Fluorescent alumina fiber material and preparation method thereof
By grafting rare earth complexes onto the surface of alumina fibers and modifying them with maleic anhydride and silane coupling agents, the problem of the lack of fluorescent properties of traditional alumina fibers and the low luminous efficiency of existing materials has been solved, achieving high efficiency and high color. Pure fluorescent properties suitable for a variety of applications.
Patent Information
- Application Number
- CN202410769633.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional alumina fibers lack fluorescent properties, which limits their use in applications that require fluorescent functions. Moreover, existing materials that combine rare earth complexes with alumina fibers have low luminous efficiency and complicated preparation processes.
By grafting rare earth complexes onto the surface of alumina fibers, the 4f electronic configuration of rare earth metal ions is used to produce characteristic luminescence, and combined with maleic anhydride and silane coupling agents to modify alumina fibers, a highly efficient, high color purity fluorescent material is formed. , using ultrasonic treatment and coordination reaction to improve the optical properties of the material.
It achieves the high efficiency and high color purity fluorescence performance of alumina fiber, simplifies the preparation process, improves the stability and durability of the material, and is suitable for fields such as biomarkers and fluorescent probe detection.
Smart Images

Figure CN118727441A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorescent fiber preparation, and specifically relates to a fluorescent alumina fiber material and a preparation method thereof. Background Art
[0002] As an important inorganic fiber material, alumina fiber is widely used in various industrial fields due to its excellent physical and chemical properties, such as high mechanical strength, good thermal stability and chemical stability. Luminescent materials have a wide range of applications in modern science and technology, especially in the fields of biomarkers and fluorescent probe detection. However, traditional alumina fibers usually do not have fluorescent properties, which limits their application in situations where fluorescent functions are required.
[0003] In recent years, rare earth complexes have attracted extensive attention due to their unique luminescence properties. Rare earth complexes have high efficiency and high color purity luminescence performance, and their luminescence wavelength can be adjusted by the selection and design of ligands. Therefore, combining rare earth complexes with alumina fibers to prepare luminescent materials with luminescence properties has become a challenging and potentially valuable research direction.
[0004] At present, although there have been some research reports on the combination of rare earth complexes and alumina fibers, these materials often have problems such as low luminous efficiency and complex preparation process. Summary of the invention
[0005] The purpose of the present invention is to provide a fluorescent alumina fiber material and a preparation method thereof, wherein a rare earth complex is grafted onto the surface of the alumina fiber through a simple chemical reaction to give it sensitive luminescence properties. The material has high efficiency, high color purity luminescence properties, and the preparation process is simple and the cost is low.
[0006] The above technical objectives of the present invention are achieved through the following technical solutions: The fluorescent alumina fiber material provided by the present invention is a rare earth metal complex fluorescent alumina fiber material, and its structure adopts that the modified alumina fiber is connected with the organic ligand through the coordination effect of the rare earth metal ion; Among them, the molar ratio of modified alumina fiber, rare earth metal ions and 1,10-phenanthroline is (1~3):1:3.
[0007] The fluorescent alumina fiber material provided by the present invention is prepared by grafting a rare earth complex onto alumina fiber. The rare earth ions have a special 4f electron configuration. When these electrons transition between different energy levels, characteristic luminescence can be generated. When the electrons return from the excited state to the ground state, light of a specific wavelength is released, and the material has high efficiency and high color purity luminescence performance. In the complex provided by the present invention, both ligands can be connected to the rare earth ions through coordination bonds, and energy is transferred to the rare earth ions, thereby stimulating the luminescence of the rare earth ions and forming an "antenna effect", so that the alumina fiber has higher luminescence efficiency and color purity, and gives the alumina fiber sensitive fluorescence characteristics.
[0008] Furthermore, the modified alumina fiber is obtained by modifying the alumina fiber with maleic anhydride.
[0009] Maleic anhydride modification can form a uniform and stable functional layer on the surface of alumina fibers, which is beneficial to the fixation and arrangement of fluorescent ligands, thereby improving the optical properties of the material and increasing the fluorescence efficiency and luminescence intensity.
[0010] Furthermore, maleic anhydride modifies the alumina fiber through a coupling agent.
[0011] Furthermore, the coupling agent is a silane coupling agent, preferably silane coupling agent HK-550.
[0012] Furthermore, the alumina fibers are uniform and continuous fibers.
[0013] In the present invention, uniform and continuous alumina fibers are selected to ensure uniform distribution of fibers in the material, so that the final fluorescent alumina fiber material has more consistent performance and characteristics. At the same time, the uniform and continuous alumina fibers can provide a larger surface area and more contact points, thereby enhancing the binding ability with organic ligands, which is beneficial to improving fluorescence efficiency and luminous intensity.
[0014] Furthermore, the rare earth metal is any one of Sm, Eu, Tb or Dy.
[0015] Furthermore, the organic ligand is 1,10-phenanthroline; 1,10-phenanthroline, as a ligand, can form a stable complex with rare earth ions.
[0016] The present invention also provides a method for preparing a fluorescent alumina fiber material, which has the same technical effect.
[0017] The present invention provides a method for preparing a fluorescent alumina fiber material, which comprises modifying modified alumina fiber with a rare earth metal to obtain rare earth metal modified alumina fiber; and performing a coordination reaction between the rare earth metal modified alumina fiber and an organic ligand to obtain the fluorescent alumina fiber material.
[0018] The present invention adopts the above-mentioned step sequence, firstly performing rare earth metal modification on alumina fiber to ensure that the rare earth metal can better combine with the surface of alumina fiber, improve the compatibility between them, and facilitate the subsequent coordination reaction; then performing coordination reaction on the basis of rare earth metal modified alumina fiber can make the organic ligand more easily combine with alumina fiber and form a stable chemical structure, thereby improving the grafting efficiency of the organic ligand.
[0019] The above-mentioned sequence of steps can also ensure that the combination of rare earth metals and alumina fibers is more firm and stable, which is beneficial to improving the stability and durability of the fluorescent alumina fiber material, and can better control the structure and properties of the fluorescent alumina fiber material, thereby optimizing its fluorescent properties, optical properties and other related properties.
[0020] Furthermore, the preparation method provided by the present invention specifically comprises the following steps: The modified alumina fiber is placed in a solution containing rare earth metal ions and subjected to ultrasonic treatment to obtain rare earth metal modified alumina fiber; The rare earth modified alumina fiber is placed in a solution containing an organic ligand and subjected to ultrasonic treatment to obtain the fluorescent alumina fiber material.
[0021] Furthermore, the solution containing rare earth metal ions is an anhydrous ethanol solution of rare earth ions with a concentration of 1 to 5 mol%.
[0022] Furthermore, the solution containing the organic ligand is an anhydrous ethanol solution of the organic ligand, and the concentration is 3-15 mol%.
[0023] Furthermore, the modified alumina fiber is ultrasonicated and soaked in an anhydrous ethanol / water solution before use.
[0024] Furthermore, the preparation method of the modified alumina fiber is as follows: the alumina fiber is placed in a solution containing maleic anhydride and a coupling agent for ultrasonic treatment, and the molar ratio of maleic anhydride, alumina fiber and coupling agent is 1:(2~5):(1~3).
[0025] The present invention can ensure that the chemical activity of the surface of the alumina fiber is moderate through good molar ratio control, which is beneficial to the fixation and arrangement of the fluorescent ligands and improves the fluorescence efficiency and luminous intensity of the fluorescent alumina fiber material.
[0026] Furthermore, the solution containing maleic anhydride and a coupling agent is an anhydrous ethanol solution of maleic anhydride and a coupling agent, and the concentration is 5-10wt%.
[0027] Furthermore, in all the anhydrous ethanol / water solutions of the present invention, the volume ratio of anhydrous ethanol to water is 1:1.
[0028] Furthermore, the preparation method of alumina fiber is as follows: an aluminum source is mixed with a spinning solution to prepare an alumina precursor spinning solution, an alumina fiber precursor is prepared by electrostatic spinning technology, and the alumina fiber is calcined to obtain the alumina fiber.
[0029] Furthermore, the calcination temperature is 700-900°C.
[0030] Furthermore, the aluminum source is aluminum isopropoxide, and the spinning solution is polyvinyl alcohol.
[0031] The present invention adopts aluminum isopropoxide and polyvinyl alcohol as the aluminum source and the spinning solution, so that the aluminum source and the spinning solution have better compatibility, thereby obtaining more uniform and continuous alumina fibers, which is beneficial to controlling the structure and properties of the fluorescent alumina fiber material, thereby optimizing its fluorescence properties, optical properties and other related properties.
[0032] In summary, the present invention has the following beneficial effects: The alumina fiber with fluorescent properties provided by the present invention is a fluorescent alumina fiber prepared by combining a rare earth complex and alumina fiber. The modified alumina fiber and 1,10-phenanthroline are bonded with rare earth ions to form an energy transfer channel. Under the excitation of excitation light, the alumina fiber is endowed with unique fluorescent properties. Compared with traditional alumina fibers, the alumina fiber grafted with the rare earth complex has higher luminous efficiency and color purity, excellent fluorescent properties, and a simple preparation method. It has broad application prospects in the fields of biological markers and fluorescent probe detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a picture of the fluorescent alumina fiber containing the Eu rare earth complex of the present invention under ultraviolet light, emitting bright red; Figure 2 This is a microscopic image of the modified alumina fiber of the present invention under a scanning electron microscope; Figure 3 This is a microscopic image of the fluorescent alumina fiber containing the Eu rare earth complex of the present invention under a scanning electron microscope; Figure 4 This is the fluorescence emission spectrum of the fluorescent alumina fiber containing the Eu rare earth complex of the present invention, the excitation wavelength is 350nm, and the maximum emission peak is located at 614nm; the abscissa is the wavelength, and the ordinate is the intensity. DETAILED DESCRIPTION
[0034] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, a fluorescent alumina fiber material and a preparation method thereof proposed in accordance with the present invention, its specific implementation method, characteristics and effects are described in detail as follows.
[0035] The sources of raw materials used in this specific implementation are as follows: Aluminum isopropoxide: Sinopharm Chemical Reagent Co., Ltd. Polyvinyl alcohol: Sinopharm Chemical Reagent Co., Ltd. Maleic anhydride: Shanghai Aladdin Biochemical Technology Co., Ltd. Silane coupling agent HK-550: Shandong Yousuo Chemical Technology Co., Ltd. Rare earth metal nitrates: Shanghai Titan Technology Co., Ltd. 1,10-Phenanthroline: Shanghai Zhanyun Chemical Co., Ltd. A fluorescent alumina fiber material provided in this specific embodiment is a rare earth metal complex fluorescent alumina fiber material, whose structure is that the modified alumina fiber is connected to the organic ligand through the coordination effect of the rare earth metal, wherein the molar ratio of the modified alumina fiber, the rare earth metal ion and the organic ligand is (1~3):1:3.
[0036] In some preferred embodiments, the rare earth ion is preferably any one of Sm, Eu, Tb or Dy, in the form of hexahydrate of nitrate as the raw material, the organic ligand is preferably 1,10-phenanthroline, and the modified alumina fiber is preferably maleic anhydride grafted alumina fiber.
[0037] This specific embodiment also provides a method for preparing the fluorescent alumina fiber material, comprising the following steps: S1. Place the modified alumina fiber in an anhydrous ethanol solution of rare earth nitrate, perform ultrasonic treatment for 20 min to 40 min, stir at 40 to 80 °C for 6 h to 8 h, and obtain the rare earth modified alumina fiber by centrifugation, washing and drying; S2. Place the rare earth modified alumina fiber into a 1,10-phenanthroline anhydrous ethanol solution, perform ultrasonic treatment for 20 min to 40 min, stir at room temperature for 1 h to 3 h, and obtain the fluorescent alumina fiber material through centrifugation, washing, and drying.
[0038] In some preferred embodiments, alumina precursor fibers are prepared by electrospinning technology, calcined at 700° C. to 900° C. to obtain alumina fibers, which are then stirred in an anhydrous ethanol / water solution for 12 h to 16 h.
[0039] In some preferred embodiments, the method for obtaining alumina fiber material by electrospinning is as follows: an aluminum source and a spinning solution are prepared into an alumina precursor spinning solution in a beaker, alumina fibers are prepared by electrospinning technology, and the alumina fibers are calcined at a high temperature of 700 to 900°C in a box furnace for 3 to 5 hours to obtain alumina fibers; in some preferred embodiments, the aluminum source is aluminum isopropoxide, and the spinning solution is polyvinyl alcohol.
[0040] In some preferred embodiments, the preparation method of modified alumina fiber is as follows: ultrasonically treat the alumina fiber in an anhydrous ethanol solution of maleic anhydride and silane coupling agent for 30 minutes to 1 hour, stir at 40 to 80°C for 10 hours to 14 hours, and obtain the modified alumina fiber after centrifugation, washing, and drying, wherein the molar ratio of maleic anhydride, alumina fiber and silane coupling agent is 1:(2 to 5):(1 to 3).
[0041] Example 1: A fluorescent alumina fiber material and a preparation method thereof The fluorescent alumina fiber material provided in this embodiment has a structure in which maleic anhydride modified alumina fiber is connected to the organic ligand 1,10-phenanthroline through the coordination effect of Eu; wherein, in the maleic anhydride modified alumina fiber, the molar ratio of Eu and 1,10-phenanthroline is 1:1:3.
[0042] The method for preparing the fluorescent alumina fiber material provided in this embodiment comprises the following steps: S1. Preparation of alumina fiber: Aluminum isopropoxide and polyvinyl alcohol are prepared into an alumina precursor spinning solution in a beaker, alumina fiber is prepared by electrospinning technology, and the alumina fiber is calcined in a box furnace at 800° C. for 4 hours to obtain alumina fiber.
[0043] S2. Pretreatment of alumina fiber: Take the above-mentioned alumina fiber, wash it with a solution of anhydrous ethanol and deionized water in a volume ratio of 1:1, wash it under ultrasonic oscillation for 30 minutes, stir it in the mixed solution of anhydrous ethanol and deionized water for 14 hours, and dry it at 70°C for 14 hours for subsequent use.
[0044] S3. Prepare modified alumina fiber solution: disperse maleic anhydride and silane coupling agent evenly in two beakers of anhydrous ethanol solution respectively, stir well, then pour the maleic anhydride solution into the coupling agent solution, and stir magnetically for 6 hours, wherein the molar ratio of maleic anhydride to silane coupling agent is 1:1, and the concentration of the anhydrous ethanol mixed solution of maleic anhydride and silane coupling agent is 8wt%.
[0045] S4, maleic anhydride and silane coupling agent mixed solution in a beaker, ultrasonic oscillation for 30 minutes, stirring at 60 ° C for 14 hours, centrifugation, washing, drying to obtain modified alumina fiber (such as Figure 2 As shown), wherein the molar ratio of maleic anhydride, alumina fiber and silane coupling agent is 1:2:1.
[0046] S5. Preparation of europium modified alumina fiber: soaking the modified alumina fiber prepared above in an anhydrous ethanol solution of europium nitrate hexahydrate with a concentration of 4 wt %, stirring at 60° C. for 8 h, and obtaining europium modified alumina fiber through centrifugation, washing, and drying.
[0047] S6. Preparation of rare earth europium complex grafted alumina fiber luminescent material: soak the europium modified alumina fiber prepared above in a 4 wt% 1,10-phenanthroline anhydrous ethanol solution, stir at room temperature for 2 h, and obtain the fluorescent alumina fiber material through centrifugation, washing and drying.
[0048] Example 2: A fluorescent alumina fiber material and a preparation method thereof The fluorescent alumina fiber material provided in this embodiment has a structure in which maleic anhydride modified alumina fiber is connected to the organic ligand 1,10-phenanthroline through the coordination effect of terbium; wherein, in the maleic anhydride modified alumina fiber, the molar ratio of terbium to 1,10-phenanthroline is 1:1:3.
[0049] The method for preparing the fluorescent alumina fiber material provided in this embodiment comprises the following steps: S1. Preparation of alumina fiber: Aluminum isopropoxide and polyvinyl alcohol are prepared into an alumina precursor spinning solution in a beaker, alumina fiber is prepared by electrospinning technology, and the alumina fiber is calcined in a box furnace at 700° C. for 4 hours to obtain alumina fiber.
[0050] S2. Pretreatment of alumina fibers: The alumina fibers were cleaned with a solution of anhydrous ethanol and deionized water in a volume ratio of 1:1, cleaned under ultrasonic oscillation for 30 minutes, and dried at 70° C. for 12 hours for subsequent use.
[0051] S3. Prepare modified alumina fiber solution: disperse maleic anhydride and silane coupling agent evenly in two beakers of anhydrous ethanol solution respectively, stir well, then pour the maleic anhydride mixed solution into the silane coupling agent mixed solution, and stir magnetically for 6 hours, wherein the molar ratio of maleic anhydride to silane coupling agent is 1:1, and the concentration of the anhydrous ethanol mixed solution of maleic anhydride and silane coupling agent is 8wt%.
[0052] S4, maleic anhydride and silane coupling agent mixed solution in a beaker, ultrasonic oscillation for 20 minutes, stirring at 60 ° C for 10 hours, centrifuging, washing and drying to obtain modified alumina fiber (, wherein the molar ratio of maleic anhydride, alumina fiber and silane coupling agent is 1:2:1.
[0053] S5. Preparation of terbium-modified alumina fibers: soaking the modified alumina fibers prepared above in an anhydrous ethanol solution of terbium nitrate hexahydrate with a concentration of 5 wt %, stirring at 60° C. for 7 h, and obtaining terbium-modified alumina fibers through centrifugation, washing, and drying.
[0054] S6. Preparation of rare earth terbium complex grafted alumina fiber luminescent material: soak the terbium modified alumina fiber prepared above in an anhydrous ethanol solution of 1,10-phenanthroline with a concentration of 5wt%, stir at room temperature for 1 hour, and obtain the fluorescent alumina fiber material through centrifugation, washing and drying.
[0055] Example 3: A fluorescent alumina fiber material and a preparation method thereof The fluorescent alumina fiber material provided in this embodiment has a structure in which maleic anhydride modified alumina fiber is connected to the organic ligand 1,10-phenanthroline through the coordination effect of samarium; wherein, in the maleic anhydride modified alumina fiber, the molar ratio of samarium to 1,10-phenanthroline is 1:1:3.
[0056] The method for preparing the fluorescent alumina fiber material provided in this embodiment comprises the following steps: S1. Preparation of alumina fiber: Aluminum isopropoxide and polyvinyl alcohol are prepared into an alumina precursor spinning solution in a beaker, alumina fiber is prepared by electrospinning technology, and the alumina fiber is calcined at 900° C. for 4 hours in a box furnace to obtain alumina fiber.
[0057] S2. Pretreatment of alumina fibers: The alumina fibers were cleaned with a solution of anhydrous ethanol and deionized water in a volume ratio of 1:1, cleaned under ultrasonic oscillation for 30 minutes, and dried at 70° C. for 16 hours for subsequent use.
[0058] S3. Prepare modified alumina fiber solution: disperse maleic anhydride and silane coupling agent evenly in two beakers of anhydrous ethanol solution respectively, stir well, then pour the maleic anhydride mixed solution into the silane coupling agent mixed solution, and stir magnetically for 6 hours, wherein the molar ratio of maleic anhydride to silane coupling agent is 1:1, and the concentration of the anhydrous ethanol mixed solution of maleic anhydride and silane coupling agent is 8wt%.
[0059] S4, maleic anhydride and silane coupling agent mixed solution in a beaker, ultrasonic oscillation for 30 minutes, stirring at 60°C for 14 hours, centrifuging, washing and drying to obtain modified alumina fiber, wherein the molar ratio of maleic anhydride, alumina fiber and silane coupling agent is 1:2:1.
[0060] S5. Preparation of samarium-modified alumina fibers: soaking the modified alumina fibers prepared above in an anhydrous ethanol solution of samarium nitrate hexahydrate at a concentration of 4 wt %, stirring at 60° C. for 8 h, and obtaining samarium-modified alumina fibers through centrifugation, washing, and drying.
[0061] S6. Preparation of rare earth samarium complex grafted alumina fiber luminescent material: soak the samarium modified alumina fiber prepared above in a 4 wt% 1,10-phenanthroline anhydrous ethanol solution, stir at room temperature for 2 h, and obtain the fluorescent alumina fiber material through centrifugation, washing and drying.
[0062] Example 4: A fluorescent alumina fiber material and a preparation method thereof The fluorescent alumina fiber material provided in this embodiment has a structure in which maleic anhydride modified alumina fiber is connected to the organic ligand 1,10-phenanthroline through the coordination effect of dysprosium; wherein, in the maleic anhydride modified alumina fiber, the molar ratio of dysprosium to 1,10-phenanthroline is 1:1:3.
[0063] The method for preparing the fluorescent alumina fiber material provided in this embodiment comprises the following steps: S1. Preparation of alumina fiber: Aluminum isopropoxide and polyvinyl alcohol are prepared into an alumina precursor spinning solution in a beaker, alumina fiber is prepared by electrospinning technology, and the alumina fiber is calcined at 900° C. for 4 hours in a box furnace to obtain alumina fiber.
[0064] S2. Pretreatment of alumina fibers: The alumina fibers were cleaned with a solution of anhydrous ethanol and deionized water in a volume ratio of 1:1, cleaned under ultrasonic oscillation for 30 minutes, and dried at 70° C. for 15 hours for subsequent use.
[0065] S3. Prepare modified alumina fiber solution: disperse maleic anhydride and silane coupling agent evenly in two beakers of anhydrous ethanol solution respectively, stir well, then pour the maleic anhydride mixed solution into the silane coupling agent mixed solution, and stir magnetically for 4 hours, wherein the molar ratio of maleic anhydride to silane coupling agent is 1:1, and the concentration of the anhydrous ethanol mixed solution of maleic anhydride and silane coupling agent is 8wt%.
[0066] S4, maleic anhydride and silane coupling agent mixed solution in a beaker, ultrasonic oscillation for 30 minutes, stirring at 60°C for 14 hours, centrifuging, washing and drying to obtain modified alumina fiber, wherein the molar ratio of maleic anhydride, alumina fiber and silane coupling agent is 1:2:1.
[0067] S5. Preparation of dysprosium-modified alumina fibers: soaking the modified alumina fibers prepared above in an anhydrous ethanol solution of dysprosium nitrate hexahydrate at a concentration of 4 wt %, stirring at 60° C. for 8 h, and obtaining dysprosium-modified alumina fibers through centrifugation, washing, and drying.
[0068] S6. Preparation of rare earth dysprosium complex grafted alumina fiber luminescent material: soak the dysprosium modified alumina fiber prepared above in a 4 wt% 1,10-phenanthroline anhydrous ethanol solution, stir at room temperature for 2 h, and obtain the fluorescent alumina fiber material through centrifugation, washing and drying.
[0069] The fluorescent alumina fiber material prepared in Example 1 was subjected to fluorescence emission spectrum test and SEM test, and pictures were taken under ultraviolet light. The test results are as follows: Figure 1 , 3 and 4.
[0070] Among them, the microscopic morphology of the rare earth europium complex fluorescent alumina fiber material with fluorescent properties under a scanning electron microscope is as follows: Figure 3 As shown; the fluorescence characteristics of the rare earth europium complex fluorescent alumina fiber material with fluorescence characteristics are as follows Figure 1 As shown, under ultraviolet light, it emits a bright red color; the fluorescence emission spectrum of the rare earth europium complex fluorescent alumina fiber material with fluorescent properties is shown in Figure 4 As shown, it can be seen that when the excitation wavelength is 350nm, the prepared rare earth europium complex grafted alumina fiber luminescent material exhibits characteristic radiation at 614nm, which indicates that the rare earth complex grafted alumina fiber prepared by the present invention has higher luminous efficiency and color purity, and has excellent fluorescence properties.
[0071] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been presented as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A fluorescent alumina fiber material, characterized in that: The fluorescent alumina fiber material is a rare earth metal complex fluorescent alumina fiber material, and its structure is that the modified alumina fiber and the organic ligand are connected through the coordination effect of rare earth metal ions; Among them, the molar ratio of modified alumina fiber, rare earth metal ions and organic ligands is (1~3):1:
3.
2. The fluorescent alumina fiber material according to claim 1, characterized in that: The modified alumina fiber is obtained by modifying alumina fiber with maleic anhydride.
3. The fluorescent alumina fiber material according to claim 2, characterized in that: Maleic anhydride was used to modify alumina fiber through coupling agent.
4. A fluorescent alumina fiber material according to claim 2 or 3, characterized in that: The alumina fibers are uniform and continuous fibers.
5. The fluorescent alumina fiber material according to claim 1, characterized in that: The rare earth metal is any one of Sm, Eu, Tb or Dy.
6. The fluorescent alumina fiber material according to claim 1, characterized in that: The organic ligand is 1,10-phenanthroline.
7. The method for preparing a fluorescent alumina fiber material according to any one of claims 1 to 6, characterized in that: After the modified alumina fiber is modified by rare earth metal, rare earth metal modified alumina fiber is obtained; the rare earth metal modified alumina fiber is subjected to coordination reaction with organic ligand to obtain the fluorescent alumina fiber material.
8. The method for preparing a fluorescent alumina fiber material according to claim 7, characterized in that: The steps include: The modified alumina fiber is placed in a solution containing rare earth metal ions and subjected to ultrasonic treatment to obtain rare earth metal modified alumina fiber; The rare earth modified alumina fiber is placed in a solution containing an organic ligand and subjected to ultrasonic treatment to obtain the fluorescent alumina fiber material.
9. The method for preparing a fluorescent alumina fiber material according to claim 7, characterized in that: The preparation method of the modified alumina fiber is as follows: the alumina fiber is placed in a solution containing maleic anhydride and a coupling agent for ultrasonic treatment, wherein the molar ratio of maleic anhydride, alumina fiber and coupling agent is 1:(2-5):(1-3).
10. The method for preparing a fluorescent alumina fiber material according to claim 9, characterized in that: The preparation method of the alumina fiber is as follows: an aluminum source is mixed with a spinning solution to prepare an alumina precursor spinning solution, an alumina fiber precursor is prepared by using an electrostatic spinning technology, and the alumina fiber is calcined to obtain the alumina fiber.