Abnormal-period process control method and fully-graphitized cathode aluminum electrolysis cell
By adjusting the parameters such as voltage, temperature and liquid level height through the abnormal period process control method, the problem of excessive bath temperature and anode carbon block cracking in the fully graphitized cathode aluminum electrolytic cell during the abnormal period is solved, and the use of the electrolytic cell is extended. lifespan and reduced energy consumption.
Patent Information
- Application Number
- CN202410827659.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-01
AI Technical Summary
Fully graphitized cathode aluminum electrolytic cells are prone to problems such as excessive cell temperature, cracking of anode carbon blocks, and irregular furnace sides during abnormal periods, which affects the life of the cell.
An abnormal period process control method is proposed. By obtaining the duration of the abnormal period, the process parameter control strategy for the corresponding time period is determined, including voltage control, electrolyte temperature control, aluminum liquid level height control, electrolyte liquid level height control, molecular Ratio control and anode replacement control, and the production process is adjusted based on these strategies.
Effectively stabilize key variables in the production process, reduce energy consumption, extend the service life of electrolytic cells and anodes, reduce maintenance and replacement costs, and improve operating efficiency and cell stability.
Smart Images

Figure CN118727064A_ABST
Abstract
Description
Technical Field
[0001] The present specification relates to the field of electrolytic aluminum production, and more specifically, the present application relates to an abnormal period process control method and a fully graphitized cathode aluminum electrolytic cell. Background Art
[0002] As a major aluminum industry country, my country's primary aluminum output in 2023 will be 41.59 million tons, accounting for 59.6% of the world's total. Electrolytic aluminum is a high-energy consumption, high-pollution, and low-energy-efficiency industry. The rapid development of the aluminum industry has brought huge energy and environmental pressures. Faced with the pressure of national energy conservation, emission reduction and electricity consumption policies, electrolytic aluminum companies urgently need to comprehensively reduce aluminum electrolysis energy consumption indicators.
[0003] In recent years, the domestic aluminum electrolysis industry has generally begun to adopt full graphitized cathode technology in order to further reduce energy consumption indicators. Fully graphitized cathode carbon blocks have the characteristics of low resistance, high thermal conductivity and small sodium expansion. In particular, the room temperature resistivity can be reduced by more than 60% compared with GS-3 and GS-5 carbon materials. The furnace bottom pressure drop of the electrolytic cell using fully graphitized cathode can reach below 200mV, and the working voltage can be achieved below 3.8V.
[0004] At present, in order to adapt to the low resistance and high thermal conductivity of the fully graphitized cathode, a new thermal insulation material with better thermal insulation performance is used in the design of the electrolytic cell lining to increase the thermal insulation effect of the bottom and lower side of the cell, and also provide energy guarantee for the next step of the electrolytic cell to operate below the working voltage of 3.8V. The impact of the change in the lining design to increase the thermal insulation effect is that the electrolytic cell will have excessively high cell temperature, cracking of the anode carbon block, irregular formation of the furnace side and shortened cell life during abnormal periods.
[0005] Therefore, in order to at least solve some of the problems of excessively high cell temperature, cracking of anode carbon blocks, irregular formation of furnace walls and impact on cell life during abnormal periods of fully graphitized cathode electrolytic cells, it is necessary to propose an abnormal period adjustment control method for fully graphitized cathode aluminum electrolytic cells. Summary of the invention
[0006] A series of simplified concepts are introduced in the Summary of the Invention section, which will be further described in detail in the Detailed Description of the Invention section. The Summary of the Invention section of this application does not mean to attempt to define the key features and essential technical features of the claimed technical solution, nor does it mean to attempt to determine the scope of protection of the claimed technical solution.
[0007] In the first aspect, the present application proposes a method for controlling the abnormal process of a fully graphitized cathode aluminum electrolytic cell, comprising:
[0008] Obtain the current duration of the abnormal period of the fully graphitized cathode aluminum electrolytic cell;
[0009] Determine the process parameter control strategy for the time period corresponding to the duration of the abnormal period, wherein the process parameter control strategy includes voltage control strategy, electrolyte temperature control strategy, aluminum liquid level control strategy, electrolyte liquid level control strategy, molecular ratio control strategy, and anode replacement control strategy;
[0010] The production process of the above-mentioned fully graphitized cathode aluminum electrolytic cell is controlled based on the process parameter control strategy.
[0011] In a feasible implementation manner, the voltage control strategy includes:
[0012] When the current duration of the abnormal period is less than or equal to 10 days, the operating voltage is controlled to gradually decrease from 6.5V to 4V at a first daily reduction rate;
[0013] When the abnormal period lasts for more than 10 days and less than or equal to 30 days, the operating voltage is controlled to gradually decrease from 4V to 3.8V at a second daily reduction rate;
[0014] When the abnormal period lasts for more than 30 days and less than or equal to 40 days, the operating voltage is controlled to gradually decrease from 3.8V to 3.75V at a third daily reduction rate;
[0015] When the abnormal period currently lasts for more than 40 days and less than or equal to 50 days, the operating voltage is controlled to gradually decrease from 3.75 V to 3.70 V at a fourth daily reduction rate.
[0016] In a feasible implementation, the electrolyte temperature control strategy includes:
[0017] When the abnormal period lasts for less than or equal to 7 days, the electrolyte temperature is controlled between 980 degrees Celsius and 990 degrees Celsius;
[0018] When the abnormal period lasts for more than 7 days and less than or equal to 28 days, the electrolyte temperature is controlled between 970 degrees Celsius and 980 degrees Celsius;
[0019] When the abnormal period lasts for more than 28 days and less than or equal to 60 days, the electrolyte temperature is controlled between 965 degrees Celsius and 975 degrees Celsius;
[0020] When the abnormal period lasts for more than 61 days and less than or equal to 90 days, the electrolyte temperature is controlled between 955 degrees Celsius and 965 degrees Celsius;
[0021] When the abnormal period lasts for more than 91 days and less than or equal to 120 days, the electrolyte temperature is controlled between 950 degrees Celsius and 960 degrees Celsius.
[0022] In a feasible implementation manner, the above aluminum liquid level control strategy includes:
[0023] Control the initial aluminum liquid height to be between 18 cm and 20 cm. If the abnormal period lasts for less than or equal to 7 days, adjust the aluminum liquid level to between 24 cm and 26 cm, and maintain the aluminum liquid level between 24 cm and 26 cm until the abnormal period lasts for 60 days.
[0024] When the abnormal period lasts for more than 60 days, the aluminum liquid level will be adjusted to between 20 cm and 22 cm.
[0025] In a feasible implementation, the electrolyte level control strategy includes:
[0026] When the abnormal period lasts for less than or equal to 7 days, the electrolyte level is controlled to be greater than or equal to 25 cm;
[0027] When the abnormal period lasts for more than 7 days and less than or equal to 60 days, the electrolyte level is controlled to be greater than or equal to 22 cm;
[0028] When the abnormal period lasts for more than 60 days and less than or equal to 120 days, the electrolyte liquid level is controlled between 18 cm and 20 cm.
[0029] In a feasible implementation, the above molecular ratio control strategy includes:
[0030] When the current duration of the abnormal period is less than or equal to 90 days, the molecular ratio is controlled to be between 2.8 and 3;
[0031] When the abnormal period lasts for more than 90 days, the molecular ratio is set between 2.4 and 2.5.
[0032] In a feasible implementation manner, the above-mentioned anode replacement control strategy includes:
[0033] When the current duration of the abnormal period is less than or equal to 35 days, the first anode replacement strategy is adopted, wherein the first anode replacement strategy is a strategy of stopping replacement in the first part of the replacement cycle and continuously replacing a single group of electrodes every day in the latter part;
[0034] When the abnormal period lasts longer than 35 days, a second anode replacement strategy is adopted, wherein the second anode replacement strategy is a strategy of intermittently and continuously replacing a single group of electrodes at equal time periods within a replacement cycle.
[0035] In a feasible implementation, the above-mentioned fully graphitized cathode aluminum electrolysis cell includes a fully graphitized cathode aluminum electrolysis cell and a copper-inserted cathode steel rod fully graphitized cathode aluminum electrolysis cell.
[0036] In a feasible embodiment, the capacity of the above-mentioned fully graphitized cathode aluminum electrolysis cell is greater than or equal to 400kA.
[0037] In a second aspect, the present application further proposes a fully graphitized cathode aluminum electrolytic cell, comprising an electrolytic cell body and a control device, wherein the control device stores the abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to any one of the first aspect.
[0038] In summary, the abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell of the embodiment of the present application includes: obtaining the current duration of the abnormal period of the fully graphitized cathode aluminum electrolytic cell; determining the process parameter control strategy for the time period corresponding to the duration of the above-mentioned abnormal period, wherein the above-mentioned process parameter control strategy includes voltage control strategy, electrolyte temperature control strategy, aluminum liquid level control strategy, electrolyte liquid level control strategy, molecular ratio control strategy, and anode replacement control strategy; based on the process parameter control strategy, the production process of the above-mentioned fully graphitized cathode aluminum electrolytic cell is controlled. The present application implements a detailed process parameter control strategy, such as the adjustment of voltage, electrolyte temperature, liquid level and molecular ratio, and the present scheme can effectively stabilize the key variables in the production process, reduce production fluctuations, and improve production efficiency. Accurate voltage and temperature control helps to reduce energy consumption, especially by reducing the working voltage and controlling energy input or output, which can significantly reduce the energy consumption of the electrolytic cell, thereby reducing production costs. By monitoring and adjusting the replacement time of the anode and maintaining the appropriate state of the electrolyte, the anode utilization rate and the establishment of the electrolytic cell furnace can be improved, the service life of the electrolytic cell and the anode can be extended, and the maintenance and replacement costs can be reduced. This solution adopts different control strategies according to different stages of the abnormal period, showing high adaptability and flexibility, and can quickly adjust the strategy according to the specific situation to cope with various abnormal situations that may occur in the production process, making the operation of the fully graphitized cathode aluminum electrolytic cell more efficient. The method proposed in this application can make the electrolytic cell smoothly transition to the normal period, reduce the power consumption during the abnormal period, improve the stability of the electrolytic cell and extend the cell life.
[0039] The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell proposed in this application, and other advantages, objectives and features of this application will be reflected in part through the following description, and in part will be understood by technical personnel in this field through research and practice of this application. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present specification. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0041] Figure 1 A schematic flow chart of an abnormal period process control method for a fully graphitized cathode aluminum electrolytic cell provided in an embodiment of the present application;
[0042] Figure 2 A structural schematic diagram of a fully graphitized cathode aluminum electrolysis cell provided in an embodiment of the present application. DETAILED DESCRIPTION
[0043] The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.
[0044] See also Figure 1 , which is a schematic flow diagram of a method for controlling a process of an abnormal period of a fully graphitized cathode aluminum electrolytic cell provided in an embodiment of the present application, and may specifically include:
[0045] S110, obtaining the current duration of the abnormal period of the fully graphitized cathode aluminum electrolytic cell;
[0046] Exemplarily, the management time for controlling the abnormal period is 4 months, 1-3 months are the adjustment period, and the 4th month is the transition period. Different process parameter control strategies are also adopted in different time periods during the abnormal period.
[0047] S120, determining the process parameter control strategy for the time period corresponding to the duration of the abnormal period, wherein the process parameter control strategy includes a voltage control strategy, an electrolyte temperature control strategy, an aluminum liquid level control strategy, an electrolyte liquid level control strategy, a molecular ratio control strategy, and an anode replacement control strategy;
[0048] Exemplarily, the voltage control strategy is to adjust the power output according to the deviation between the actual voltage of the electrolytic cell and the standard voltage to stabilize the voltage of the electrolytic cell. The electrolyte temperature control strategy is to maintain the electrolyte temperature within the optimal range by adjusting the output of the heating or cooling system. The aluminum liquid level control strategy is to control the aluminum liquid level by adjusting the addition or extraction rate of the aluminum liquid. The electrolyte liquid level control strategy is to adjust the supply or discharge of the electrolyte to maintain a suitable liquid level. The molecular ratio control strategy is to adjust the ratio of chemical components in the electrolyte to ensure the efficiency and stability of the electrolytic reaction. The anode replacement control strategy is to determine the timing of replacing the anode based on the anode consumption and working efficiency.
[0049] S130. Control the production process of the above-mentioned fully graphitized cathode aluminum electrolytic cell based on the process parameter control strategy.
[0050] For example, the automatic control system is activated or the operator is notified to manually adjust the relevant parameters. The system monitors the effect of the adjustment in real time and ensures that each parameter reaches the preset target through a feedback loop.
[0051] In summary, this application implements a detailed process parameter control strategy, such as voltage, electrolyte temperature, liquid level and molecular ratio adjustment, and this solution can effectively stabilize the key variables in the production process, reduce production fluctuations and improve production efficiency. Accurate voltage and temperature control helps to reduce energy consumption, especially by reducing the operating voltage and controlling energy input or output, which can significantly reduce the energy consumption of the electrolytic cell, thereby reducing production costs. By monitoring and adjusting the timing of anode replacement and maintaining the appropriate state of the electrolyte, the anode utilization rate and the establishment of the electrolytic cell furnace can be improved, the service life of the electrolytic cell and the anode can be extended, and the maintenance and replacement costs can be reduced. This solution adopts different control strategies according to different stages of the abnormal period, showing a high degree of adaptability and flexibility, and can quickly adjust the strategy according to the specific situation to cope with various abnormal situations that may occur in the production process, making the operation of the fully graphitized cathode aluminum electrolytic cell more efficient. The method proposed in this application can make the electrolytic cell smoothly transition to the normal period, reduce the power consumption during the abnormal period, improve the stability of the electrolytic cell and extend the life of the cell.
[0052] In some examples, the voltage control strategy includes:
[0053] When the current duration of the abnormal period is less than or equal to 10 days, the operating voltage is controlled to gradually decrease from 6.5V to 4V at a first daily reduction rate;
[0054] When the abnormal period lasts for more than 10 days and less than or equal to 30 days, the operating voltage is controlled to gradually decrease from 4V to 3.8V at a second daily reduction rate;
[0055] When the abnormal period lasts for more than 30 days and less than or equal to 40 days, the operating voltage is controlled to gradually decrease from 3.8V to 3.75V at a third daily reduction rate;
[0056] When the abnormal period currently lasts for more than 40 days and less than or equal to 50 days, the operating voltage is controlled to gradually decrease from 3.75 V to 3.70 V at a fourth daily reduction rate.
[0057] For example, by carefully dividing the duration of the abnormal period, the solution specifies the voltage adjustment measures that should be taken in different time periods. The following is a detailed explanation and logic of each time period:
[0058] Time periods and corresponding voltage adjustment strategies:
[0059] 1. Abnormal period lasts ≤ 10 days:
[0060] The voltage is gradually reduced from the initial 6.5V to 4V. Rapid voltage reduction at the beginning of the abnormal period may be to quickly alleviate abnormal conditions in the electrolyzer, such as overheating or electrochemical instability of the electrolyzer caused by excessive voltage. The daily reduction rate needs to be set according to actual conditions to ensure that other key parameters of the electrolysis process are not affected by excessive voltage reduction.
[0061] 2. Abnormal period lasts for >10 days and ≤30 days:
[0062] The voltage is gradually reduced from 4V to 3.8V. The voltage reduction is relatively slow in this stage because the state of the cell has been partially stabilized. The voltage needs to be carefully adjusted to further optimize the operating conditions to avoid too low voltage affecting the production efficiency of aluminum. The daily reduction rate in the second stage is slower than that in the first stage, and more attention is paid to fine-tuning to ensure a balance between production efficiency and safety. The daily reduction rate in the second stage can be 10mV per day.
[0063] 3. Abnormal period lasts for >30 days and ≤40 days:
[0064] The voltage is adjusted to gradually decrease from 3.8V to 3.75V. After the abnormal period enters the middle stage, the voltage is further fine-tuned to a lower stable level, aiming to refine the control to adapt to the possible new equilibrium state of the electrolyzer. The daily reduction rate in the third stage is very slight, which indicates that the state of the electrolyzer is close to normal operating conditions and the adjustments required are more subtle to avoid excessive adjustments interfering with the production process that has already stabilized. The third daily reduction rate can be 5mV per day
[0065] 4. Abnormal period lasts for >40 days and ≤50 days:
[0066] The voltage is gradually reduced from 3.75V to 3.70V. In the final stage of the abnormal period, the voltage is further reduced, probably to fine-tune and fully restore the optimal operating state of the electrolyzer. The reduction rate at this stage may be slightly slowed down again to ensure a smooth transition and avoid triggering a new abnormal state due to too rapid adjustment.
[0067] By adjusting the voltage in stages, the solution aims to respond to abnormal operating conditions of fully graphitized cathode aluminum electrolytic cells at different stages. The voltage adjustment at each stage is based on a comprehensive assessment of the current state of the electrolytic cell, including the stability of its electrochemical reaction, the aluminum production efficiency, and the safe operation of the equipment. The gradual reduction of voltage helps to alleviate electrolysis imbalances caused by excessive voltage, such as overheating, material degradation, or abnormal chemical reaction rates. At the same time, fine-tuning the voltage can also help operators better understand the operating characteristics of the electrolytic cell, optimize the production process, and improve product quality and energy efficiency.
[0068] In some examples, the electrolyte temperature control strategy described above includes:
[0069] When the abnormal period lasts for less than or equal to 7 days, the electrolyte temperature is controlled between 980 degrees Celsius and 990 degrees Celsius;
[0070] When the abnormal period lasts for more than 7 days and less than or equal to 28 days, the electrolyte temperature is controlled between 970 degrees Celsius and 980 degrees Celsius;
[0071] When the abnormal period lasts for more than 28 days and less than or equal to 60 days, the electrolyte temperature is controlled between 965 degrees Celsius and 975 degrees Celsius;
[0072] When the abnormal period lasts for more than 61 days and less than or equal to 90 days, the electrolyte temperature is controlled between 955 degrees Celsius and 965 degrees Celsius;
[0073] When the abnormal period lasts for more than 91 days and less than or equal to 120 days, the electrolyte temperature is controlled between 950 degrees Celsius and 960 degrees Celsius.
[0074] Exemplarily, when the abnormal period lasts ≤ 7 days, the temperature range is 980° C. to 990° C. In the initial stage of the abnormal period, the electrolyte temperature is kept relatively high to quickly stabilize the reaction conditions of the electrolyzer and restore normal operation as soon as possible.
[0075] When the abnormal period lasts for >7 days and ≤28 days, the temperature range is 970°C to 980°C. As the abnormal state continues, the electrolyte temperature is gradually reduced to reduce energy consumption and reduce excessive electrolyte consumption or equipment damage that may be caused by excessive temperature.
[0076] When the abnormal period lasts for >28 days and ≤60 days, the temperature range is 965°C to 975°C. After a longer period of abnormal operation, the temperature is further reduced to optimize the electrolysis efficiency, reduce unnecessary energy consumption, and prevent the instability of the aluminum electrolyte due to high temperature.
[0077] When the abnormal period lasts for more than 61 days and ≤ 90 days, the temperature range is 955°C to 965°C. During longer abnormal periods, the temperature will continue to be lowered to seek the best energy efficiency ratio and material protection to prevent potential damage to the equipment caused by long-term high temperature.
[0078] When the abnormal period lasts for more than 91 days and less than 120 days, the temperature range is 950°C to 960°C. When the abnormal period is nearing the end, the temperature is adjusted to a lower stable level to ensure the continuous stability of the electrolysis process and make final preparations for resuming normal operation.
[0079] By adjusting the electrolyte temperature in stages, this solution aims to precisely control the thermal conditions during the electrolysis process, thereby optimizing electrolysis efficiency and quality control. The temperature adjustment at each stage is based on the characteristics and requirements of the current abnormal operating state to ensure the stability and efficiency of the electrolysis process under various challenges. This strategy, through systematic temperature management, not only helps to maintain the stable operation of the electrolytic cell during abnormal periods, but also provides support for the eventual restoration of normal operating conditions, ensuring the continuity and economic benefits of the entire aluminum electrolysis process.
[0080] In some examples, the above aluminum liquid level control strategy includes:
[0081] Control the initial aluminum liquid height to be between 18 cm and 20 cm. If the abnormal period lasts for less than or equal to 7 days, adjust the aluminum liquid level to between 24 cm and 26 cm, and maintain the aluminum liquid level between 24 cm and 26 cm until the abnormal period lasts for 60 days.
[0082] When the abnormal period lasts for more than 60 days, the aluminum liquid level will be adjusted to between 20 cm and 22 cm.
[0083] Exemplarily, the initial setting liquid level height range is: 18 cm to 20 cm. A standard initial liquid level height is set to ensure the stability and efficiency of the electrolyzer under normal operating conditions.
[0084] When the abnormal period lasts ≤ 60 days, adjust the aluminum liquid level to between 24 cm and 26 cm. In the early stage of the abnormal period, raising the aluminum liquid level can help deal with possible current instability or thermal runaway problems. A higher liquid level can provide a larger aluminum reserve, increase heat absorption and dispersion, and thus stabilize the electrolysis process. Maintain this height until the abnormal period lasts 60 days. During this period, the higher liquid level helps reduce the pressure inside the electrolytic cell and provides a buffer for the system to return to normal operation.
[0085] When the abnormal period lasts for more than 60 days, adjust the aluminum liquid level to between 20 cm and 22 cm. After the abnormal period lasts for more than 60 days, if the tank state begins to stabilize, gradually lowering the liquid level will help restore to more economical operating conditions and reduce energy and material consumption. A lower liquid level can improve operating efficiency after the electrolytic cell stabilizes, while reducing potential risks caused by excessive liquid levels, such as electrolyte overflow.
[0086] Through this staged aluminum liquid level control, the electrolysis conditions can be optimized according to the specific needs and responses of the electrolytic cell during abnormal operation. This method makes the adjustment of the aluminum liquid level more targeted and timely, and effectively supports the management and recovery of the electrolytic cell in unstable or abnormal conditions. It helps to protect equipment and maintain the stability of the production process, and also helps to improve overall production efficiency and product quality. Through precise control of the aluminum liquid level, the electrolytic cell can be restored to the best working condition as soon as possible while ensuring safety.
[0087] In some examples, the electrolyte level control strategy includes:
[0088] When the abnormal period lasts for less than or equal to 7 days, the electrolyte level is controlled to be greater than or equal to 25 cm;
[0089] When the abnormal period lasts for more than 7 days and less than or equal to 60 days, the electrolyte level is controlled to be greater than or equal to 22 cm;
[0090] When the abnormal period lasts for more than 60 days and less than or equal to 120 days, the electrolyte liquid level is controlled between 18 cm and 20 cm.
[0091] For example, proper control of the electrolyte level is crucial to maintaining the stability of the electrolysis process because it affects the current distribution, uniformity of the chemical reaction, and thermal management. The following is a detailed strategy explanation and logic:
[0092] When the abnormal period lasts ≤7 days, maintain the electrolyte level greater than or equal to 25 cm. In the initial stage of the abnormal period, the electrolyzer may face unstable electrochemical reactions or heat management problems. A higher electrolyte level helps to enhance the thermal capacity and electrochemical reaction area of the electrolyzer, thereby providing sufficient buffer to stabilize the tank's conditions.
[0093] When the abnormal period lasts for >7 days and ≤60 days, keep the electrolyte level greater than or equal to 22 cm. At this stage, as the abnormal situation continues, it may be necessary to gradually adjust the liquid level to optimize electrolysis efficiency and reduce energy consumption. By appropriately lowering the liquid level, electrolyte consumption and heat loss can be reduced while maintaining a sufficient liquid level to avoid instability during the electrolysis process.
[0094] When the abnormal period lasts for >60 days and ≤120 days, the electrolyte level is adjusted between 18 cm and 20 cm. After the abnormal period lasts for a long time, further reducing the liquid level will help gradually restore the electrolyzer to conditions closer to normal operation. The liquid level adjustment at this stage is intended to optimize the electrolysis efficiency while ensuring that there are no potential risks caused by excessive liquid level inside the electrolyzer, such as electrolyte overflow or reduced electrolysis efficiency.
[0095] By adjusting the electrolyte level in stages, this strategy aims to precisely control key variables in the electrolysis process to optimize the operating efficiency and product quality of the electrolyzer, while preventing or reducing problems that may occur under abnormal operating conditions. By adjusting the liquid level, current efficiency can be improved and energy consumption can be reduced. The appropriate liquid level helps prevent overflow or short circuit events during the electrolysis process. Avoid premature wear or damage to equipment caused by inappropriate liquid level. Ensure that the electrolyte level is at the optimal height to maintain stable chemical reactions during the electrolysis process.
[0096] In some examples, the above molecular ratio control strategy includes:
[0097] When the current duration of the abnormal period is less than or equal to 90 days, the molecular ratio is controlled to be between 2.8 and 3;
[0098] When the abnormal period lasts for more than 90 days, the molecular ratio is controlled between 2.4 and 2.5.
[0099] Illustratively, the molecular ratio, i.e., the ratio of sodium fluoride (NaF) to aluminum fluoride (AlF3), is a key parameter in the aluminum electrolysis process, which directly affects the electrochemical properties of the electrolyte, the operating temperature of the electrolytic cell, and the electrolysis efficiency.
[0100] When the abnormal period lasts ≤90 days, the molecular ratio is controlled in the range of 2.8 to 3.0. In the early to middle stage of the abnormal period, maintaining a higher molecular ratio helps to increase the sodium fluoride content in the electrolyte, thereby increasing the conductivity of the electrolytic cell and maintaining a high electrolysis temperature. A higher molecular ratio helps to reduce the heat load inside the electrolytic cell, thereby reducing energy consumption and extending equipment life.
[0101] In the case of abnormal periods lasting > 90 days, the molecular ratio is controlled in the range of 2.4 to 2.5. When the abnormal period lasts for a long time, gradually reducing the molecular ratio helps to adjust the chemical balance of the electrolyte and restore conditions more suitable for normal aluminum production. At this time, it may be necessary to reduce the proportion of sodium fluoride and increase the content of aluminum fluoride to improve the electrolysis efficiency and optimize the quality of aluminum. A lower molecular ratio helps to improve the stability and electrolysis efficiency of the electrolysis process, especially when the chemical environment and physical state of the electrolytic cell have partially returned to normal.
[0102] Proper adjustment of the molecular ratio is an important means of controlling the electrolyte composition in electrolytic aluminum production. By adjusting the molecular ratio at different stages, various problems that arise during abnormal operation, such as thermal management problems inside the electrolytic cell, low electrolysis efficiency, or product quality problems, can be effectively dealt with. Flexibly adjusting the molecular ratio according to the actual operating status of the electrolytic cell helps to quickly respond to various challenges that arise in production. By controlling the molecular ratio, the energy consumption of the electrolytic process can be optimized and production costs can be reduced. The appropriate molecular ratio helps to improve the purity and consistency of the final product aluminum. The appropriate molecular ratio can reduce the operating temperature of the electrolytic cell, reduce equipment wear and corrosion, and extend the service life of the equipment.
[0103] In some examples, the anode replacement control strategy includes:
[0104] When the current duration of the abnormal period is less than or equal to 35 days, the first anode replacement strategy is adopted, wherein the first anode replacement strategy is a strategy of stopping replacement in the first part of the replacement cycle and continuously replacing a single group of electrodes every day in the latter part;
[0105] When the abnormal period lasts longer than 35 days, a second anode replacement strategy is adopted, wherein the second anode replacement strategy is a strategy of intermittently and continuously replacing a single group of electrodes at equal time periods within a replacement cycle.
[0106] Exemplarily, when the current duration of the above-mentioned abnormal period is less than or equal to 35 days, the first anode replacement strategy is adopted, and when the current duration of the above-mentioned abnormal period is greater than 35 days, the second anode replacement strategy is adopted. For example, the replacement cycle is 35 days, and the entire electrolytic cell includes a total of 28 groups of electrodes numbered 1, 2...28. When the first anode replacement strategy is adopted, the electrodes are not replaced in the first 1-7 days, and the 28 groups of electrodes are replaced in sequence from 8 to 35 days. When the second anode replacement strategy is adopted, taking 36-70 days as an example, it is divided into 28 equal time periods, and a group of electrode replacement operations are performed at the end of each equal time period.
[0107] Not replacing anodes during the initial abnormal period (first 1-7 days) allows the cell to stabilize without being disturbed by anode replacement operations. This helps avoid introducing additional variables during the most unstable period of the cell, thereby reducing potential risks and problems. Continuously replacing all anode groups (one group per day) from 8 to 35 days ensures that all anodes are in optimal working condition. This strategy helps maintain the efficiency and stability of the cell, especially during abnormal normal operating conditions, as the new anodes can provide more uniform current distribution and better chemical reaction conditions.
[0108] In some examples, the above-mentioned fully graphitized cathode aluminum electrolysis cell includes a fully graphitized cathode aluminum electrolysis cell and a fully graphitized cathode aluminum electrolysis cell with a copper-inserted cathode steel rod.
[0109] In some examples, the capacity of the fully graphitized cathode aluminum electrolysis cell is greater than or equal to 400 kA.
[0110] For example,
[0111] Example 1
[0112] 500kA fully graphitized electrolytic cell, after startup, is operated and managed according to the abnormal period adjustment method of fully graphitized cathode aluminum electrolytic cell. The set voltage is reduced to 3.73V on the 52nd day; aluminum is poured to 20cm after startup, and it is adjusted to 24cm on the 5th day and maintained. The aluminum output begins to increase on the 61st day, and the aluminum level is adjusted to 22cm on the 65th day and maintained; molecular ratio: 2.8-3.0 in the first to third months; in the fourth month, aluminum fluoride is added quantitatively to adjust the molecular ratio to 2.4-2.5; the electrolyte temperature is 983℃ on the 7th day, reaching 961℃ on the 65th day; and the normal temperature of 956℃ is reached on the 100th day. The first anode replacement time starts from the 9th day after startup, and then one group is replaced every day. On the 125th day, the furnace internal shape test of the tank is carried out, and the average furnace wall thickness is 17cm, the leg length is 7cm, and the leg height is 6cm. This method prolongs the management time during the abnormal period, quickly lowers the set voltage, reduces the power consumption during the abnormal period, lowers the initial electrolysis temperature during the abnormal period, forms a furnace shape that is conducive to long life, and achieves the effect of extending the life of the tank.
[0113] Example 2
[0114] 400kA fully graphitized electrolytic cell, after startup, is operated and managed according to the abnormal period adjustment method of fully graphitized cathode aluminum electrolytic cell. The set voltage is reduced to 3.74V on the 56th day; after startup, aluminum is poured to 19cm, adjusted to 23cm on the 5th day and maintained, and the aluminum output is increased on the 61st day, and the aluminum level is adjusted to 21cm on the 65th day and maintained; molecular ratio: 2.8-3.0 in the first three months; in the fourth month, aluminum fluoride is added quantitatively to adjust the molecular ratio to 2.4-2.5; the electrolyte temperature is 981℃ on the 7th day, reaching 960℃ on the 65th day; and the normal temperature of 954℃ is reached on the 100th day. The first anode replacement time is from the 7th day after startup, and then one group is replaced every day. On the 122nd day, the furnace internal shape test of the tank was carried out, and the average furnace wall thickness was 16cm, the leg length was 8cm, and the leg height was 6cm. This method prolongs the management time during the abnormal period, quickly lowers the set voltage, reduces the power consumption during the abnormal period, lowers the initial electrolysis temperature during the abnormal period, forms a furnace shape that is conducive to long life, and achieves the effect of extending the life of the tank.
[0115] Example 3
[0116] 500kA fully graphitized cathode copper electrolytic cell, after startup, operation and management are carried out according to the abnormal period adjustment method of fully graphitized cathode aluminum electrolytic cell. The set voltage is reduced to 3.72V on the 48th day; aluminum is poured to 21cm after startup, and it is adjusted to 25cm on the 5th day and maintained. The aluminum output begins to increase on the 61st day, and the aluminum level is adjusted to 22cm on the 65th day and maintained; molecular ratio: 2.8-3.0 in the first three months; in the fourth month, aluminum fluoride is added quantitatively to adjust the molecular ratio to 2.45-2.55; the electrolyte temperature is 986℃ on the 7th day, reaching 966℃ on the 65th day; and the normal temperature of 956℃ is reached on the 100th day. The first anode replacement time starts from the 9th day after startup, and then one group is replaced every day. On the 123rd day, the furnace internal shape test of the tank is carried out, and the average furnace wall thickness is 18cm, the leg length is 9cm, and the leg height is 5cm. This method prolongs the management time during the abnormal period, quickly lowers the set voltage, reduces the power consumption during the abnormal period, lowers the initial electrolysis temperature during the abnormal period, forms a furnace shape that is conducive to long life, and achieves the effect of extending the life of the tank.
[0117] Comparative Example 1
[0118] The same tank capacity as in Example 1 is used, the cathode carbon block is 50% graphite, and the abnormal period is 4 months. The set voltage is reduced to 3.84V on the 65th day; aluminum is poured to 18cm after startup, adjusted to 22cm on the 10th day, and adjusted to 26cm on the 60th day and then maintained; molecular ratio: 2.8-3.0 in the 1st to 3rd month; in the 4th month, aluminum fluoride is added quantitatively to adjust the molecular ratio to 2.4-2.5; the electrolyte temperature is 986℃ on the 7th day, 968℃ on the 65th day; and reaches the normal temperature of 959℃ on the 100th day. The first anode replacement time is from the 3rd day after startup. On the 125th day, the furnace internal shape test of the tank is carried out, and the average furnace wall thickness is 13cm, the leg length is 11cm, and the leg height is 7cm.
[0119] Comparative Example 2
[0120] The same tank capacity as in Example 2 is used, the cathode carbon block is 50% graphite, and the abnormal period is 4 months. The set voltage is reduced to 3.86V on the 65th day; aluminum is poured to 18cm after startup, adjusted to 23cm on the 10th day, and adjusted to 25cm on the 60th day and then maintained; molecular ratio: 2.8-3.0 in the 1st to 3rd month; in the 4th month, aluminum fluoride is added quantitatively to adjust the molecular ratio to 2.45-2.55; the electrolyte temperature is 984℃ on the 7th day, reaching 966℃ on the 65th day; and reaching the normal temperature of 956℃ on the 100th day. The first anode replacement time is from the 3rd day after startup. On the 125th day, the furnace internal shape test of the tank is carried out, and the average furnace wall thickness is 14cm, the leg length is 12cm, and the leg height is 8cm.
[0121]
[0122] Table 1
[0123] It can be seen from the data in Table 1 that the abnormal period adjustment method of the fully graphitized cathode aluminum electrolytic cell provided in Examples 1 to 3 of the present invention can adjust the set voltage to 3.72-3.74V, the furnace wall thickness can reach more than 15cm, and the leg length and height are within a controllable range, which is a feature of the long life of the electrolytic cell.
[0124] Comparative Examples 1 and 2 were managed according to the traditional abnormal period management method, with the voltage set to 3.84-3.86V, the furnace wall thickness below 15cm, and the leg length and height being too large, which was a cold tank trend and was not conducive to the stability of the electrolytic cell.
[0125] Second, Figure 2 As shown, the present application also proposes a fully graphitized cathode aluminum electrolytic cell 10, comprising an electrolytic cell body 101 and a control device 102, wherein the above-mentioned control device stores the abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to any one of the first aspect.
[0126] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for controlling the abnormal process of a fully graphitized cathode aluminum electrolytic cell. It is characterized in that include: Obtain the current duration of the abnormal period of the fully graphitized cathode aluminum electrolytic cell; Determine the process parameter control strategy for the time period corresponding to the duration of the abnormal period, wherein the process parameter control strategy includes voltage control strategy, electrolyte temperature control strategy, aluminum liquid level control strategy, electrolyte liquid level control strategy, molecular ratio control strategy, and anode replacement control strategy; The production process of the fully graphitized cathode aluminum electrolytic cell is controlled based on a process parameter control strategy.
2. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The voltage control strategy includes: When the current duration of the abnormal period is less than or equal to 10 days, controlling the operating voltage to gradually decrease from 6.5V to 4V at a first daily reduction rate; When the abnormal period lasts for more than 10 days and less than or equal to 30 days, controlling the operating voltage to gradually decrease from 4V to 3.8V at a second daily reduction rate; When the current duration of the abnormal period is greater than 30 days and less than or equal to 40 days, controlling the operating voltage to gradually decrease from 3.8 V to 3.75 V at a third daily reduction rate; When the current duration of the abnormal period is greater than 40 days and less than or equal to 50 days, the operating voltage is controlled to gradually decrease from 3.75 V to 3.70 V at a fourth daily reduction rate.
3. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The electrolyte temperature control strategy includes: When the current duration of the abnormal period is less than or equal to 7 days, controlling the electrolyte temperature to be between 980 degrees Celsius and 990 degrees Celsius; When the abnormal period lasts for more than 7 days and less than or equal to 28 days, controlling the electrolyte temperature to be between 970 degrees Celsius and 980 degrees Celsius; When the abnormal period lasts for more than 28 days and less than or equal to 60 days, controlling the electrolyte temperature to be between 965 degrees Celsius and 975 degrees Celsius; When the abnormal period lasts for more than 61 days and less than or equal to 90 days, controlling the electrolyte temperature to be between 955 degrees Celsius and 965 degrees Celsius; When the abnormal period currently lasts for more than 91 days and less than or equal to 120 days, the electrolyte temperature is controlled between 950 degrees Celsius and 960 degrees Celsius.
4. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The aluminum liquid level control strategy includes: Controlling the initial aluminum liquid height to be between 18 cm and 20 cm, and when the current duration of the abnormal period is less than or equal to 7 days, adjusting the aluminum liquid level to between 24 cm and 26 cm, and maintaining the aluminum liquid level between 24 cm and 26 cm until the current duration of the abnormal period is 60 days; When the abnormal period lasts for more than 60 days, the aluminum liquid level is adjusted to between 20 cm and 22 cm.
5. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The electrolyte liquid level control strategy includes: When the current duration of the abnormal period is less than or equal to 7 days, the electrolyte liquid level is controlled to be greater than or equal to 25 cm; When the abnormal period lasts for more than 7 days and less than or equal to 60 days, the electrolyte level is controlled to be greater than or equal to 22 cm; When the abnormal period currently lasts for more than 60 days and less than or equal to 120 days, the electrolyte liquid level is controlled to be between 18 cm and 20 cm.
6. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The molecular ratio control strategy includes: When the current duration of the abnormal period is less than or equal to 90 days, controlling the molecular ratio to be between 2.8 and 3; When the abnormal period currently lasts for more than 90 days, the molecular ratio is set between 2.4 and 2.
5.
7. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The anode replacement control strategy includes: When the current duration of the abnormal period is less than or equal to 35 days, a first anode replacement strategy is adopted, wherein the first anode replacement strategy is a strategy of stopping replacement in the first part of the replacement cycle and continuously replacing a single group of electrodes every day in the latter part; When the abnormal period currently lasts longer than 35 days, a second anode replacement strategy is adopted, wherein the second anode replacement strategy is a strategy of intermittently and continuously replacing a single group of electrodes at equal time periods within a replacement cycle.
8. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The fully graphitized cathode aluminum electrolytic cell includes a fully graphitized cathode aluminum electrolytic cell and a copper-inserted cathode steel rod fully graphitized cathode aluminum electrolytic cell.
9. The abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to claim 1, It is characterized in that The capacity of the fully graphitized cathode aluminum electrolytic cell is greater than or equal to 400 kA.
10. A fully graphitized cathode aluminum electrolytic cell, comprising an electrolytic cell body and a control device, in, The control device stores the abnormal period process control method of the fully graphitized cathode aluminum electrolytic cell according to any one of claims 1 to 9.
Citation Information
Cited By
A production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell
CN123108663A