Scale preparation method and application of CoNi-Al-based heterojunction material
Through the preparation method of CoNi-Al based heterostructure, the problem of competitive hydrogen evolution reaction of electrocatalysts at high overpotential is solved, and efficient preparation of p-aminobenzoic acid is achieved. It has excellent catalytic activity and stability and is suitable for industrial applications. .
Patent Information
- Application Number
- CN202410645693.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-10-01
AI Technical Summary
Existing electrocatalysts suffer from irrepressible competitive hydrogen evolution reaction at high overpotential, resulting in low Faradaic efficiency and insufficient material cycle stability, which limits the efficient preparation of p-aminobenzoic acid.
Using the preparation method of CoNi-Al based heterostructure, the conductive base electrode is incubated in a cobalt source solution, ultrasonic treated and reacted in a dimethylimidazole aqueous solution, and hydrothermal treatment is performed in combination with aluminum nitrate and urea to form a flower cluster-shaped heterostructure. Mass junction material, used for electrocatalytic reduction of p-nitrobenzoic acid to p-aminobenzoic acid.
It improves the catalytic activity and realizes the batch synthesis of high value-added chemicals. It has excellent conversion rate, selectivity and Faradaic efficiency, and is suitable for industrial production.
Smart Images

Figure CN118726973A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic nano functional materials, and specifically relates to a large-scale preparation method of a CoNi-Al-based heterojunction material and application thereof. Background Art
[0002] PABA (para-aminobenzoic acid) is an important substrate for the synthesis of various biological scaffolds. Drugs such as folic acid and benzocaine are used to treat certain biological diseases, and their pharmacological significance is obvious. Although it is not a vitamin, it is still called a member of the vitamin B group. PABA deficiency can lead to several diseases such as unstable white areas of the skin, gray hair, fatigue, depression and irritability. In addition to its important medicinal value, PABA is also used to synthesize various biologically active heterocyclic nuclei such as benzimidazoles, aziridones, thiazolidinones, pyrazoline, etc. It has the importance of being a multifunctional substrate. Para-nitrobenzoic acid (PNBA) as a nitroaromatic pollutant has adverse effects on the natural environment and human body, so it is of extraordinary significance to hydrogenate PNBA to high value-added PABA. Electrocatalytic hydrogenation is an economical and sustainable method for the preparation of high-purity para-aminobenzoic acid (PABA) with high selectivity, high yield and Faradaic efficiency. However, the existing electrocatalysts lack research on them, and the low Faraday efficiency caused by the unsuppressible competitive hydrogen evolution reaction at high overpotential and the cyclic stability of the material itself hinder its realization. Therefore, the electrocatalytic reduction technology is used to convert them into high value-added molecules to promote the application of electrocatalytic synthesis technology in industrial production. Summary of the invention
[0003] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0004] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0005] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a CoNi-Al based heterostructure.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a CoNi-Al-based heterostructure, characterized in that: it comprises:
[0007] The conductive substrate electrode is immersed in a cobalt source solution and kept warm to obtain a substrate loaded with basic cobalt salt, the substrate solution is ultrasonically treated in water and anhydrous ethanol in sequence, and finally the substrate loaded with basic cobalt salt is placed in a vacuum drying oven for drying;
[0008] The above-mentioned substrate loaded with alkali cobalt salt was transferred into a beaker of dimethylimidazole aqueous solution, stirred evenly, and the reaction was completed at room temperature. The substrate was washed with anhydrous ethanol and deionized water, and the sample was vacuum dried to obtain the prepared cobalt-based MOF precursor.
[0009] Put aluminum nitrate and urea into a beaker and stir evenly. Then put the CNH-ZIF precursor and the solution in the beaker into the reactor and heat until the reaction is completed. Wash with anhydrous ethanol and deionized water, and dry the sample under vacuum to obtain a CoNi-Al-based heterostructure.
[0010] As a preferred embodiment of the preparation method described in the present invention, the conductive base electrode material includes one or more of carbon paper, nickel foam, copper foam, and stainless steel mesh; the cobalt source solution is any one of a cobalt salt aqueous solution, a cobalt salt ionic liquid, and a cobalt salt low-temperature molten salt, wherein the low-temperature molten salt includes at least one of a cobalt salt or an ionic liquid having a melting point below 400°C; the ionic liquid includes a molten salt that is in a liquid state at a temperature below 100°C, one or more of imidazoles, ammonium salts, and tetrafluoroborates; the nickel aluminum source includes at least one of nitrates, chlorides, sulfates, phosphates, acetates, and carbonates, wherein the molar ratio of CoNiAl is 0.1-5:0.5-10:10-30.
[0011] As a preferred embodiment of the preparation method of the present invention, the size of the foam nickel substrate is at least 4 cm×4 cm, and it is immersed in a cobalt source solution, wherein the insulation temperature is 90-120° C., the time is 6-10 hours, the ultrasonic time is 10 minutes, and the vacuum drying temperature is 60° C., and the time is 5-6 hours.
[0012] As a preferred embodiment of the preparation method of the present invention, the stirring time of the above-mentioned base solution loaded with basic cobalt salt into the dimethylimidazole aqueous solution is 30 minutes, the reaction temperature is 20-25° C., and the reaction time is 5-10 hours.
[0013] The cobalt-based MOF-loaded precursor is transferred into an aqueous solution of aluminum nitrate and urea, the reaction temperature is 140° C., and the reaction time is 8 to 12 hours.
[0014] As a preferred embodiment of the preparation method of the present invention, the washing with anhydrous ethanol and deionized water is performed for more than 3 times, and the sample after washing is vacuum dried at a temperature of 60° C. for 6 hours.
[0015] As a preferred embodiment of the preparation method of the present invention, the CoNi-Al heterostructure has a molar ratio of CoNiAl of about 5:4:24, and the volume of the formed solution is 10 to 100 mL.
[0016] The molar ratio of CoNiAl is about 5:4:24, and the volume of the solution is 10-100 mL.
[0017] As a preferred embodiment of the preparation method of the present invention, the working electrode electrolyte of the CoNi-Al heterostructure in the electrolyte cell is an aqueous solution containing p-nitrobenzoic acid with a concentration of 5 mM or more.
[0018] As a preferred embodiment of the preparation method of the present invention, the application system is a three-electrode system, an H-type electrolytic cell is used, a stone mill rod sheet / platinum sheet is used as the counter electrode, a reference electrode is a calomel electrode, the electrolyte solution is a neutral PBS solution, the pH is about 7, the electrolysis voltage is 0.4V to -0.8V, and the constant voltage reaction is for more than 0.5h.
[0019] As a preferred embodiment of the preparation method of the present invention, the CoNi-Al heterostructure is used as a cathode catalyst, and p-nitrobenzoic acid can be converted into high-value-added chemicals such as sodium salt, potassium salt and ammonium salt corresponding to p-aminobenzoic acid through electrocatalytic reduction.
[0020] As a preferred embodiment of the preparation method of the present invention, the application of the CoNi-Al-based heterostructure in electrocatalytic synthesis can realize the large-scale synthesis of high-value-added chemicals by continuously adding the raw material p-nitrobenzoic acid during the reaction process.
[0021] Another object of the present invention is to overcome the deficiencies in the prior art and provide a product obtained by a method for preparing a CoNi-Al based heterostructure.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a CoNi-Al-based heterostructure and use the product in the electrosynthesis of gram-level p-aminobenzoic acid.
[0023] Beneficial effects of the present invention:
[0024] (1) The present invention provides a synthesis scheme for forming a flower cluster heterojunction material by combining a cobalt salt and an aluminum salt, which realizes the synthesis of MOFs by room temperature from a simple synthesized transition metal basic salt during the reaction process, and then forms a heterojunction structure by low temperature hydrothermal treatment, thereby optimizing the surface morphology and improving the catalytic activity of the material. The synthesis process is simple, can be synthesized in batches, is environmentally friendly and economical, has low raw material costs, and meets the requirements of industrial applications. This material has excellent performance in the field of electrocatalytic reduction of p-nitrobenzoic acid to p-aminobenzoic acid.
[0025] (2) The present invention provides a method for preparing the above-mentioned electrode material, which is prepared by three steps: a cobalt salt loading method, a room temperature solvent soaking method, and a hydrothermal method. The nickel foam is soaked in a cobalt nitrate aqueous solution and kept at 90-120°C for 6-10 hours to obtain in situ grown basic cobalt nitrate (referred to as CNH); the base solution of the basic cobalt salt loaded is transferred into a dimethylimidazole aqueous solution with a stirring time of 30 minutes, a reaction temperature of 20-25°C, and a time of 5-10 hours; the precursor of the cobalt-based MOF loaded is transferred into an aluminum nitrate and urea aqueous solution, the reaction temperature is 140°C, and the time is 8-12 hours; it is naturally cooled to room temperature, washed with anhydrous ethanol and deionized water for more than 3 times, and the prepared sample is vacuum dried at 60°C for 10 hours to obtain the prepared electrode material. The synthesis method is simple and convenient, and the mild conditions are conducive to large-scale industrial production.
[0026] (3) The present invention provides a CoNi-Al-based heterostructured mixed electrode material, which has the unique advantage of being able to be prepared on a large scale and has broad application prospects in the field of electrocatalytic oxidation of biomass small molecules, especially in the electrocatalytic reduction of p-nitrobenzoic acid to prepare p-aminobenzoic acid, with excellent conversion rate, high p-aminobenzoic acid selectivity, high Faraday efficiency and good stability. In the entire reaction process, the device is simple, so it has broad market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0028] The electrode material is referred to as CoAlCH / Al(OH)3.
[0029] Figure 1 The powder X-ray diffraction pattern of the typical CoAlCH / Al(OH)3 electrode material and the precursor CNH-ZIF described in Example 1
[0030] Figure 2 This is the EDX spectrum of CoAlCH / Al(OH)3 electrode.
[0031] Figure 3 This is a scanning electron microscope image of the typical CoAlCH / Al(OH)3 electrode material described in Example 1.
[0032] Figure 4 This is the XPS energy spectrum of the CoAlCH / AlAl(OH)3 electrode material described in Example 1.
[0033] Figure 5 The CoAlCH / AlAl(OH)3 electrode material described in Example 1 was 5mVs -1 Polarization curves with scan rate.
[0034] Figure 6 This is a liquid chromatogram of the product obtained from the CoAlCH / AlAl(OH)3 electrode material described in Example 1.
[0035] Figure 7 Graph showing the yield, conversion rate and Faraday efficiency of the cyclic stability of the CoAlCH / AlAl(OH)3 electrode material described in Example 1.
[0036] Figure 8 Electrode materials prepared on a large scale.
[0037] Fig. 9 The electrode materials prepared in Examples 2 to 7 were 5 mVs -1 Polarization curves with scan rate.
[0038] Fig.10 The CoAlCH / AlAl(OH)3 electrode material described in Example 1 and the material of Comparative Example 1 are the CoAlCH / AlAl(OH)3 electrode materials described in Example 1. DETAILED DESCRIPTION
[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0040] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0041] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0042] Example 1
[0043] The present invention provides a large-scale preparation method of a CoNi-Al-based heterojunction material:
[0044] (1) 10 g of cobalt nitrate was placed in a polytetrafluoroethylene inner chamber containing 100 mL, and then placed in an oven and kept at 120°C for 6 h. A 4*4 cm flat piece of nickel foam was placed in the oven and immersed in the cobalt nitrate solution to obtain basic cobalt nitrate (denoted as CNH) grown in situ on the nickel foam.
[0045] (2) CNH was ultrasonically treated in water and anhydrous ethanol for 10 min, and finally CNH was placed in a vacuum drying oven at 60°C for 6 h; 2 g of 2-methylimidazole was dissolved in water, stirred evenly, and then CNH was transferred into the solution, kept at room temperature for 5 h, washed with anhydrous ethanol and deionized water for more than 3 times, and placed in a vacuum drying oven at 60°C for 6 h to obtain ZIF generated by basic cobalt nitrate (referred to as CNH-ZIF).
[0046] (3) 2 g of aluminum nitrate was put into a 100 mL beaker and stirred, and the aluminum nitrate solution and CNH-ZIF were put into a reactor together and kept at 140°C for 6 h; naturally cooled to room temperature, washed with anhydrous ethanol and deionized water for more than 3 times, and the prepared sample was vacuum dried at 60°C for 6 h to obtain the prepared electrode material (CoNiCH / Al(OH)3).
[0047] Example 2
[0048] The difference from Example 1 is that the cobalt source in step (1) is cobalt nitrate, the aluminum source in step (3) is aluminum sulfate, the molar ratio of cobalt source: aluminum source: aqueous solution is 1:5:10, the substrate is nickel foam, the reaction temperature is 130°C, and the time is 10 h.
[0049] Example 3
[0050] The difference from Example 1 is that the cobalt source in step (1) is cobalt nitrate, the liquid in (2) is DMF, the aluminum source in step (3) is aluminum sulfate, the molar ratio of cobalt source: aluminum source: ionic liquid is 1:10:20, the substrate is nickel foam, the reaction temperature is 150°C, and the time is 10 h.
[0051] Example 4
[0052] The difference from Example 1 is that in step (1), the type of cobalt source is cobalt carbonate, in (2), the type of liquid is ethyl acetate, in step (3), the nickel source is nickel nitrate, and is synchronously mixed with aluminum nitrate, the molar ratio of cobalt source: aluminum source: nickel source: ionic liquid is 0.5:1:0.5:5, the substrate is foamed copper, the reaction temperature is 160°C, and the time is 1 hour.
[0053] Example 5
[0054] The difference from Example 1 is that the cobalt source in step (1) is cobalt sulfate, the liquid in (2) is acetonitrile, the aluminum source in step (3) is aluminum sulfate, the molar ratio of cobalt source: aluminum source: ionic liquid is 0.5:20:10, the reaction temperature is 170°C, and the reaction time is 2h.
[0055] Example 6
[0056] The difference from Example 1 is that in step (1), the cobalt source is cobalt nitrate, which is dissolved in 100 mL of water, and then the nickel foam is placed therein and kept warm at 130° C., in step (3), the aluminum source is aluminum nitrate, the molar ratio of cobalt source: aluminum source: ionic liquid is 0.1:10:5, the substrate is nickel foam, the reaction temperature is 160° C., and the time is 3 h.
[0057] The crystal structure of the CoNi-Al based heterojunction material prepared in Example 1 was analyzed:
[0058] Powder X-ray diffraction was carried out on a D8 X-ray powder diffractometer from Bruker, Germany, with a fixed target monochromatic light source of Cu-Kα and a wavelength of The scanning range was 5-60°, and the scanning step was 0.02°. Sample 1# was a typical electrode material prepared in Example 1.
[0059] like Figure 1 The X-ray diffraction pattern obtained by fitting is consistent with Figure 1 By comparing the spectrum obtained by X-ray diffraction test after scraping the powder from sample 1#, it can be found that the prepared heterojunction contains (NixCoy)(OH)(CO3)(PDF#33-0429) and Al(OH)3(PDF#37-1377), indicating that under mild and environmentally friendly conditions, basic cobalt nitrate can be easily grown on nickel foam in the form of molten salt on a large scale, and then the aluminum source is introduced by a mild hydrothermal method to successfully form a regular CoNi-Al trimetallic hydroxide heterojunction electrode material on the substrate.
[0060] In addition, from Figure 2 From the EDX spectrum, it can be found that the main components of the material are Ni, Co, O, C, and Al, which further proves that the obtained material is a CoNi-Al trimetallic hydroxide heterojunction material.
[0061] The CoNi-Al based heterojunction material prepared in Example 1 was subjected to characterization tests:
[0062] The morphology of the prepared Example 1 was characterized by SEM. The prepared precursor material has a regular cubic structure as a whole, a length of nanometers, a relatively uniform morphology, and a smaller size than the existing materials, such as Figure 3(df) As shown; after the Al source is introduced, a large number of petal-like structures are grown on the original sheet layer, such as Figure 3 As shown in (ac), a heterojunction structure is formed, which increases the contact area between the catalyst and the reaction substrate and exposes more reaction active sites, thereby improving the catalytic activity of the catalyst.
[0063] Figure 4 The XPS spectrogram of the CoAlCH / AlAl(OH)3 electrode material described in Example 1 confirms the presence of Ni, Co, Al, O and C on the surface of the electrocatalyst by x-ray photoelectron spectroscopy (XPS), which is consistent with the results of EDS, and further studies the chemical composition and chemical state of the surfaces of these products. Ni is represented by two significant peaks of 856.3eV and 873.9eV, respectively, indicating that Ni is in the Ni2+ oxidation state. As can be seen from the Al figure, there are two peaks with binding energies of 74.1eV and 68.3eV, respectively, indicating the presence of Al3+. In the Co spectrum, two groups of peaks can be seen, namely satellite peaks with combined energies of 797.3eV and 802.1eV and satellite peaks with combined energies of 781.2eV and 785.7eV. In the O spectrum, three main peaks of Metal-O bond (530.7eV), Metal-OH bond (531.5eV) and surface adsorbed water molecules (533.0eV) can be clearly identified.
[0064] The polarization curve of the CoNi-Al based heterojunction material prepared in Example 1 is as follows:
[0065] The CoNiCH / Al(OH)3 heterojunction electrode material was used as the working electrode, and the calomel electrode and Pt sheet were used as the reference electrode and counter electrode, respectively. 0.1M PBS neutral solution and 50mM p-nitrobenzoic acid (PNBA) were used as the electrolyte and electrolyte, respectively. The electrochemical workstation was operated at 5mV·s -1 The LSV polarization curve test was performed at a rate of 100 mV / s. Before the linear sweep voltammetry (LSV) test, 20 cycles were scanned at 100 mV / s to reach a stable state, and then the test was performed at a scan rate of 5 mV / s. The potential value was calculated according to the equation E vs RHE = E vs SCE + 0.2412 + 0.0591 pH, where E vs RHE is the relative reversible hydrogen electrode potential (V) and E vs SCE is the relative saturated calomel electrode potential (V). The polarization curve is shown in Figure 5 As shown in the figure, the CoNiCH / Al(OH)3 heterojunction electrode material has excellent performance for PNBA reduction, and the current density can exceed -200mA / cm at -0.6V (vsRHE). 2 , meeting industrial current density requirements and can be used in industrial production applications.
[0066] The catalytic reaction path, after detecting the intermediate product, PNBA is converted into p-aminobenzoic acid (PABA) under the conditions of the invention. Therefore, in the whole process, 6 electrons are transferred, and 1 mol of PABA can be obtained for every 1 mol of PNBA converted.
[0067] Liquid chromatogram of the CoNi-Al based heterojunction material prepared in Example 1:
[0068] CoNiCH / Al(OH)3 was electrocatalyzed in a 0.1M PBS neutral solution containing 50mM PNBA, and the products obtained at different reaction times were characterized by liquid chromatography, such as Figure 6 Shown are the retention time and peak area of each product in HPLC at different reaction times.
[0069] The p-aminobenzoic acid yield, Faraday efficiency and cycle stability of the CoNi-Al based heterojunction material prepared in Example 1 are:
[0070] The CoNiCH / Al(OH)3 electrode was placed in an H-type electrolytic cell as the working electrode, the calomel electrode as the reference electrode, the Pt sheet as the counter electrode, the Nafion proton exchange membrane as the diaphragm, and a 0.1M PBS neutral solution containing 50mM PNBA as the electrolyte. Figure 7 As shown, the bar graph represents the yield, PABA selectivity and Faraday efficiency from left to right, and the horizontal axis represents the number of cycles. Under the same voltage, multiple cycles show higher PABA yield and high Faraday efficiency, indicating that the prepared electrode material has the characteristics of high yield and high catalytic stability for the electrocatalytic reduction of PNBA.
[0071] The recyclability of CoNiCH / Al(OH)3 electrode material was tested in 0.1M PBS neutral solution at -0.545V vs RHE voltage. Figure 7 As shown, after 8 cycles, the catalyst can still maintain excellent PNBA reduction conversion efficiency (≥88%) and high selectivity (≥88%). This shows that the stability and cyclic practicability of the prepared catalyst are conducive to industrial application and promotion, and this technology has certain guiding significance for the material synthesis of electrocatalytic biomass small molecules.
[0072] Achieve large-scale production of electrode materials and enable reactions to scale to the gram level.
[0073] First large-scale synthesis of 4x4cm 2 CoNiCH / Al(OH)3 electrodes of different sizes, as shown in the actual picture Figure 8 ; Add 25mmol PNBA reaction material (about 4.175g) and place it in a 4x 4cm 2The large and small CoNiCH / Al(OH)3 were used as electrodes. After 42 hours of reaction, the reaction solution was diluted and analyzed by high performance liquid chromatography. The yield was 80%, indicating that the electrode material has the advantage of being scalable under electrosynthesis conditions.
[0074] Commercial nickel foam electrode material was used as the working electrode, saturated calomel electrode and stone mill rod were used as the reference electrode and counter electrode respectively, and placed in 50 mL aqueous solution containing 0.1 M PBS and 0.1 M PBS and 50 mM PNBA to carry out electrochemical catalytic reaction. Fig.10 As shown in the figure, it can be seen from the LSV curve that after adding PNBA, the applied voltage is reduced, but it is higher than the electrode material prepared by the present invention. It can be seen that the heterojunction material prepared by the present invention has significant advantages over the existing commercial electrode materials.
[0075] Comparative Example 1
[0076] (1) 10 g of cobalt nitrate was placed in a polytetrafluoroethylene inner tube containing 100 mL, and a 4*4 cm flat piece of nickel foam was placed in a beaker to immerse it in the cobalt nitrate solution and kept at 120°C for 6 h. The mixture was then placed in a reactor and then in an oven. CNH was ultrasonically treated in water and anhydrous ethanol for 10 min. Finally, the CNH was placed in a vacuum drying oven at 60°C for 6 h to obtain basic cobalt nitrate (referred to as CNH) grown in situ on the nickel foam.
[0077] (2) Dissolve 2 g of 2,5-dihydroxyterephthalic acid in water and stir evenly, then transfer CNH into the solution and keep it at room temperature for 5 h. Take it out and wash it with anhydrous ethanol and deionized water for more than 3 times, put it in a vacuum drying oven at 60°C and dry it for 6 h to obtain Co-MOF-74 generated by basic cobalt nitrate.
[0078] (3) 2 g of aluminum nitrate was put into a 100 mL beaker and stirred, and the aluminum nitrate solution and CNH-ZIF were put into a reactor together and kept at 140 ° C for 6 h; naturally cooled to room temperature, washed with anhydrous ethanol and deionized water for more than 3 times, and the prepared sample was vacuum dried at 60 ° C for 6 h to obtain the prepared electrode material (CoNiCH / Al(OH)3), with a final effect yield of 75%.
[0079] Comparative Example 2
[0080] 1g of cobalt nitrate and aluminum nitrate and 3g of 2-methylimidazole were placed in a polytetrafluoroethylene inner village containing 100mL, and then placed in a reactor, and then placed in an oven, and a 4*4cm flat piece of nickel foam was placed in a beaker to immerse it in the solution, and kept warm at 120°C for 6h, ultrasonically treated in water and anhydrous ethanol for 10min, and finally placed in a vacuum drying oven at 60°C for 6h to obtain an in-situ growth material on the nickel foam, with a final yield of 60%.
[0081] Comparative Example 3
[0082] Put 1g of cobalt nitrate and 1g of syringic acid in a 100mL polytetrafluoroethylene inner village, and take a 4*4cm flat piece of nickel foam and put it in a beaker to soak it in the solution, then put it into a reactor, and then put it in an oven and keep it at 140℃ for 10h, ultrasonically treat it in water and anhydrous ethanol for 10min, and finally put it in a vacuum drying oven at 60℃ for 6h to obtain the in-situ growth material on the nickel foam, with a final effect yield of 70%.
[0083] Comparative Example 4
[0084] 1g of copper nitrate and 1g of syringic acid were placed in a 100mL polytetrafluoroethylene inner chamber, and a 4*4cm flat piece of nickel foam was placed in a beaker to immerse it in the solution, and then placed in a reactor, and then placed in an oven and kept at 140°C for 10h, ultrasonically treated in water and anhydrous ethanol for 10min, and finally placed in a vacuum drying oven at 60°C for 6h to obtain an in-situ grown material on the nickel foam, and then in-situ reduced for 600s at a potential of 1.2V vs. RHE to obtain SyA-Cu / Cu, with a final yield of 66%.
[0085] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing a CoNi-Al heterojunction material, Features: include, The substrate loaded with alkali cobalt salt is mixed with a dimethylimidazole aqueous solution, stirred evenly, and the reaction is completed at room temperature, and then washed with anhydrous ethanol and deionized water, and vacuum dried to obtain a cobalt-based MOF precursor; The aluminum salt and alkaline medium aqueous solution are mixed and then added to the MOF precursor substrate and heated to react to obtain the CoNi-Al based heterojunction material.
2. The preparation method according to claim 1, Features: The base loaded with alkali cobalt salt is obtained by soaking a conductive base electrode in a cobalt source solution for heat preservation, then ultrasonically treating the solution in water and anhydrous ethanol, and vacuum drying the solution.
3. The preparation method according to claim 2, Features: The conductive base electrode material includes one or more of carbon paper, nickel foam, copper foam, and stainless steel mesh; the cobalt source solution is any one of a cobalt salt aqueous solution, a cobalt salt ionic liquid, and a cobalt salt low-temperature molten salt, wherein the low-temperature molten salt includes at least one of a cobalt salt or an ionic liquid with a melting point below 400°C; the ionic liquid includes a molten salt that is in a liquid state at a temperature below 100°C, one or more of imidazoles, ammonium salts, and tetrafluoroborates; the nickel aluminum source includes at least one of nitrates, chlorides, sulfates, phosphates, acetates, and carbonates, wherein the molar ratio of CoNiAl is 0.1-5:0.5-10:10-30.
4. The preparation method according to claim 2, Features: The insulation temperature is 90-120° C., the time is more than 6 hours, the ultrasonic time is more than 10 minutes, and the vacuum drying temperature is 60° C., and the time is 5 hours.
5. The preparation method according to claim 1, Features: The loaded basic cobalt salt substrate is transferred into a dimethylimidazole aqueous solution and stirred for more than 30 minutes, the reaction temperature is 20-25°C, and the time is more than 5 hours; the loaded cobalt-based MOF precursor is transferred into an aluminum salt and alkaline medium aqueous solution, the reaction temperature is 140°C, and the time is 8-12 hours.
6. The preparation method according to claim 1, Features: The alkaline medium aqueous solution includes at least one of thiourea, urea, sodium carbonate and potassium carbonate.
7. The CoNi-Al based heterojunction material obtained by the preparation method according to claims 1 to 6.
8. Application of the CoNi-Al based heterojunction material according to claim 7, Features: The applications include electrocatalytic treatment of nitrate-containing wastewater, soil remediation, coatings, anti-counterfeiting, printing, textiles, toxic gas adsorption environmental engineering, synthesis of pharmaceutical intermediates, and electrocatalytic reduction of organic nitrobenzene and its derivatives to amines.
9. The use according to claim 8, Features: The application in the field of electrocatalytic reduction of organic nitrobenzene and its derivatives into amines includes: the heterojunction material is used as a cathode catalyst to reduce nitrobenzene and its derivatives into high-value-added aromatic amine chemicals through electrocatalytic reduction.
10. The use according to claim 9, Features: The CoNi-Al-based heterojunction material is used as an electrocatalytic reducing agent for electrocatalytic hydrogenation reaction, using a stone mill rod sheet / platinum sheet as a counter electrode, a reference electrode as a calomel electrode, an electrolyte solution as a neutral PBS solution, a pH of about 7, an electrolysis voltage of -0.4V to -0.8V, and a constant voltage reaction of more than 0.5h.
Citation Information
Patent Citations
NiCoAl-LDH-modified ferric oxide composite photoanode material and preparation method and application thereof
CN107268021A
Three-dimensional multi-layered structure cobalt-nickel-aluminum ternary metal electrocatalyst for oxygen evolution reaction as well as preparation and application methods thereof
CN108531938A
Ni-Co-ZIF composite material and preparation method and application thereof
CN114044912A
Metal organic framework loaded substrate composite material and preparation method and application thereof
CN114433235A
Catalyst as well as preparation method and application thereof
CN116062722A