Surface modification method of waste paper fibers
By bleaching, alkalizing and carboxymethylating the waste paper pulp, the problem of reduced swelling capacity of waste paper fibers and high cost is solved, the quality and number of recycling times of waste paper recycling are improved, and cost reduction and performance are achieved promote.
Patent Information
- Application Number
- CN202410979188.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology has the problems of high cost and easy loss of reinforcing additives when improving the swelling capacity and recycling of waste paper fibers, which limits the effectiveness and quality of waste paper recycling.
By screening, bleaching, alkalizing and carboxymethylating the waste paper pulp, the carboxyl groups on the surface of the fiber are converted into carboxymethyl groups to improve the performance of the fiber, and ethanol is used for washing and drying to reduce costs.
It improves the swelling capacity of waste paper fibers and the quality of finished products, reduces the use of reinforcing additives, reduces the cost of waste paper recycling, and reduces fiber keratinization through carboxymethylation treatment, extending the number of fiber cycles. .
Smart Images

Figure CN118727484A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of papermaking, and in particular to a surface modification method for waste paper fibers. Background Art
[0002] Paper and paperboard are important necessities for human life and activities, and are also important industrial raw materials. Recycled fiber accounts for more than 60% of the total fiber raw materials for papermaking in my country. Recycling secondary fiber for papermaking not only has good economic value, but also helps to save energy and reduce emissions, protect the environment, and achieve clean production in the papermaking process.
[0003] During the pulping process, the fiber raw materials are subjected to mechanical and chemical effects, the papermaking process is subjected to drying and pressing, and the paper use process is subjected to dry heat aging and other factors, which will lead to fiber quality decay, reduced swelling ability, fiber morphology changes and other phenomena, also known as fiber keratinization; with the accelerated internal circulation of domestic waste paper and the increase in the number of cycles, the fiber keratinization phenomenon has intensified, and the quality of paper and paperboard has been greatly affected.
[0004] The commonly used method now is to use NaOH dilute solution to soak the recycled fibers to increase the fiber porosity and improve the swelling and water absorption capacity of the recycled fibers. Most of the high molecular polymers used as chemical additives contain active groups such as carboxyl, amino, and hydroxyl groups. During the addition process, the active groups are combined with the carboxyl and hydroxyl groups in the fibers to enhance the connection strength between the fibers. It is also possible that the macromolecular structure plays a "bridging role" between the fibers to facilitate the combination between the fibers.
[0005] However, aqueous solution additives are only effective at high concentrations, so the cost is relatively high; and when the recycled fiber is reused, the additives are easily lost, so this method has limitations in practical applications. Summary of the invention
[0006] The purpose of the present invention is to provide a surface modification method for waste paper fibers, which performs carboxymethylation treatment on the fibers to convert the surface carboxyl groups into carboxymethyl groups, which is not only beneficial to improving the performance of the recycled fibers and improving the product quality, but also can reduce the use of reinforcing additives and reduce the cost of waste paper recycling.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is: A surface modification method for waste paper fiber comprises the following steps: firstly, waste paper pulp is screened to obtain surface pulp, and then the surface pulp is placed in a pulp pool for bleaching; then, according to the pH of the pulp after bleaching, an alkaline solution is added to the pulp pool for alkalization treatment to obtain alkaline cellulose; after the alkalization treatment is completed, a solution containing methyl groups is continuously added to the pulp pool for etherification reaction; after the etherification reaction is completed, the pH of the surface pulp is adjusted to neutral, and cellulose containing carboxymethyl groups is obtained after washing and drying.
[0008] Optionally, the bleaching treatment of the face pulp adopts an oxidation bleaching method, and a sodium hypochlorite aqueous solution is added to the pulp pool to bleach the waste paper fibers in the face pulp.
[0009] Optionally, the alkaline solution is an ethanol aqueous solution containing sodium hydroxide.
[0010] Optionally, the alkalization treatment is carried out with heating and stirring at a temperature of 25°C to 45°C, and the reaction time is 30min to 120min.
[0011] Optionally, the solution containing methyl groups is an ethanol aqueous solution containing chloroacetic acid or TEMPO.
[0012] Optionally, the etherification reaction process is to first react the ethanol aqueous solution containing chloroacetic acid or TEMPO at 60°C to 70°C for 30 minutes, and then add the alkaline catalyst solution to carry out the etherification reaction at 60°C to 70°C for 60 minutes to 180 minutes.
[0013] Optionally, during the etherification reaction, the total mass ratio of cellulose to ethanol is 1:19-22, the total mass ratio of cellulose to water is 1:2.5-6.5, and the mass ratio of cellulose to chloroacetic acid is 1:0.8-1.6.
[0014] Optionally, adjust the pH of the batter to neutral with dilute hydrochloric acid.
[0015] Optionally, wash twice with 75% ethanol and then twice with 95% ethanol.
[0016] Optionally, drying is performed at a temperature of 60°C after washing.
[0017] Beneficial Effects
[0018] (1) In the present invention, the surface pulp separated from the waste paper pulp is subjected to carboxymethylation treatment, that is, bleaching, alkalization treatment, etherification reaction are carried out in sequence, the surface pulp is adjusted to neutrality, and then washed and dried to obtain cellulose with carboxymethyl groups; this method can convert the carboxyl groups on the fiber surface into carboxymethyl groups, which is not only beneficial to improving the performance of the recycled fiber and improving the product quality, but also can reduce the use of reinforcing additives and reduce the cost of waste paper recycling.
[0019] (2) In the present invention, ethanol is used for washing. Due to the strong volatility of ethanol, it will not remain on the fiber surface during the drying process. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the process of the present invention; Figure 2 It is a schematic diagram of the structure of the pulp fiber of the present invention for improving the bonding strength; DETAILED DESCRIPTION
[0021] The present invention will now be further described in detail with reference to the accompanying drawings and embodiments. These drawings are simplified schematic diagrams that only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.
[0022] Embodiment 1
[0023] like Figure 1-Figure 2 As shown, a surface modification method of waste paper fiber comprises the following steps: S1. Screening waste paper pulp to obtain flour pulp.
[0024] First, stir the waste paper pulp evenly to ensure that the concentration and properties of the pulp are relatively stable. Then, according to the characteristics of the waste paper pulp and the quality requirements of the required surface pulp, adjust the screen gap or screen hole size, pulp inlet pressure, rotation speed and other parameters of the pulp screening machine; then, feed the waste paper pulp into the pulp screening machine at a uniform speed. Under the action of the pulp screening machine, finer fibers (surface pulp) pass through the screen gap or screen hole, while larger impurities and coarse fibers are intercepted. Finally, the surface pulp passing through the screen gap or screen hole is collected.
[0025] S2. Place the screened dough in a slurry pool and pre-treat it.
[0026] Pretreatment includes bleaching the pulp. Oxidative bleaching is preferred here, that is, adding sodium hypochlorite aqueous solution into the pulp pool to bleach the waste paper fibers in the face pulp; sodium hypochlorite is a highly efficient oxidant that will hydrolyze in water to form hypochlorous acid and sodium hydroxide. New ecological oxygen has a strong oxidizing ability and can destroy organic pigment groups and discolor colored substances. Therefore, sodium hypochlorite is often used to bleach pulp in the papermaking industry.
[0027] S3. Alkalize the bleached flour paste.
[0028] An alkaline solution is added to the pulp tank in step S2. Since sodium hypochlorite will form hypochlorous acid and sodium hydroxide after hydrolysis in step S2, the alkaline solution here is preferably an ethanol aqueous solution containing sodium hydroxide, and then heated and stirred at a temperature of 25°C to 45°C. The reaction time is 30min to 120min to obtain alkaline cellulose.
[0029] In the alkalinization solution system, the mass ratio of cellulose to ethanol is 1:12 to 15, and the mass ratio of cellulose to water is 1:1 to 5. The total amount of sodium hydroxide is added twice. Since sodium hydroxide will be formed after the hydrolysis of sodium hypochlorite in step S2, which will change the pH of the dough, an alkaline solution needs to be added to the dough in this step according to the pH of the dough after bleaching, and the amount of sodium hydroxide added in this step is 1 / 3 of the total amount.
[0030] S4, etherifying the alkalized dough.
[0031] After the alkalization treatment is completed, the solution containing methyl groups is continuously added to the pulp pool for etherification reaction; that is, the ethanol aqueous solution of chloroacetic acid is continuously added to the pulp pool in step S3, and the temperature is raised to 60°C to 70°C for reaction for 30 minutes. The remaining 2 / 3 of the ethanol aqueous solution containing sodium hydroxide is then added as an alkaline catalyst solution, and the etherification reaction is carried out at 60°C to 70°C for 60 minutes to 180 minutes.
[0032] During the etherification reaction, the total mass ratio of cellulose to ethanol is 1:19-22, the total mass ratio of cellulose to water is 1:2.5-6.5, and the mass ratio of cellulose to chloroacetic acid is 1:0.8-1.6.
[0033] S5. Post-processing.
[0034] After the etherification reaction is completed, the pH of the paste is adjusted to neutral with dilute hydrochloric acid, filtered, and the precipitate is washed with ethanol. It can be washed twice with 75% ethanol, then washed twice with 95% ethanol, and finally dried at 60°C to obtain cellulose containing carboxymethyl.
[0035] This method uses waste paper as raw material, which has low cost and wide source; waste paper resources can be used for high added value to achieve the purpose of protecting the environment; the double alkali addition method can inhibit side reactions and product degradation and improve product substitution degree; the operation process is relatively simple; ethanol is used as the main organic solvent, which can be recycled and reused, reducing costs and reducing the complexity of subsequent processing.
[0036] After the waste paper fibers are modified, the surface properties of the fibers can be improved through the chemical and physical connections between the modified substances and the pulp fibers, thereby improving the final paper properties.
[0037] Embodiment 2
[0038] On the basis of Example 1, the solution containing methyl groups in step S4 of the present invention can also be an ethanol aqueous solution containing TEMPO.
[0039] TEMPO is the abbreviation of 2,2,6,6-tetramethylpiperidine oxide, which is a piperidine nitrogen oxide free radical and is weakly alkaline.
[0040] TEMPO oxidation can introduce hydrophilic groups such as carboxyl groups on the fiber surface, making it easier for the fiber to combine with water molecules, thereby improving the wettability and water absorption of the fiber, which helps to improve the uniformity and strength of the paper. During the production process, pulp fibers treated with TEMPO can be dispersed more quickly and evenly when mixed with water, reducing the phenomenon of fiber agglomeration and making the texture of the paper more uniform.
[0041] TEMPO oxidation increases the active groups on the fiber surface, which can promote hydrogen bonding and chemical cross-linking between fibers during the paper formation process, thereby improving the strength properties of paper, such as tensile strength, tear strength, etc. When manufacturing packaging paper, paper produced from TEMPO-treated pulp can withstand greater tensile and tearing forces, improving the reliability of packaging.
[0042] TEMPO treatment can change the charge distribution on the fiber surface, affect the electrostatic interaction of the fiber in the suspension, and thus improve the retention and drainage performance of the fiber. In the wet section of the paper machine, after appropriate TEMPO treatment, the fiber can be more effectively retained in the wire section, while increasing the dehydration speed and improving production efficiency.
[0043] TEMPO oxidation can refine the fibers to a certain extent, making the fiber shape more uniform and smaller in size, which helps to improve the smoothness and glossiness of the paper. When used for printing paper, this treatment can provide better printing effects, clearer images and brighter colors.
[0044] In addition, the introduced carboxyl and other groups make the fiber more easily react with other additives or modifiers, providing the possibility of further optimizing paper properties.
[0045] In summary, the fiber surface contains abundant carboxylic acid groups which can increase the fiber's swelling properties, improve the fiber's softness, and increase the fiber's bonding ability in the paper sheet. Carboxymethylation can reduce the fiber's keratinization to a certain extent. Therefore, if the fiber is carboxymethylated and the surface hydroxyl groups are converted into carboxymethyl groups, it will not only help to improve the performance of the recycled fiber, solve the problem of keratinization of the fiber during the recycling process that limits the number of cycles of the recycled fiber and the quality of the finished product, improve product quality, but also reduce the use of reinforcing additives and reduce the cost of recycling waste paper.
[0046] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0047] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A method for surface modification of waste paper fibers, characterized in that: First, the waste paper pulp is screened to obtain the surface pulp, and then the surface pulp is placed in a pulp tank for bleaching treatment; then, according to the pH of the pulp after bleaching, an alkaline solution is added to the pulp tank for alkalization treatment to obtain alkaline cellulose; After the alkalization treatment is completed, a solution containing methyl groups is continuously added to the pulp pool to carry out an etherification reaction. After the etherification reaction is completed, the pH of the dough is adjusted to neutral, and cellulose containing carboxymethyl groups is obtained after washing and drying.
2. The surface modification method of waste paper fiber according to claim 1, characterized in that: The bleaching treatment of the surface pulp adopts an oxidation bleaching method, in which a sodium hypochlorite aqueous solution is added to the pulp pool to bleach the waste paper fibers in the surface pulp.
3. The surface modification method of waste paper fiber according to claim 1, characterized in that: The alkaline solution is an ethanol aqueous solution containing sodium hydroxide.
4. The surface modification method of waste paper fiber according to claim 3, characterized in that: The alkalization treatment is carried out with heating and stirring at a temperature of 25°C to 45°C, and the reaction time is 30min to 120min.
5. The surface modification method of waste paper fiber according to claim 1, characterized in that: The solution with methyl groups adopts an ethanol aqueous solution containing chloroacetic acid or TEMPO.
6. The surface modification method of waste paper fiber according to claim 5, characterized in that: The process of the etherification reaction is to first react the ethanol aqueous solution containing chloroacetic acid or TEMPO at 60°C to 70°C for 30 minutes, and then add the alkaline catalyst solution to carry out the etherification reaction at 60°C to 70°C for 60min to 180min.
7. The surface modification method of waste paper fiber according to claim 6, characterized in that: During the etherification reaction, the total mass ratio of cellulose to ethanol is 1:19-22, the total mass ratio of cellulose to water is 1:2.5-6.5, and the mass ratio of cellulose to chloroacetic acid is 1:0.8-1.
6.
8. The surface modification method of waste paper fiber according to claim 1, characterized in that: Adjust the pH of the batter to neutral with dilute hydrochloric acid.
9. The surface modification method of waste paper fiber according to claim 8, characterized in that: When washing, wash twice with 75% ethanol and then wash twice with 95% ethanol.
10. The surface modification method of waste paper fiber according to claim 9, characterized in that: After washing, the fabric was dried at 60°C.
Citation Information
Patent Citations
Preparation method of carboxymethyl cellulose
CN102250256A
Preparation method for paper pulp containing multiple functional groups
CN104098704A
Method for preparing carboxymethyl cellulose by waste paper serving as raw material
CN107915783A
Method for preparing carboxymethylated nanocellulose
CN114716574A
Method for making carboxyalkyl cellulose
CN1796654A