature of 120-160° C. for 1-2 hours, and then freeze-dried at a temperature of -40 to -20° C. for 3-5 hours to obtain the modified graphene.

7. The method for preparing a high-hardness micro-diameter ball-end milling cutter coating according to any one of claims 1 to 6, characterized in that: The steps include: Weigh the raw materials of the functional layer according to the ratio and mix them evenly as the target material; The tool substrate is pre-treated and placed in a vacuum chamber; Evacuate the vacuum chamber and preheat it to 350-450°C; The existing arc-enhanced glow discharge technology is used to ion clean and etch the tool substrate for 10-20 minutes; N2 and Ar are continuously introduced into the vacuum chamber, and the tool substrate is coated with a film by using the existing magnetron sputtering technology to form a functional layer; After coating, cool for 90-120 minutes.

8. The method for preparing a high-hardness micro-diameter ball-end milling cutter coating according to claim 7, characterized in that: The N2 flow rate is 40-60 sccm, the Ar flow rate is 80-120 sccm, and the coating time is 60-80 min.

9. The method for preparing a high-hardness micro-diameter ball-end milling cutter coating according to claim 7, characterized in that: The pretreatment of the tool substrate comprises immersing the tool substrate in acetone for ultrasonic cleaning for 3-5 minutes, then immersing the tool substrate in ethanol for ultrasonic cleaning for 4-6 minutes, and then blowing it dry.

10. The method for preparing a high-hardness micro-diameter ball-end milling cutter coating according to claim 9, characterized in that: The method also includes, after drying, immersing the to-be-coated portion of the tool substrate under the liquid surface of a mixed liquid in a container, wherein the mixed liquid includes nano-titanium powder and Acetobacter xylinum fermentation liquid in a mass ratio of 1:20-30, culturing at 30-35°C for 36-48 hours, taking out the tool substrate, washing it with distilled water 2-3 times, and then drying it.

Citation Information

Patent Citations

  • Surface roughening treatment method for cubic boron nitride base body, modified cubic boron nitride base body and cubic boron nitride coated cutting tool

    CN105951039A

  • Titanized cubic boron nitride clad sheet and preparation process thereof

    CN108950561A

  • Integral PCBN blade and preparation method thereof

    CN108971497A

  • Bonding agent, polycrystalline cubic boron nitride tool and preparation method of polycrystalline cubic boron nitride tool

    CN109574678A

  • High-toughness thermally conductive polycrystalline cubic boron nitride composite sheet and preparation method thereof

    CN111961943A

Cited By

  • A wear-resistant coated ball end mill based on automotive stamping dies

    CN224977575U