Method for preparing cuprous oxide loaded polytetrafluoroethylene nanofiber membrane through in-situ reduction

The preparation of cuprous oxide-loaded polytetrafluoroethylene nanofiber membranes through in-situ reduction solves the problem of limited antibacterial and antiviral performance of polytetrafluoroethylene nanofiber membranes, achieves efficient antibacterial and antiviral effects and reduces production costs. Suitable for personal protection and air purification fields.

CN118727434AInactive Publication Date: 2024-10-01DONGHUA UNIV

Patent Information

Application Number
CN202410714059.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polytetrafluoroethylene nanofiber membrane has limited antibacterial and antiviral performance. The modification method is costly and ineffective. The probability of exposure of antibacterial and antiviral agents is small, making it difficult to fully exert its performance.

Method used

A method of in-situ reduction is used to prepare cuprous oxide-loaded polytetrafluoroethylene nanofiber membranes. Copper sulfate solution is sprayed and reacted in an alkaline environment to generate copper hydroxide. Ascorbic acid is then used as a reducing agent to form a stable cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane. , ensuring that it is exposed and fully exerts its antibacterial and antiviral properties.

Benefits of technology

The high-efficiency antibacterial and antiviral properties of the polytetrafluoroethylene nanofiber membrane are achieved, the production cost is reduced, it is suitable for large-scale production, and has broad application prospects in the fields of personal protective equipment and air purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727434A_ABST
    Figure CN118727434A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a cuprous oxide loaded polytetrafluoroethylene nanofiber membrane through in-situ reduction, which comprises the following steps: uniformly spraying a prepared copper sulfate solution on the surface of a polytetrafluoroethylene nanofiber membrane, and drying to obtain a copper sulfate seed crystal loaded polytetrafluoroethylene nanofiber membrane, and further reducing the copper sulfate seed crystal into cuprous oxide in situ by using a reducing agent solution, and finally obtaining the cuprous oxide loaded polytetrafluoroethylene nanofiber membrane through heat setting. The cuprous oxide loaded polytetrafluoroethylene nanofiber membrane has an excellent antiviral effect and can be applied to the fields of personal protection articles, air purification and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and particularly relates to a method for preparing a cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane by in-situ reduction. Background Art

[0002] Public safety and health issues caused by various pathogenic bacteria and viruses have become a frontier issue of global concern. They are mainly transmitted through media such as dust, droplets and bioaerosols. Therefore, anti-epidemic products highlight their important role. Whether it is anti-epidemic products such as masks or protective clothing, as the first line of defense against infection, they mainly block aerosols containing viruses and directly contact carriers containing viruses. However, anti-epidemic products only passively block viruses, not actively inactivate pathogenic bacteria and viruses, which exposes the problem that the surface of anti-epidemic products is contaminated with viruses, which can easily cause human infection and large-scale use pollutes the environment. Therefore, developing a class of anti-epidemic products with antibacterial and antiviral functions is an important means and effective way to resist pathogenic bacteria and viruses.

[0003] Polytetrafluoroethylene nanofiber membrane is a microporous film produced by premixing, extrusion, calendering, three-dimensional asynchronous stretching and other processes using polytetrafluoroethylene dispersed resin. It has excellent chemical stability, thermal stability and electrical insulation. At the same time, its unique "node" structure is conducive to the interweaving of fibers into a mesh structure, giving it excellent waterproofness, moisture permeability and charge storage stability. It has broad application prospects in clothing, air filtration and air purification. However, due to the extremely low surface energy of polytetrafluoroethylene, the surface of polytetrafluoroethylene nanofiber membrane is extremely inert and has poor bonding with other materials. It can only play a physical interception role, but cannot remove viruses and bacteria carried in particles.

[0004] In order to give polytetrafluoroethylene nanofiber membranes antibacterial and antiviral effects, the development of new functional polytetrafluoroethylene materials has become the current direction of material development. The commonly used polytetrafluoroethylene nanofiber membrane modification methods are mainly surface modification, such as irradiation, grafting, filling and chemical corrosion, which effectively improve the surface binding force between polytetrafluoroethylene nanofiber membranes and antibacterial and antiviral agents, but these modification methods have high production costs and have great limitations; another modification method is filling modification, mixing antibacterial and antiviral agents with polytetrafluoroethylene nanofiber membranes. Since the antibacterial and antiviral agents are inside the fibers, the probability of exposure is small, making it difficult to fully exert the antibacterial and antiviral properties. Therefore, it is of great significance to develop a simple polytetrafluoroethylene nanofiber membrane with antibacterial and antiviral properties. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane by in-situ reduction. The nanofiber membrane has excellent antiviral effect and can be applied to the fields of personal protective equipment and air purification.

[0006] The present invention provides a method for preparing a cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane by in-situ reduction, comprising the following steps:

[0007] (1) Weighing copper sulfate and dissolving it in a solvent, stirring to obtain a copper sulfate solution; spraying the copper sulfate solution evenly on the surface of the polytetrafluoroethylene nanofiber membrane, and drying to obtain the copper sulfate-loaded polytetrafluoroethylene nanofiber membrane;

[0008] (2) The copper sulfate-loaded polytetrafluoroethylene nanofiber membrane obtained in step (1) is immersed in an alkaline solution, and the copper sulfate crystals react in situ to generate copper hydroxide under an alkaline environment; a reducing agent solution is then added to react fully, and after vacuum heat setting, the in-situ reduction is obtained to prepare the cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane.

[0009] Preferably, the solvent in step (1) is a mixed solvent of ethanol and water, and the volume proportion of water is 25% to 100%.

[0010] Preferably, the molar concentration of the copper sulfate solution in step (1) is 0.05 mol / L to 0.2 mol / L.

[0011] Preferably, the spraying amount of the copper sulfate solution in step (1) is 0.001 g / cm 2 -0.1g / cm 2 .

[0012] Preferably, the drying temperature in step (1) is 75° C. to 125° C., and the drying time is 2 min to 20 min.

[0013] Preferably, the alkali solution in step (2) is a sodium hydroxide solution with a molar concentration of 0.1 mol / L to 2.0 mol / L.

[0014] Preferably, the reducing agent solution in step (2) is an ascorbic acid solution with a molar concentration of 0.1 mol / L to 2.0 mol / L.

[0015] Preferably, the vacuum heat setting temperature in step (2) is 75° C. to 200° C., and the heat setting time is 5 min to 120 min.

[0016] Preferably, the cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane obtained in step (2) is used in the fields of personal protection and air filtration.

[0017] By adopting the above technical scheme, the copper sulfate crystals evenly dispersed on the surface of the polytetrafluoroethylene nanofiber membrane react in an alkaline environment to generate copper hydroxide, which is reduced to cuprous oxide using ascorbic acid as a reducing agent. After the reaction, deionized water is used to wash away the residual sodium hydroxide and incompletely reacted precursors on the surface of the polytetrafluoroethylene nanofiber membrane. In a high-temperature vacuum environment, the cuprous oxide on the surface of the polytetrafluoroethylene nanofiber membrane is not easily oxidized, and is kept warm for a period of time under a certain stress, which is beneficial to ensure the stability of the pores of the polytetrafluoroethylene nanofiber membrane.

[0018] By adopting the above technical scheme, on the one hand, copper sulfate can be uniformly attached to the surface of the polytetrafluoroethylene nanofiber membrane by using the spraying technology, thereby reducing the occurrence of copper sulfate crystal agglomeration; on the other hand, after the drying process, the ethanol / water mixed solvent on the surface of the polytetrafluoroethylene nanofiber membrane evaporates, and copper sulfate crystals are precipitated and loaded on the fibers or nodes of the polytetrafluoroethylene nanofiber membrane, which is beneficial to the subsequent in-situ reduction to generate cuprous oxide.

[0019] By adopting the above technical scheme, the copper sulfate crystals loaded on the polytetrafluoroethylene nanofiber membrane fibers first react with the sodium hydroxide solution in situ, and then are reduced by ascorbic acid to generate cuprous oxide, so that the cuprous oxide is stably loaded on the polytetrafluoroethylene nanofiber membrane fibers or nodes to the maximum extent, which not only avoids the occurrence of cuprous oxide falling off, but also ensures that the cuprous oxide is exposed, so that the antibacterial and antiviral properties can be fully exerted.

[0020] By adopting the above technical scheme, the polytetrafluoroethylene nanofiber membrane has a unique "node" structure and is interwoven to form a mesh structure. Fibers of different fineness and irregular and disorderly arrangement can effectively regulate the distance between fibers, thereby achieving the adjustment of fiber filling density. At the same time, the pore size formed between the fibers is smaller than the diameter of water droplets, much larger than the diameter of water vapor molecules, and has a high porosity, so it has excellent particle capture ability, low filtration resistance and good waterproof and moisture permeability, and has broad application prospects in the field of air purification.

[0021] By adopting the above technical solution, the molar concentration of the copper sulfate solution affects the particle size of cuprous oxide on the surface of the polytetrafluoroethylene nanofiber membrane, and the particle size affects the specific surface area of ​​direct contact between cuprous oxide and bacteria and viruses. Generally speaking, the larger the contact area, the higher the inactivation rate, and vice versa.

[0022] By adopting the above technical scheme, the molar concentration of the copper sulfate solution affects the cuprous oxide loading on the surface of the polytetrafluoroethylene nanofiber membrane. Utilizing the known antibacterial and antiviral mechanism, it is known that cuprous oxide can only achieve effective antibacterial and antiviral effects when it is in direct contact with bacteria and viruses or exposed to the air, and the amount and distribution of cuprous oxide will affect its effect.

[0023] The adoption of the above technical scheme is conducive to the infiltration of the polytetrafluoroethylene nanofiber membrane. Since the polytetrafluoroethylene nanofiber membrane has strong hydrophobicity and copper sulfate is a water-soluble crystal, ethanol can infiltrate the pores of the polytetrafluoroethylene nanofiber membrane on the basis of dissolving the copper sulfate crystals, thereby achieving the copper sulfate solution loading on the polytetrafluoroethylene nanofiber membrane fibers.

[0024] By adopting the above technical solution, water on the surface of the polytetrafluoroethylene nanofiber membrane and ethanol inside the polytetrafluoroethylene nanofiber membrane gradually evaporate from the surface and inside of the polytetrafluoroethylene nanofiber membrane during the drying process, and copper sulfate crystals are precipitated from the ethanol / water mixed solvent, thereby being loaded on the polytetrafluoroethylene nanofiber membrane fibers.

[0025] By adopting the above technical solution, OH - Concentration relative to Cu 2+ The concentration is excessive, as OH - As the concentration increases, the morphology of cuprous oxide crystals gradually changes from cubes to octahedrons. The

[100] crystal face of cuprous oxide is composed of saturated O atoms, while the

[111] crystal face contains unsaturated Cu atoms, which have higher surface energy and are positively charged, so OH - It tends to adsorb on the

[111] crystal plane, making the surface energy of the

[111] crystal plane lower than that of the

[100] crystal plane, thereby increasing the surface area of ​​the

[111] crystal plane, having higher activity, and at the same time having higher antibacterial and antiviral properties.

[0026] By adopting the above technical solution, copper sulfate crystals react in an alkaline environment to generate copper hydroxide, OH - Excessive concentration will cause copper hydroxide to dissolve to form [Cu(OH)4] 2- , and then reduced by ascorbic acid to generate cuprous oxide, and the amount of ascorbic acid added becomes the main factor in the reduction process. Insufficient reducing agent will lead to insufficient reduction reaction and further affect the antibacterial and antiviral effects.

[0027] By adopting the above technical scheme, a simple and highly operable method for cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane is provided, and the in-situ reduced and exposed cuprous oxide gives the polytetrafluoroethylene nanofiber membrane antibacterial and antiviral effects. Therefore, the cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane of the present invention can be used in the field of personal protective equipment, such as medical surgical masks, protective clothing, or in the field of air purification, such as air purifiers.

[0028] Beneficial Effects

[0029] (1) The present invention uses a copper sulfate solution to spray the polytetrafluoroethylene nanofiber membrane, which reduces the agglomeration of inorganic crystals and is more conducive to the uniform dispersion of subsequent in-situ reduction of cuprous oxide. The copper sulfate crystals are loaded on the fibers of the polytetrafluoroethylene nanofiber membrane by high-temperature drying, which improves the adhesion of cuprous oxide in the polytetrafluoroethylene nanofiber membrane and further ensures the exposure of cuprous oxide. At the same time, the present invention does not use corrosive reagents and complex equipment to modify the surface of the polytetrafluoroethylene nanofiber membrane, so it is safer and suitable for large-scale production.

[0030] (2) Since the polytetrafluoroethylene nanofiber membrane is not chemically treated in the present invention, the influence on the performance of the polytetrafluoroethylene nanofiber membrane itself is reduced, and the operability is strong and the cost is low.

[0031] (3) The cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane prepared by the present invention has high antibacterial and antiviral properties, and the binding force between the cuprous oxide and the polytetrafluoroethylene nanofiber membrane will not decrease after multiple washings. It is recyclable and can be applied to personal protective equipment, air purification and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 (i) is an electron microscope image of the polytetrafluoroethylene nanofiber membrane of Example 1; (ii) is a corresponding partial enlarged image;

[0033] Figure 2 (i) is an electron microscope image of the in-situ reduction-prepared cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane obtained in Example 1; (ii) is a corresponding partial enlarged image;

[0034] Figure 3 This is a photo of the Escherichia coli colony prepared by in-situ reduction of cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane in Example 1;

[0035] Figure 4 This is a photo of the colony of Staphylococcus aureus prepared by in-situ reduction of cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane in Example 1;

[0036] Figure 5 This is the antibacterial statistical spectrum of the cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane prepared by in-situ reduction in Example 1.

[0037] Figure 6 This is the antiviral statistical spectrum of cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane prepared by in-situ reduction in Example 1. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0039] The antibacterial and antiviral polytetrafluoroethylene nanofiber membrane obtained in the example and the polytetrafluoroethylene nanofiber membrane in the control group were tested for the pore size, moisture permeability and killing rate of influenza virus. The testing method is as follows:

[0040] Fiber membrane pore size: tested according to QB / T 5002-2016 standard;

[0041] Moisture permeability: Tested in accordance with GB 19082-2009 standard;

[0042] Antibacterial rate: refer to GB / T20944.3-2008;

[0043] Antiviral rate: tested in accordance with ISO 18184 standard.

[0044] Example 1

[0045] (1) Raw material preparation:

[0046]

[0047] (2) Copper sulfate crystal loaded polytetrafluoroethylene nanofiber membrane: prepare a copper sulfate solution with a molar concentration of 0.1 mol / L, and spray the copper sulfate solution evenly on the polytetrafluoroethylene nanofiber membrane with a spraying amount of 0.05 g / cm 2 , and finally put it into a 125℃ oven and dry it for 2 minutes.

[0048] (3) In situ reduction of cuprous oxide: Sodium hydroxide and ascorbic acid are dissolved in an ethanol / water mixed solvent (water volume accounts for 30%), the copper sulfate-loaded polytetrafluoroethylene nanofiber membrane obtained above is immersed in a 1.5 mol / L sodium hydroxide solution, and then 0.1 mol / L ascorbic acid solution is slowly added thereto. After sufficient reaction, in situ reduced cuprous oxide is obtained.

[0049] (4) Heat setting: After the reaction is completed, the membrane is washed with deionized water several times and placed in a vacuum oven at 180°C for 120 min. After cooling and taking out, a cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane is obtained.

[0050] Example 2

[0051] (1) Raw material preparation:

[0052]

[0053] (2) Copper sulfate crystal loaded polytetrafluoroethylene nanofiber membrane: prepare a copper sulfate solution with a molar concentration of 0.1 mol / L, and spray the copper sulfate solution evenly on the polytetrafluoroethylene nanofiber membrane with a spraying amount of 0.1 g / cm 2 , and finally put it into a 100℃ oven to dry for 20 minutes.

[0054] (3) In situ reduction of cuprous oxide: Sodium hydroxide and ascorbic acid are dissolved in an ethanol / water mixed solvent (water volume accounts for 25%), the copper sulfate-loaded polytetrafluoroethylene nanofiber membrane obtained above is immersed in a 2 mol / L sodium hydroxide solution, and then a 2 mol / L ascorbic acid solution is slowly added thereto. After sufficient reaction, in situ reduced cuprous oxide is obtained.

[0055] (4) Heat setting: After the reaction is completed, the membrane is washed with deionized water several times and placed in a vacuum oven at 200°C for 5 minutes. After cooling and taking out, a cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane is obtained.

[0056] Example 3

[0057] (1) Raw material preparation:

[0058]

[0059]

[0060] (2) Copper sulfate crystal loaded polytetrafluoroethylene nanofiber membrane: prepare a copper sulfate solution with a molar concentration of 0.2 mol / L, and spray the copper sulfate solution evenly on the polytetrafluoroethylene nanofiber membrane with a spraying amount of 0.001 g / cm 2 Finally, put it in a 75℃ oven and dry it for 10 minutes

[0061] (3) In situ reduction of cuprous oxide: Sodium hydroxide and ascorbic acid are dissolved in an ethanol / water mixed solvent (water volume accounts for 100%), the copper sulfate-loaded polytetrafluoroethylene nanofiber membrane obtained above is immersed in a 0.1 mol / L sodium hydroxide solution, and then a 1.5 mol / L ascorbic acid solution is slowly added thereto. After sufficient reaction, in situ reduced cuprous oxide is obtained.

[0062] (4) Heat setting: After the reaction is completed, the membrane is washed with deionized water several times and placed in a 75°C vacuum oven for 60 min. After cooling and taking out, a cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane is obtained.

[0063] The antibacterial and antiviral polytetrafluoroethylene nanofiber membranes obtained in Examples 1 to 3 were tested for fiber membrane pore size, moisture permeability, bacteria killing rate, and virus disinfecting rate. The test results are shown in the following table.

[0064]

[0065] By analyzing the data in the above table, it can be seen that the antibacterial and antiviral polytetrafluoroethylene nanofiber membrane obtained in Example 1 has the smallest pore size and the highest moisture permeability, especially when the spraying amount is 0.05 g / cm 2 When the cuprous oxide is uniformly dispersed on the surface of the polytetrafluoroethylene nanofiber membrane, it is more conducive to cuprous oxide to directly contact bacteria through electrostatic adsorption. Thus, the effect of inactivating bacteria is achieved. The results show that the inhibition rates of Escherichia coli and Staphylococcus aureus are both 99.9%, which shows that in the preparation method of the in-situ reduction cuprous oxide loaded polytetrafluoroethylene nanofiber membrane of the present invention, the molar concentration of copper sulfate is 0.1 mol / L and the spraying amount is 0.05 g / cm 2 , dried in an oven at 125°C for 2 min, the water volume proportion in the ethanol / water mixed solvent was 50%, the molar concentration of the sodium hydroxide solution was 1 mol / L, and the molar concentration of the ascorbic acid solution was 0.1 mol / L, the obtained cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane had both the best moisture permeability efficiency and antibacterial and antiviral effects.

[0066] Depend on Figure 1 It can be seen that the polytetrafluoroethylene nanofiber membrane in the control group showed a microscopic morphology of radial polymer chain fibers and island nodes, and had a "fibril-node" fiber network structure.

[0067] Depend on Figure 2 It can be seen that the in-situ reduction method has no effect on the microscopic morphology of the polytetrafluoroethylene nanofiber membrane. The antibacterial and antiviral nanofiber membrane still presents a porous structure and an interconnected nanofiber network structure formed by nodes at the microscopic level, and cuprous oxide is loaded on the "fibril-node" structure.

[0068] Depend on Figure 3 It can be seen that, taking Escherichia coli as the experimental bacteria, compared with the control group polytetrafluoroethylene nanofiber membrane, there is almost no colony produced on the agar plate of the antibacterial and antiviral polytetrafluoroethylene nanofiber membrane, indicating that the obtained antibacterial and antiviral polytetrafluoroethylene nanofiber membrane has an excellent effect of inactivating Escherichia coli.

[0069] Depend on Figure 4 It can be seen that, taking Staphylococcus aureus as the experimental bacteria, compared with the control group polytetrafluoroethylene nanofiber membrane, the antibacterial and antiviral polytetrafluoroethylene nanofiber membrane produced almost no colonies on the agar plate, indicating that the obtained antibacterial and antiviral polytetrafluoroethylene nanofiber membrane has an excellent effect of inactivating Staphylococcus aureus.

[0070] Depend on Figure 5It can be seen that statistical analysis shows that the inactivation rate of the antibacterial and antiviral polytetrafluoroethylene nanofiber membrane for Escherichia coli and Staphylococcus aureus is over 99%, indicating that it has a broad-spectrum antibacterial property.

[0071] Depend on Figure 6 It can be seen that the antiviral properties of the antibacterial and antiviral polytetrafluoroethylene nanofiber membrane are characterized by fluorescent protein, and statistical analysis shows that it can significantly reduce the infection rate of the virus and has an excellent effect of inactivating viruses.

[0072] The specific embodiments are only explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A method for preparing cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane by in-situ reduction, comprising the following steps: (1) Weighing copper sulfate and dissolving it in a solvent, stirring to obtain a copper sulfate solution; spraying the copper sulfate solution evenly on the surface of the polytetrafluoroethylene nanofiber membrane, and drying to obtain the copper sulfate-loaded polytetrafluoroethylene nanofiber membrane; (2) The copper sulfate-loaded polytetrafluoroethylene nanofiber membrane obtained in step (1) is immersed in an alkaline solution, and the copper sulfate crystals react in situ to generate copper hydroxide under an alkaline environment; a reducing agent solution is then added to react fully, and after vacuum heat setting, the in-situ reduction is obtained to prepare the cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane.

2. The method according to claim 1, characterized in that: The solvent in step (1) is a mixed solvent of ethanol and water, and the volume proportion of water is 25% to 100%.

3. The method according to claim 1, characterized in that: The molar concentration of the copper sulfate solution in step (1) is 0.05 mol / L to 0.2 mol / L.

4. The method according to claim 1, characterized in that: The spraying amount of the copper sulfate solution in step (1) is 0.001 g / cm 2 -0.1g / cm 2 .

5. The method according to claim 1, characterized in that: The drying temperature in step (1) is 75° C. to 125° C., and the drying time is 2 min to 20 min.

6. The method according to claim 1, characterized in that: The alkali solution in step (2) is a sodium hydroxide solution with a molar concentration of 0.1 mol / L to 2.0 mol / L.

7. The method according to claim 1, characterized in that: The reducing agent solution in step (2) is an ascorbic acid solution with a molar concentration of 0.1 mol / L to 2.0 mol / L.

8. The method according to claim 1, characterized in that: The vacuum heat setting temperature in step (2) is 75° C. to 200° C., and the heat setting time is 5 min to 120 min.

9. The method according to claim 1, characterized in that: The cuprous oxide-loaded polytetrafluoroethylene nanofiber membrane obtained in the step (2) is applied to the fields of personal protection and air filtration.

Citation Information

Patent Citations

  • Antibacterial nanofiber membrane and preparation method thereof

    CN108251965A

  • Antibacterial and antiviral protective material and preparation method thereof

    CN113622186A

  • Antibacterial and antiviral mask and preparation method thereof

    CN113925240A

  • Preparation method of antibacterial and anti-virus air purification material

    CN114247309A

  • Antiviral polytetrafluoroethylene nanofiber membrane as well as preparation method and application thereof

    CN117567825A

Cited By

  • Weakly acidic medical non-woven fabric and preparation method thereof

    CN122856511A