Hollow porous fiber with controllable slow release function and preparation method thereof

By combining Schiff base bond hydrogel with nanoparticle functional substances in hollow porous fibers, controllable sustained release and long-lasting release of functional substances are achieved, which solves the problem of difficulty in controlling the release rate and amount in the existing technology. , enhanced biocompatibility and self-healing capabilities.

CN118727446AInactive Publication Date: 2024-10-01FUJIAN CHANGLE CITY CHANGYUAN TEXTILE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410766188.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, hollow porous fibers cannot effectively control the release rate and amount of functional substances during use, resulting in insufficient controllability of the sustained release function.

Method used

The Schiff base bond hydrogel generated by the reaction of aldehyde-containing compounds and carboxymethyl chitosan is used as a sustained-release filler. It forms a dynamic equilibrium system through Schiff base bond linkage and combines with nanoparticle functional substances to achieve slow release of functional substances. Release, and regulate the release rate through external mechanical stimulation.

Benefits of technology

It achieves controlled and sustained release of functional substances, protects the activity of functional substances, avoids direct contact with the human body, reduces potential damage to human tissues and cells, and reduces the release rate through the self-repair mechanism, achieving antibacterial and decontamination effects. Long-lasting release of odorous and aromatic substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727446A_ABST
    Figure CN118727446A_ABST
Patent Text Reader

Abstract

The invention relates to a hollow porous fiber with a controllable slow release function and a preparation method thereof, the product comprises a hollow porous fiber, the hollow porous fiber is axially provided with a cavity, and micropores communicated with the cavity are uniformly distributed on the cavity wall; slow-release fillers are arranged in cavities and micropores of the hollow porous fibers, and functional substances are uniformly distributed in the slow-release fillers; the slow-release filler is hydrogel with a Schiff base bond, which is obtained by reacting an aldehyde group-containing compound with carboxymethyl chitosan; the preparation method comprises the following steps: firstly, treating the hollow porous fibers to obtain filled hollow porous fibers; and immersing the product into a carboxymethyl chitosan solution for treatment to obtain the product. The preparation method disclosed by the invention is simple and easy to implement, and the prepared hollow porous fiber can slowly release antibacterial, deodorant and aromatic functional substances based on a Schiff base reaction principle, and has unique advantages including self-repairing capability, controllable release rate and good biocompatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fiber molding, and relates to a hollow porous fiber with a controllable sustained-release function and a preparation method thereof. Background Art

[0002] Hollow porous fiber is a kind of chemical fiber with a special structure. Its cross section has a cavity along the axial direction, and the cavity wall has a porous structure, which gives the fiber unique properties. Its internal porous structure not only improves the warmth retention and fluffiness of the fiber, but also gives the fiber good air permeability and moisture absorption. Therefore, this fiber has a wide range of applications in many fields. For example, it can be made into various winter clothing and household items by utilizing its excellent warmth retention and comfort; it can be made into various filter equipment by utilizing its filtering performance; in the medical and health field, it can be made into various medical supplies, such as masks and bandages.

[0003] In addition, due to its hollow structure, the hollow porous fiber can also be used as an ideal drug delivery carrier. By controlling the pore size and surface properties, this fiber can accommodate various drug molecules and achieve precise release control. Therefore, hollow porous fibers can be used to prepare drug delivery systems, such as fiber films for local drug release, fiber catheters for drug delivery, etc.

[0004] In the prior art, hollow porous fibers have been used to achieve the sustained release function. For example, patent application CN1183289C discloses a fiber product with sustained release function and a preparation method thereof. The hollow channels of the prepared microporous fibers with sustained release function are filled with active agents, and the openings at both ends are blocked with permeable or impermeable resins. However, the rate at which the active agent is released from the fiber mainly depends on the number and pore size of the microporous fibers and the number and pore size of the holes generated by the subsequent resin blocking. Although this porous structure is conducive to the sustained release of functional materials, it cannot achieve the controlled release of functional substances during use.

[0005] In order to solve the above problems, patent application CN100540056C discloses a method for preparing drug thermosensitive hydrogel hollow fibers and its application. The prepared drug thermosensitive hydrogel hollow fibers use hollow fibers as carriers, and the inner cavity of the hollow fibers contains drug thermosensitive hydrogel to achieve temperature control of drug release.

[0006] Patent application CN1286528C discloses a hollow fiber drug carrier and its preparation method and application, wherein the hollow fiber drug carrier is a drug release material with controlled drug release obtained by deposition and adsorption of drugs in the hollow fiber carrier matrix using hollow inorganic bioactive fibers or degradable polymer fibers as carriers.

[0007] It can be seen from the above patents that hollow porous fibers can be used as functional sustained-release systems, but the existing technology achieves sustained-release function mainly relying on the special structure of hollow porous fibers and the load amount in the fibers to achieve controllable sustained-release of functional substances, and is unable to control the rate and amount of release of functional substances during the use of fiber products. Summary of the invention

[0008] The purpose of the present invention is to solve the problems existing in the prior art and to provide a hollow porous fiber with a controllable sustained release function and a preparation method thereof.

[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A hollow porous fiber with a controllable sustained release function comprises a hollow porous fiber, wherein the hollow porous fiber has a cavity in the axial direction, and micropores connecting the cavity are evenly distributed on the cavity wall;

[0011] The hollow porous fiber has a sustained-release filler in the cavity and micropores, and the functional substance is evenly distributed in the sustained-release filler;

[0012] The sustained-release filler is a hydrogel having a Schiff base bond obtained by reacting an aldehyde-containing compound with carboxymethyl chitosan;

[0013] The aldehyde-containing compound is polyethylene glycol modified with a dialdehyde group, oxidized sodium alginate or oxidized hyaluronic acid.

[0014] The hollow porous fiber with controllable sustained release function of the present invention has a sustained release filler and a functional substance inside, which forms a dynamic equilibrium system linked by a Schiff base structure (-N=C-) bond formed by an aldehyde group and an amino group; the sustained release filler is a hydrogel with self-repairing ability obtained by reacting an aldehyde-containing compound with carboxymethyl chitosan, and nano-particle functional substances are uniformly distributed and wrapped inside the hydrogel, and this structure is conducive to the slow release of the functional substances and also protects the activity of the functional substances; in addition, for functional substances with certain cytotoxicity (such as nano-silver, nano-cuprous oxide, nano-zinc, etc.), this structure avoids direct contact with the human body during use, thereby reducing damage to human tissues and cells.

[0015] When the hollow porous fiber of the present invention is stimulated by external forces, the bending, curling, and squeezing of the fiber will cause the chemical bonds of the hydrogel system linked by Schiff base bonds to break, thereby releasing a large amount of functional substances through the pore walls of the hollow porous fiber; when the external mechanical stimulation stops, and due to the presence of the Schiff base structure, the hydrogel system will self-repair, thereby reducing the release of functional substances, which shows that the present invention achieves the function of regulating the release of functional substances through external mechanical stimulation; in addition, when pressing is performed in an environment simulating body fluids, when the hollow fiber is deformed, the release of functional substances (such as silver ions, copper ions, and zinc ions) will be promoted, and the ions will be released through both ends of the fiber and the micropores; after the deformation is completed, the Schiff base structure is repaired and can be restored to a coated structure, and the release of silver ions is reduced, thereby achieving controllable and long-lasting release of antibacterial substances.

[0016] As the preferred technical solution:

[0017] In the hollow porous fiber with controllable sustained release function as described above, the functional substance is an antibacterial agent, a deodorant or a fragrance with a particle size of 5 to 100 nm.

[0018] A hollow porous fiber with a controlled sustained release function as described above, wherein the antibacterial agent is one or more of nano-silver, nano-cuprous oxide and nano-zinc;

[0019] The deodorant is one or more of nano titanium dioxide, nano silicon dioxide and nano bamboo charcoal;

[0020] The fragrance is a fragrance microcapsule formed by encapsulating essence with a shell material, and the shell material is gelatin, sodium alginate, chitosan, gum arabic or agar.

[0021] The hollow porous fiber with controllable sustained release function as described above is polyester fiber, polyamide fiber or polyacrylonitrile fiber; the fiber fineness of the hollow porous fiber is 2.0-15.0 dtex, the hollowness is 25-35%, and the micropore diameter is 0.01-0.5 μm.

[0022] The present invention also provides a method for preparing a hollow porous fiber with a controllable sustained release function as described in any of the preceding items, firstly, the hollow porous fiber is divided into two sections A and B, section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 30-40°C, section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed (section A is pressurized and section B is vacuumed at the same time), the pressurization and vacuuming process is repeated 3-5 times, and the pressure of sections A and B is controlled. The force difference is 0.05-0.3MPa. After the reaction is completed, the hollow porous fiber is washed with anhydrous ethanol and dried in sequence to achieve filling of the hollow porous fiber to obtain the filled hollow porous fiber; then the filled hollow porous fiber is immersed in a carboxymethyl chitosan solution according to a bath ratio of 1:50-65, and after being taken out, it is dried and cured in a vacuum drying oven at a relative vacuum pressure of -0.1-0MPa and a temperature of 26-32°C for 30-60min to obtain a hollow porous fiber with a controllable sustained release function;

[0023] The precursor composite solution is a mixed solution of an aldehyde compound aqueous solution and a functional substance; the concentration of the aldehyde compound aqueous solution is 0.5-3wt%; the content of the functional substance in the precursor composite solution is 1-10wt%.

[0024] As the preferred technical solution:

[0025] In the method for preparing the hollow porous fiber with controllable sustained release function, the carboxymethyl chitosan solution is obtained by adding carboxymethyl chitosan into water, stirring at 30-36° C. for 2-5 hours, and filtering 2-4 times.

[0026] In the method for preparing the hollow porous fiber with controllable sustained release function, the substitution degree of carboxymethyl chitosan is ≥80%; the concentration of the carboxymethyl chitosan solution is 1-5wt%, and the viscosity is 10-100mPa·s.

[0027] In the method for preparing a hollow porous fiber with a controllable sustained release function as described above, the length ratio of segments A and B is 1:1.

[0028] Principle of the invention:

[0029] As a dynamic covalent chemical system, the Schiff base reaction has a unique equilibrium reversible property, which makes it have broad application prospects in the field of medical materials. This reaction involves the breaking and forming of chemical bonds, especially imine bonds. The reversibility of these bonds gives the material the ability to self-repair. Figure 3As shown, the carbonyl group (C=O) of the aldehyde-containing compound of the present invention reacts with the amino group (-NH2) in the carboxymethyl chitosan to form an imine bond, the structure of which is R-CH=N-R', wherein R and R' represent two different groups connected to the nitrogen atom. The main reaction mechanism is as follows:

[0030] 1. Polyethylene glycol (PEG) modified with dialdehyde contains carbonyl. In chemistry, aldehyde (-CHO) is a functional group containing a carbon atom connected to a hydrogen atom, and its structure contains a carbonyl (C=O). Therefore, when polyethylene glycol (PEG) is modified with dialdehyde, it means that two aldehyde functional groups are introduced into the PEG molecule, and each aldehyde functional group contains a carbonyl group. It can form a covalent bond with molecules containing amino groups through Schiff base reaction.

[0031] 2. Oxidized sodium alginate contains carbonyl groups. During the preparation of oxidized sodium alginate, some hydroxyl groups of sodium alginate are oxidized to aldehyde groups, and the aldehyde groups contain carbonyl (C=O) functional groups. Therefore, oxidized sodium alginate can form covalent bonds with molecules containing amino groups through Schiff base reactions.

[0032] 3. Some hydroxyl groups (-OH) of hyaluronic acid can be oxidized to aldehyde groups (-CHO), thereby introducing carbonyl groups. Oxidized hyaluronic acid can form a Schiff base structure with compounds containing amino groups.

[0033] The hollow porous fiber of the present invention has a controllable slow-release function, and its uniqueness lies in the dynamic equilibrium system formed by the internal slow-release filler and the functional substance linked by Schiff base bonds. This structure not only realizes the slow release of the functional substance, but also protects the activity of the functional substance, while avoiding direct contact with the human body, reducing potential damage to human tissues and cells. Specifically, when the precursor solution of the slow-release filler reacts with carboxymethyl chitosan, a hydrogel with self-repairing ability is formed. Nanoparticle functional substances, such as nanosilver, nanocuprous oxide, nanozinc, etc., are evenly distributed and wrapped inside the hydrogel. These nanoparticle functional substances are wrapped by the hydrogel, thereby avoiding direct exposure to the external environment. Under normal use conditions, the functional substance is slowly released through the pore wall of the hollow porous fiber, achieving the effect of long-term release. When the fiber is stimulated by external forces, such as bending, curling, extrusion, etc., the hydrogel system linked by Schiff base bonds inside will break chemical bonds. This break causes the structure of the hydrogel to change, so that the functional substance can be released in large quantities through the pore wall of the fiber. This mechanism allows the release of functional substances to be regulated by external mechanical stimulation. Once the external mechanical stimulation stops, the hydrogel system will self-repair due to the presence of the Schiff base structure. This self-repair process not only restores the structural integrity of the hydrogel, but also reduces the release rate of the functional substance, allowing the fiber to achieve a slow release effect again.

[0034] The hollow porous fibers prepared by the Schiff base reaction of the present invention can slowly release antibacterial, deodorizing and aromatic functional substances, and have unique advantages, including self-repairing ability, controllable release rate and good biocompatibility. Such hollow porous fibers with controllable slow-release function can be prepared into various functional slow-release textiles, such as non-woven fabrics, woven fabrics and knitted fabrics, through a variety of processing methods. These textiles not only inherit the excellent properties of fibers, but also have better flexibility and wearability, making them have broad application potential in many fields such as medical care, home, personal care, and environmental protection.

[0035] Beneficial effects:

[0036] (1) In the present invention, the cavity and micropores of the hollow porous fiber contain a sustained-release filler, and the sustained-release filler and the functional substance form a dynamic equilibrium system through Schiff base bonds. This structure enables the functional substance to be released slowly over a certain period of time, rather than all at once, thereby achieving a sustained-release effect;

[0037] (2) The present invention can regulate the release rate and amount of functional substances through external mechanical stimulation. This regulation is to stimulate the hollow porous fibers through the action of external forces, so that the Schiff base bonds are broken and a large amount of functional substances are released at the same time. When the stimulation to the fibers stops, the hydrogel system will self-repair and reduce the release rate of the functional substances;

[0038] (3) The sustained-release filler of the present invention is a hydrogel with Schiff base bonds, and the nanoparticle functional substances are uniformly distributed and wrapped inside the hydrogel, which not only helps the slow release of the functional substances, but also protects the activity of the functional substances and avoids the inactivation of the functional substances during storage and use; at the same time, some metal ions also help stabilize the Schiff base chemical bonds;

[0039] (4) The structure of the hydrogel in the present invention avoids direct contact between functional substances with certain cytotoxicity and the human body during use, thereby reducing potential damage to human tissues and cells, which is crucial for improving the biosafety of the material and the feasibility of clinical application. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of the overall structure of the hollow porous fiber with controllable sustained release function;

[0041] Figure 2 Schematic diagram of the internal structure of the hollow porous fiber with controlled sustained release function;

[0042] Figure 3 The diagram is the mechanism of Schiff base reaction;

[0043] Figure 4 The diagram is the mechanism of the Schiff base reaction between dialdehyde-modified polyethylene glycol and carboxymethyl chitosan;

[0044] Figure 5 It is a schematic diagram of a hollow multi-fiber adsorption filler;

[0045] Among them, 1- sustained release filler, 2- micropores, 3- functional substances. DETAILED DESCRIPTION

[0046] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0047] The test method involved in the present invention is as follows:

[0048] Antibacterial test: GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method" was used to test the antibacterial properties, and the test bacteria were Escherichia coli and Staphylococcus aureus.

[0049] Formaldehyde degradation test in air (deodorization performance): refer to GB / T 15516-1995 "Determination of formaldehyde in air quality - Acetylacetone spectrophotometry", place the test sample in a transparent closed box, pass the formaldehyde into the closed box after vaporization, use a 100W high-pressure mercury lamp as the light source, measure the formaldehyde content in the box every 1 hour; calculate the formaldehyde degradation rate of the sample.

[0050] Determination of fragrance retention effect: Using the UV spectrophotometer method, the sample that has been naturally placed for a certain period of time is immersed in ethanol for extraction for 24 hours, and the absorbance at the maximum absorption wavelength is measured by the UV spectrophotometer. The absorbance corresponding to the maximum absorption wavelength is proportional to the concentration of essential oil, so this method can be used to determine the fragrance retention effect of the sample's aromatic microcapsules.

[0051] Example 1

[0052] A method for preparing a hollow porous fiber with a controllable sustained release function, the specific steps are as follows:

[0053] (1) Preparation of raw materials;

[0054] Aldehyde-containing compounds: dialdehyde-modified polyethylene glycol (molecular weight 600, Chongqing Yusi Pharmaceutical Technology Co., Ltd.);

[0055] Functional material: nanosilver with an average particle size of 5nm;

[0056] Carboxymethyl chitosan: Shanghai MacLean Biochemical Technology Co., Ltd., product number: C832672, degree of substitution: 90%;

[0057] Hollow porous fiber: polyester fiber; the hollowness of polyester fiber is 30%, the average pore size of micropores is 0.5μm, and the fiber fineness is 2dtex;

[0058] water;

[0059] Anhydrous ethanol;

[0060] (2) Preparation of precursor composite solution;

[0061] A 3wt% aqueous solution of an aldehyde-containing compound is mixed with a functional substance to obtain a precursor composite solution; the content of the functional substance in the precursor composite solution is 5wt%;

[0062] (3) Preparation of carboxymethyl chitosan solution;

[0063] Add carboxymethyl chitosan to water, stir at 36°C for 2 hours, and filter twice to obtain a carboxymethyl chitosan solution with a concentration of 5 wt% and a viscosity of 80 mPa·s;

[0064] (4) Figure 5 As shown, the hollow porous fiber is divided into two sections, A and B, with a length ratio of 1:1. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 38°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed respectively. The pressurization and vacuuming process is repeated 3 times, and the pressure difference between sections A and B is controlled to be 0.2MPa. After the reaction is completed, anhydrous ethanol cleaning and drying are performed in sequence to achieve filling of the hollow porous fiber, and a filled hollow porous fiber is obtained;

[0065] (5) The filled hollow porous fiber was immersed in a carboxymethyl chitosan solution at a bath ratio of 1:50, and then taken out and dried and cured in a vacuum drying oven at a relative vacuum pressure of -0.1 MPa and a temperature of 32°C for 60 min to obtain a hollow porous fiber with a controllable sustained release function.

[0066] like Figures 1-2 As shown, the finally prepared hollow porous fiber with controllable sustained release function includes a hollow porous fiber, the hollow porous fiber has a cavity in the axial direction, and micropores 2 connecting the cavity are evenly distributed on the cavity wall; the cavity and micropores 2 of the hollow porous fiber contain a sustained release filler 1, and functional substances 3 are evenly distributed in the sustained release filler 1; the sustained release filler is a hydrogel with Schiff base bonds obtained by the reaction of an aldehyde-containing compound and carboxymethyl chitosan (the reaction mechanism is as shown in Figure 4The hollow porous fiber with controlled sustained release function has an antibacterial rate of 99.9% against Escherichia coli and Staphylococcus aureus.

[0067] Example 2

[0068] A method for preparing a hollow porous fiber with a controllable sustained release function, the specific steps are as follows:

[0069] (1) Preparation of raw materials;

[0070] Aldehyde-containing compound: dialdehyde-modified polyethylene glycol (molecular weight 600, Chongqing Yuci Pharmaceutical Technology Co., Ltd.);

[0071] Functional material: nano titanium dioxide with an average particle size of 20nm;

[0072] Carboxymethyl chitosan: Shanghai MacLean Biochemical Technology Co., Ltd., product number: C832672, degree of substitution: 95%;

[0073] Hollow porous fiber: polyamide fiber; the hollowness of polyamide fiber is 25%, the average pore size of micropores is 0.01μm, and the fiber fineness is 15dtex;

[0074] water;

[0075] Anhydrous ethanol;

[0076] (2) Preparation of precursor composite solution;

[0077] A precursor composite solution is obtained by mixing an aldehyde-containing compound aqueous solution with a concentration of 0.5 wt % with a functional substance; the content of the functional substance in the precursor composite solution is 10 wt %;

[0078] (3) Preparation of carboxymethyl chitosan solution;

[0079] Carboxymethyl chitosan was added into water, stirred at 34°C for 4 hours, and filtered three times to obtain a carboxymethyl chitosan solution with a concentration of 1 wt% and a viscosity of 10 mPa·s;

[0080] (4) dividing the hollow porous fiber into two sections, A and B, with a length ratio of 1:1, immersing section A in a pressurized container containing a precursor composite solution and maintaining a constant temperature of 30° C., and placing section B in a vacuum container, pressurizing section A and vacuumizing section B respectively, and repeating the pressurization and vacuuming process 4 times, controlling the pressure difference between sections A and B to be 0.05 MPa. After the reaction is completed, washing with anhydrous ethanol and drying treatment are performed in sequence to achieve filling of the hollow porous fiber, thereby obtaining a filled hollow porous fiber;

[0081] (5) The filled hollow porous fiber was immersed in a carboxymethyl chitosan solution at a bath ratio of 1:65, and then taken out and dried and cured in a vacuum drying oven at a relative vacuum pressure of 0 MPa and a temperature of 26° C. for 30 min to obtain a hollow porous fiber with a controllable sustained release function.

[0082] The finally obtained hollow porous fiber with controllable sustained release function includes a hollow porous fiber, the hollow porous fiber has a cavity in the axial direction, and micropores connecting the cavity are evenly distributed on the cavity wall; the cavity and micropores of the hollow porous fiber contain a sustained release filler, and functional substances are evenly distributed in the sustained release filler; the sustained release filler is a hydrogel with Schiff base bonds obtained by the reaction of an aldehyde-containing compound and carboxymethyl chitosan; the hollow porous fiber with controllable sustained release function is tested for formaldehyde degradation in air, and the formaldehyde degradation rate is 97% after 6 hours.

[0083] Example 3

[0084] A method for preparing a hollow porous fiber with a controllable sustained release function, the specific steps are as follows:

[0085] (1) Preparation of raw materials;

[0086] Aldehyde-containing compound: oxidized sodium alginate (manufacturer: Xi'an Qiyue Biotechnology Co., Ltd., product number: Q0028341);

[0087] Functional substance: aromatic agent with an average particle size of 100 nm; the aromatic agent is an aromatic microcapsule formed by encapsulating jasmine essential oil with gelatin (manufacturer: Sinopharm Group, item number: 9000-70-8);

[0088] Carboxymethyl chitosan: Shanghai MacLean Biochemical Technology Co., Ltd., product number: C832672, degree of substitution: 92%;

[0089] Hollow porous fiber: polyacrylonitrile fiber; the hollowness of polyacrylonitrile fiber is 35%, the average pore size of micropores is 0.1μm, and the fiber fineness is 7dtex;

[0090] water;

[0091] Anhydrous ethanol;

[0092] (2) Preparation of precursor composite solution;

[0093] A 1wt% aqueous solution of an aldehyde-containing compound is mixed with a functional substance to obtain a precursor composite solution; the content of the functional substance in the precursor composite solution is 7wt%;

[0094] (3) Preparation of carboxymethyl chitosan solution;

[0095] Add carboxymethyl chitosan to water, stir at 30°C for 5 hours, and filter 4 times to obtain a carboxymethyl chitosan solution with a concentration of 3 wt% and a viscosity of 40 mPa·s;

[0096] (4) dividing the hollow porous fiber into two sections, A and B, with a length ratio of 1:1, immersing section A in a pressurized container containing a precursor composite solution and maintaining a constant temperature of 32° C., and placing section B in a vacuum container, pressurizing section A and vacuumizing section B respectively, and repeating the pressurization and vacuuming process 5 times, controlling the pressure difference between sections A and B to be 1 MPa. After the reaction is completed, washing with anhydrous ethanol and drying treatment are performed in sequence to achieve filling of the hollow porous fiber, thereby obtaining a filled hollow porous fiber;

[0097] (5) immersing the filled hollow porous fiber into a carboxymethyl chitosan solution at a bath ratio of 1:50, taking it out and drying and curing it in a vacuum drying oven at a relative vacuum pressure of -0.05 MPa and a temperature of 28° C. for 30 min to obtain a hollow porous fiber with a controllable sustained release function;

[0098] The finally obtained hollow porous fiber with controllable sustained release function comprises a hollow porous fiber, wherein the hollow porous fiber has a cavity in the axial direction, and micropores connecting the cavity are evenly distributed on the cavity wall; a sustained release filler is provided in the cavity and micropores of the hollow porous fiber, and functional substances are evenly distributed in the sustained release filler; the sustained release filler is a hydrogel with Schiff base bonds obtained by reacting an aldehyde-containing compound with carboxymethyl chitosan; the hollow porous fiber with controllable sustained release function has an initial absorbance of 0.814 at a maximum absorption wavelength of 284 nm, and an absorbance of 0.365 after being naturally placed for 6 weeks; and an absorbance of 0.731 after being naturally placed for 6 weeks and washed once (in the present invention, due to the introduction of a sustained release system containing Schiff base bonds, the fiber will be twisted and deformed during the washing process, resulting in the breaking of the Schiff base bonds, thereby causing the functional substances wrapped therein to be slowly released, causing the precipitation of aromatic essential oils, which is manifested as an increase in absorbance from the data).

[0099] Example 4

[0100] A method for preparing a hollow porous fiber with a controllable sustained release function, the specific steps are as follows:

[0101] (1) Preparation of raw materials;

[0102] Aldehyde-containing compound: oxidized sodium alginate (manufacturer: Xi'an Qiyue Biotechnology Co., Ltd., product number: Q0028341);

[0103] Functional substance: a mixture of nano cuprous oxide (average particle size 50 nm) and nano zinc (average particle size 50 nm) in a mass ratio of 1:1;

[0104] Carboxymethyl chitosan: Shanghai MacLean Biochemical Technology Co., Ltd., product number: C832672, degree of substitution: 90%;

[0105] Hollow porous fiber: polyester fiber; the hollowness of polyester fiber is 30%, the average pore size of micropores is 0.2μm, and the fiber fineness is 12dtex;

[0106] water;

[0107] Anhydrous ethanol;

[0108] (2) Preparation of precursor composite solution;

[0109] A precursor composite solution is obtained by mixing an aldehyde-containing compound aqueous solution with a concentration of 1.5 wt % with a functional substance; the content of the functional substance in the precursor composite solution is 5 wt %;

[0110] (3) Preparation of carboxymethyl chitosan solution;

[0111] Add carboxymethyl chitosan to water, stir at 32°C for 4 hours, and filter 4 times to obtain a carboxymethyl chitosan solution with a concentration of 2 wt% and a viscosity of 60 mPa·s;

[0112] (4) dividing the hollow porous fiber into two sections, A and B, with a length ratio of 1:1, immersing section A in a pressurized container containing a precursor composite solution and maintaining a constant temperature of 36° C., and placing section B in a vacuum container, pressurizing section A and vacuumizing section B respectively, and repeating the pressurization and vacuuming process 3 times, controlling the pressure difference between sections A and B to be 1.5 MPa. After the reaction is completed, washing with anhydrous ethanol and drying treatment are performed in sequence to achieve filling of the hollow porous fiber, thereby obtaining a filled hollow porous fiber;

[0113] (5) immersing the filled hollow porous fiber into a carboxymethyl chitosan solution at a bath ratio of 1:55, taking it out and drying and curing it in a vacuum drying oven at a relative vacuum pressure of -0.08 MPa and a temperature of 28° C. for 50 min to obtain a hollow porous fiber with a controllable sustained release function;

[0114] The finally obtained hollow porous fiber with controllable sustained release function comprises a hollow porous fiber, wherein the hollow porous fiber has a cavity in the axial direction, and micropores connecting the cavity are evenly distributed on the cavity wall; a sustained release filler is provided in the cavity and micropores of the hollow porous fiber, and a functional substance is evenly distributed in the sustained release filler; the sustained release filler is a hydrogel with Schiff base bonds obtained by the reaction of an aldehyde-containing compound and carboxymethyl chitosan; the hollow porous fiber with controllable sustained release function has an antibacterial rate of 98.6% against Escherichia coli and an antibacterial rate of 98.1% against Staphylococcus aureus.

[0115] Example 5

[0116] A method for preparing a hollow porous fiber with a controllable sustained release function, the specific steps are as follows:

[0117] (1) Preparation of raw materials;

[0118] Aldehyde-containing compounds: dialdehyde-modified oxidized hyaluronic acid (manufacturer: Xi'an Qiyue Biotechnology Co., Ltd., catalog number: Q0247797);

[0119] Functional material: nano-silicon dioxide with an average particle size of 60nm;

[0120] Carboxymethyl chitosan: Shanghai MacLean Biochemical Technology Co., Ltd., product number: C832672, degree of substitution: 85%;

[0121] Hollow porous fiber: polyamide fiber; the hollowness of polyamide fiber is 25%, the average pore size of micropores is 0.4μm, and the fiber fineness is 3dtex;

[0122] water;

[0123] Anhydrous ethanol;

[0124] (2) Preparation of precursor composite solution;

[0125] A 2wt% aqueous solution of an aldehyde-containing compound is mixed with a functional substance to obtain a precursor composite solution; the content of the functional substance in the precursor composite solution is 3wt%;

[0126] (3) Preparation of carboxymethyl chitosan solution;

[0127] Carboxymethyl chitosan was added into water, stirred at 36°C for 3 hours, and filtered twice to obtain a carboxymethyl chitosan solution with a concentration of 4 wt% and a viscosity of 80 mPa·s;

[0128] (4) dividing the hollow porous fiber into two sections, A and B, with a length ratio of 1:1, immersing section A in a pressurized container containing a precursor composite solution and maintaining a constant temperature of 38° C., and placing section B in a vacuum container, pressurizing section A and vacuumizing section B respectively, and repeating the pressurization and vacuuming process 4 times, controlling the pressure difference between sections A and B to be 0.25 MPa. After the reaction is completed, washing with anhydrous ethanol and drying treatment are performed in sequence to achieve filling of the hollow porous fiber, thereby obtaining a filled hollow porous fiber;

[0129] (5) immersing the filled hollow porous fiber into a carboxymethyl chitosan solution at a bath ratio of 1:60, taking it out and drying and curing it in a vacuum drying oven at a relative vacuum pressure of -0.1 MPa and a temperature of 30° C. for 60 min to obtain a hollow porous fiber with a controllable sustained release function;

[0130] The finally obtained hollow porous fiber with controllable sustained release function includes a hollow porous fiber, the hollow porous fiber has a cavity in the axial direction, and micropores connecting the cavity are evenly distributed on the cavity wall; the cavity and micropores of the hollow porous fiber contain a sustained release filler, and functional substances are evenly distributed in the sustained release filler; the sustained release filler is a hydrogel with Schiff base bonds obtained by the reaction of an aldehyde-containing compound and carboxymethyl chitosan; the hollow porous fiber with controllable sustained release function is subjected to a formaldehyde degradation test in the air, and the formaldehyde degradation rate is 94% after 6 hours.

[0131] Example 6

[0132] A method for preparing a hollow porous fiber with a controllable sustained release function, the specific steps are as follows:

[0133] (1) Preparation of raw materials;

[0134] Aldehyde-containing compounds: dialdehyde-modified oxidized hyaluronic acid (manufacturer: Xi'an Qiyue Biotechnology Co., Ltd., catalog number: Q0247797);

[0135] Functional substance: an aromatic agent with an average particle size of 80 nm, the aromatic agent is an aromatic microcapsule formed by encapsulating wormwood essential oil with sodium alginate (manufacturer: Sinopharm Group, item number: 9005-38-3);

[0136] Carboxymethyl chitosan: Shanghai MacLean Biochemical Technology Co., Ltd., product number: C832672, degree of substitution: 80%;

[0137] Hollow porous fiber: polyacrylonitrile fiber; the hollowness of the hollow porous fiber is 35%, the average pore size of the micropores is 0.3μm, and the fiber fineness is 10dtex;

[0138] water;

[0139] Anhydrous ethanol;

[0140] (2) Preparation of precursor composite solution;

[0141] A 2.5 wt% aqueous solution of an aldehyde-containing compound is mixed with a functional substance to obtain a precursor composite solution; the content of the functional substance in the precursor composite solution is 1 wt%;

[0142] (3) Preparation of carboxymethyl chitosan solution;

[0143] Add carboxymethyl chitosan to water, stir at 36°C for 2 hours, and filter three times to obtain a carboxymethyl chitosan solution with a concentration of 5 wt% and a viscosity of 100 mPa·s;

[0144] (4) dividing the hollow porous fiber into two sections, A and B, with a length ratio of 1:1, immersing section A in a pressurized container containing a precursor composite solution and maintaining a constant temperature of 40° C., and placing section B in a vacuum container, pressurizing section A and vacuumizing section B respectively, and repeating the pressurization and vacuuming process 5 times, controlling the pressure difference between sections A and B to be 0.3 MPa. After the reaction is completed, washing with anhydrous ethanol and drying treatment are performed in sequence to achieve filling of the hollow porous fiber, thereby obtaining a filled hollow porous fiber;

[0145] (5) immersing the filled hollow porous fiber into a carboxymethyl chitosan solution at a bath ratio of 1:50, taking it out and drying and curing it in a vacuum drying oven at a relative vacuum pressure of -0.1 MPa and a temperature of 32° C. for 60 min to obtain a hollow porous fiber with a controllable sustained release function;

[0146] The finally obtained hollow porous fiber with controllable sustained release function includes a hollow porous fiber, the hollow porous fiber has a cavity in the axial direction, and micropores connecting the cavity are evenly distributed on the cavity wall; the cavity and micropores of the hollow porous fiber contain a sustained release filler, and functional substances are evenly distributed in the sustained release filler; the sustained release filler is a hydrogel with Schiff base bonds obtained by the reaction of an aldehyde-containing compound and carboxymethyl chitosan; the hollow porous fiber with controllable sustained release function has an initial absorbance of 0.851 at the maximum absorption wavelength of 202nm, an absorbance of 0.451 after being naturally placed for 6 weeks, and an absorbance of 0.682 after being naturally placed for 6 weeks and washed once.

Claims

1. A hollow porous fiber with controlled sustained release function, characterized in that: The hollow porous fiber comprises a cavity in the axial direction of the hollow porous fiber, and micropores connecting the cavity are evenly distributed on the cavity wall; The hollow porous fiber has a sustained-release filler in the cavity and micropores, and the functional substance is evenly distributed in the sustained-release filler; The sustained-release filler is a hydrogel having a Schiff base bond obtained by reacting an aldehyde-containing compound with carboxymethyl chitosan; The aldehyde-containing compound is polyethylene glycol modified with a dialdehyde group, oxidized sodium alginate or oxidized hyaluronic acid.

2. The hollow porous fiber with controlled sustained release function according to claim 1, characterized in that: The functional substance is an antibacterial agent, a deodorant or a fragrance with a particle size of 5 to 100 nm.

3. The hollow porous fiber with controlled sustained release function according to claim 2, characterized in that: The antibacterial agent is one or more of nano-silver, nano-cuprous oxide and nano-zinc; The deodorant is one or more of nano titanium dioxide, nano silicon dioxide and nano bamboo charcoal; The fragrance is a fragrance microcapsule formed by encapsulating essence with a shell material, and the shell material is gelatin, sodium alginate, chitosan, gum arabic or agar.

4. The hollow porous fiber with controlled sustained release function according to claim 1, characterized in that: The hollow porous fiber is polyester fiber, polyamide fiber or polyacrylonitrile fiber; the hollowness of the hollow porous fiber is 25-35%, and the average pore size of the micropores is 0.01-0.5 μm.

5. The method for preparing a hollow porous fiber with a controllable sustained release function according to any one of claims 1 to 4, characterized in that: First, the hollow porous fiber is divided into two sections, A and B. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 30-40°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed respectively. The pressurization and vacuuming processes are repeated 3-5 times, and the pressure difference between sections A and B is controlled to be 0.05-0.3MPa. After the reaction is completed, the hollow porous fiber is washed with anhydrous ethanol and dried in sequence to achieve filling of the hollow porous fiber to obtain the filled hollow porous fiber; then the filled hollow porous fiber is immersed in a carboxymethyl chitosan solution according to a bath ratio of 1:50-65, and after being taken out, it is dried and cured in a vacuum drying oven at a relative vacuum pressure of -0.1-0MPa and a temperature of 26-32°C for 30-60min to obtain a hollow porous fiber with a controllable sustained release function; The precursor composite solution is a mixture of an aldehyde-containing compound aqueous solution and a functional substance; the concentration of the aldehyde-containing compound aqueous solution is 0.5 to 3 wt%; The content of the functional substance in the precursor composite solution is 1-10wt%.

6. The method for preparing a hollow porous fiber with a controllable sustained release function according to claim 5, characterized in that: The carboxymethyl chitosan solution is obtained by adding carboxymethyl chitosan to water, stirring at 30-36° C. for 2-5 hours, and filtering 2-4 times.

7. The method for preparing a hollow porous fiber with a controllable sustained release function according to claim 6, characterized in that: The substitution degree of carboxymethyl chitosan is ≥80%; the concentration of the carboxymethyl chitosan solution is 1-5wt%, and the viscosity is 10-100mPa·s.

8. The method for preparing a hollow porous fiber with a controllable sustained release function according to claim 7, characterized in that: The ratio of the lengths of segments A and B is 1:1.

Citation Information

Patent Citations

  • Method for preparing hollow fiber with temperature sensitive medicinal hydrogel and application thereof

    CN100540056C

  • Fibre product with slow-releasing function and its preparing method

    CN1183289C

  • Hollow fiber medicine carrier and its preparing method and use

    CN1286528C

  • Injectable temperature-sensitive drug sustained-release carrier hydrogel and preparation method thereof

    CN114042034A

  • C / SiC-HfC ceramic-based composite material and preparation method thereof

    CN115716760A