Alkali pulping process capable of slowly releasing alkali concentration

The chemical reaction between sodium carbonate and quicklime generates sodium hydroxide, which dissolves cellulose in the early stage of low alkalinity and releases highly active alkali during high-temperature cooking. This solves the problem of cellulose degradation and causticization caused by excessive alkalinity in the traditional alkaline pulping process. It solves the problem of low efficiency, improves delignification efficiency and alkali recovery rate, and reduces production costs and environmental pollution.

CN118727486APending Publication Date: 2024-10-01SHENZHEN DEWEI INTELLIGENT MFG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411085555.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the traditional alkaline pulping process, the alkaline concentration is too high in the early stage of cooking, which leads to cellulose degradation, and the causticization rate is low, resulting in the waste of effective alkali and low delignification efficiency.

Method used

The chemical reaction between sodium carbonate and quicklime is used to generate sodium hydroxide. The low alkalinity initially dissolves active lignin and soluble hemicellulose. High-active alkali is released during high-temperature cooking to meet the demand for delignification, and the OH- in the causticizing section is controlled. Ion concentration increases causticizing rate.

Benefits of technology

It achieves effective dissolution of cellulose in the early stage of low alkalinity, prevents cellulose degradation, increases the causticization rate, reduces unnecessary consumption of alkali and environmental pollution, and reduces production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention aims to provide an alkaline pulping process capable of slowly releasing alkali concentration, which can effectively dissolve out part of active lignin and soluble hemicellulose at the initial reaction stage of plant fiber raw materials by using lower alkali concentration. The invention relates to an alkaline pulping process capable of slowly releasing alkali concentration, which comprises the following steps of: chopping or separating a plant fiber raw material, uniformly mixing sodium carbonate recovered by an alkali recovery boiler with the shredded raw material, and putting into a digester; meanwhile, according to the chemical equal-proportion reaction of the quick lime and the sodium carbonate, weighing the quick lime or the slaked lime, putting the quick lime or the slaked lime into a digester, then supplying heat energy to the plant fiber raw materials in the digester according to the ratio of the cooking liquor for high-temperature cooking, and extracting black liquor after cooking is completed. Sodium carbonate and quick lime are used for replacing traditional sodium hydroxide, and the method has the advantages that part of active lignin and soluble hemicellulose are dissolved out with the lowest effective alkali concentration, meanwhile, alkaline degradation of cellulose and effective alkali consumption caused by alkaline degradation are reduced, and the causticization procedure of a traditional alkali recovery process is omitted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking and pulping, in particular to an alkali pulping process with slow-release alkali concentration. Background Art

[0002] The traditional alkaline pulping process is to pre-treat the raw materials before putting them into the digester, and then add a cooking agent, such as sodium hydroxide, to the digester to expose the cellulose in the raw materials. In the initial stage of the reaction of the plant fiber raw materials, that is, the initial stage of cooking, some lignin and soluble hemicellulose in the raw materials have very low requirements for the alkalinity of the liquid. At this stage, only the lowest effective alkali concentration is needed to dissolve some lignin and most of the soluble hemicellulose. The alkaline concentration of the liquid in the traditional alkaline cooking is very high, which not only wastes the reaction agents, but also degrades the cellulose due to excessive alkalinity. As the cooking process proceeds, the reaction activity of the lignin in the raw materials becomes lower and lower, and the requirement for the effective alkali concentration becomes higher and higher. At this time, the causticization reaction will release more effective alkali to meet the delignification requirements. In the traditional cooking process, in the rapid delignification stage, the concentration of effective alkali decreases, and even leads to condensation of the dissolved lignin. Summary of the invention

[0003] In order to solve the above problems, the purpose of the present invention is to provide an alkali pulping process with a slow-release alkali concentration, which can effectively dissolve part of the active lignin and soluble hemicellulose at a lower alkali concentration in the early stage of the reaction of the plant fiber raw material.

[0004] The technical solution of the present invention is achieved in this way:

[0005] An alkali pulping process with slow-release alkali concentration, comprising:

[0006] The plant fiber raw materials are chopped or divided into silks, and the sodium carbonate recovered from the alkali recovery boiler is mixed evenly with the shredded raw materials and put into the digester; at the same time, according to the chemical proportional reaction of quicklime and sodium carbonate, quicklime or slaked lime is measured and put into the digester, and then the plant fiber raw materials in the digester are supplied with heat energy according to the cooking liquid ratio for high-temperature cooking, and black liquor is extracted after the cooking is completed.

[0007] Preferably, oxygen is introduced into the digester, and one or more of magnesium sulfate, magnesium hydroxide, a chelating agent, anthraquinone and a protective agent are added.

[0008] Preferably, the method further comprises replenishing sodium ions lost in the alkali recovery boiler or in the black liquor extraction process with sodium hydroxide.

[0009] Preferably, in the digester, sodium sulfide is added thereto.

[0010] Preferably, the method further comprises replenishing the sodium ions and sulfur ions lost in the alkali recovery boiler or in the black liquor extraction process with sodium sulfate.

[0011] Preferably, the cooking temperature is greater than or equal to 100° C. to 185° C., the cooking time is greater than or equal to 20 minutes, and the cooking liquid ratio is 1:2 to 1:5.

[0012] Preferably, the amount of quicklime or slaked lime used is higher than the amount chemically reacted with sodium carbonate in equal proportion, and the amount of lime exceeding the amount chemically reacted is 1% to 10% of the amount chemically reacted.

[0013] Beneficial effects of the present invention:

[0014] 1) The present invention uses sodium carbonate and quicklime to replace the traditional pulping and cooking agent sodium hydroxide. During the high-temperature cooking process, sodium carbonate will react chemically with quicklime calcium hydroxide in an aqueous solution to gradually generate the active effective ingredient sodium hydroxide that decomposes plant fibers, and the byproduct is solid calcium carbonate. Among them, fine particles of solid calcium carbonate will adhere to the fiber surface to improve certain physical properties of the fiber surface, and large particles of calcium carbonate will enter the black liquor and be extracted. One of the advantages of this method is that in the early stage of cooking when a high concentration of active alkali is not required, the effective alkali concentration is the lowest, because the causticizing process has just begun, and the lowest effective alkali concentration dissolves part of the active lignin and soluble hemicellulose, which can prevent the alkaline degradation of cellulose and the unnecessary consumption of effective alkali caused by the degradation of cellulose; while in the difficult-to-dissolve delignification stage that requires a high active alkali concentration and the highest temperature requirement, the highest concentration of active alkali is released, which just meets the optimal process conditions for delignification.

[0015] 2) In the conventional causticizing section of alkali recovery, due to the common ion effect (OH- ions generated by causticizing will hinder the progress of the causticizing process), the causticizing rate is difficult to exceed 90%, and at least 10% of the effective alkali is potentially lost and cannot participate in the delignification process. In the present invention, since the OH- ions in the digester are only one tenth to several tens of tenths of those in the conventional causticizing section, the present invention can easily increase the causticizing rate to more than 98%.

[0016] 3) In the black liquor extraction process of the pulp produced by the present invention, part of the product calcium carbonate will be mixed into the black liquor, and the calcium carbonate mixed into the black liquor will be calcined in the alkali recovery boiler to generate calcium oxide, because the decomposition temperature of calcium carbonate is not only basically consistent with the furnace temperature of the alkali recovery boiler, but also because its particles are very fine, it will be quickly calcined into calcium oxide and recovered. The recovered calcium oxide reduces the amount of lime used in the subsequent causticizing process and also reduces the amount of solid calcium carbonate discharged into the environment. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] An alkali pulping process with slow-release alkali concentration, comprising:

[0019] The plant fiber raw materials are chopped or divided into silks, the sodium carbonate recovered from the alkali recovery boiler is dissolved in water, and mixed with the shredded silk raw materials in a certain proportion, and then put into the digester; at the same time, according to the chemical reaction ratio of quicklime and sodium carbonate, the quicklime is measured and put into the digester, and then a protective agent or chelating agent is added, and then the digester is boiled at high temperature. The cooking liquid ratio is the ratio of the dry plant fiber raw materials to the liquid volume.

[0020] In the digester, oxygen is introduced, and one or more of magnesium sulfate, magnesium hydroxide, a chelating agent and a protective agent are also added.

[0021] When pulping by introducing oxygen, the sodium ions lost in the alkali recovery boiler and black liquor extraction process should be supplemented with sodium hydroxide instead of sodium sulfate.

[0022] When using the kraft pulping process, sodium sulfide is also added to the digester. Sodium sulfate is used to supplement the sodium ions and sulfur ions lost in the alkali recovery boiler or black liquor extraction process.

[0023] The cooking temperature is greater than or equal to 100° C. to 185° C., the cooking time is greater than or equal to 20 minutes, and the cooking liquid ratio is 1:2 to 1:5.

[0024] The amount of quicklime or slaked lime used is higher than the chemical reaction amount in equal proportion, and the amount of lime exceeding the chemical reaction amount is 5% to 10% of the chemical reaction amount.

[0025] In the early stage of cooking, in order to increase the causticization rate in the digester, 1% to 10% excess lime can be added. In this way, not only can the causticization rate be increased, but a small amount of excess lime (calcium hydroxide) can also easily enter the black liquor and eventually become part of the green liquor and be recovered. At the same time, calcium hydroxide will also capture sulfur ions in the boiler furnace to prevent them from escaping with the flue gas and polluting the atmosphere.

[0026] During the high-temperature cooking process, sodium carbonate reacts with quicklime and calcium oxide in aqueous solution to gradually generate sodium hydroxide that decomposes plant fibers, and the byproduct is solid calcium carbonate. Fine particles of solid calcium carbonate will adhere to the fiber surface to improve certain physical properties of the fiber surface, and large particles of calcium carbonate will enter the black liquor and be extracted.

[0027] After the cooking process is completed, high-temperature and high-concentration black liquor is extracted. Before extracting the black liquor, the cooked pulp is subjected to one or more of the following processes: debonding, knot removal, screening, and purification. The extracted black liquor can be concentrated directly or after filtering and recovering the fibers in it, and then evaporated and concentrated to a certain solid content of 30%-60%. It then enters the alkali recovery boiler to be further concentrated using the flue gas of the boiler or directly enters the boiler combustion chamber for combustion. Various combustion-supporting materials can be added or it can be directly burned without adding combustion-supporting fuel. The organic matter in the black liquor (mainly lignin and hemicellulose) is converted into heat energy for reuse, and the various organic sodium compounds therein are converted into inorganic molten sodium carbonate and discharged out of the boiler. The calcium carbonate particles therein will be efficiently (because the particles are relatively fine) calcined into calcium oxide in the high-temperature furnace, thereby reducing the amount of quicklime added during cooking. The solid calcium oxide will be taken out of the alkali recovery furnace by the molten fluid sodium carbonate and enter the dissolving tank for dissolution before entering the digester.

[0028] After the cooking step, pulping, fiber separation and screening, and pulp processing are carried out to finally produce the finished pulp, which is then stored.

[0029] The present invention describes its technical solution in detail with several embodiments.

[0030] Embodiment 1

[0031] The kraft softwood chemical pulp is produced by using a steam-heated batch cooker, with a sodium carbonate content (calculated as sodium hydroxide) of 25%, a sulfidation degree of 25%, a liquid ratio of 1:4, a cooking temperature of 170°C, a heating time of 60 minutes, a heat preservation cooking time of 120 minutes, a lime dosage (calculated as CaO) of 19%, and a pulping yield of 50%. After separating the solid calcium carbonate particles from the pulp, the pulp quality is reduced by more than 5% in hardness value compared with the traditional kraft pulp under the above conditions, but the pulping yield is increased by more than 1%.

[0032] Comparison: The same alkaline pulping process is adopted, and NaOH is used as the cooking reagent. The reaction time, reaction temperature, etc. of the whole process are the same as those in Example 1. The consumption of one ton of pulp is 500 kg calculated by sodium hydroxide (the same below), and the alkali recovery rate is increased by at least 10%. 50 kg more alkali is recovered per ton of pulp; the recovery cost per ton of alkali is reduced by 1.5 tons of steam. Therefore, the preparation process of the present invention reduces the cost for producing the same tonnage of pulp, saves the amount of steam, reduces equipment investment, has low energy consumption, discharges white mud calcium carbonate into the environment, and does not contain sodium hydroxide that is harmful to the environment.

[0033] Embodiment 2

[0034] The kraft wheat straw chemical pulp was produced by using a steam-heated batch cooker, with a sodium carbonate content (calculated as sodium hydroxide) of 14%, a sulfidation degree of 25%, a liquid ratio of 1:3, a cooking temperature of 150°C, a heating time of 120 minutes, a heat preservation cooking time of 20 minutes, a lime dosage (calculated as CaO) of 11%, and a pulping yield of 45%. After separating the solid calcium carbonate particles from the pulp, the pulping quality was 2.5% lower than the pulping hardness of the traditional kraft pulp under the above conditions, and the pulping yield was increased by 3%.

[0035] Comparison: The same alkaline pulping process is adopted, and NaOH is used as the cooking reagent. The reaction time, reaction temperature, etc. of the whole process are the same as those in Example 2. The amount of sodium hydroxide used per ton of pulp (the same below) is 311 kg, and the alkali recovery rate is increased by at least 10%. 31 kg more alkali is recovered per ton of pulp; the recovery cost of one ton of alkali is reduced by 1.5 tons of steam. Therefore, the preparation process of the present invention reduces the cost of producing the same tonnage of pulp, saves the amount of steam and the amount of plant fiber raw materials, and improves the pulp quality (reduces the lignin content and increases the fiber polymerization degree).

[0036] Embodiment 3

[0037] The sodium hydroxide oxygen process wheat straw chemical pulp was produced by using a steam-heated batch cooker, with a sodium carbonate content (calculated as sodium hydroxide) of 12%, a liquid ratio of 1:4, a cooking temperature of 125°C, a heating time of 60 minutes, a heat preservation cooking time of 120 minutes, a lime dosage (calculated as CaO) of 10%, and a pulp yield of 46%. After separating the solid calcium carbonate particles from the pulp, the pulp quality was 2.5% lower than the pulp hardness of the traditional oxygen alkali pulp under the above conditions, and the pulp yield was increased by 3%.

[0038] Comparison: The same oxygen-alkali pulping process is adopted, and NaOH is used as the cooking reagent. The reaction time, reaction temperature, etc. of the whole process are the same as those in Example 3. The amount of sodium hydroxide used per ton of pulp (the same below) is 261 kg, and the alkali recovery rate is increased by at least 10%. 26 kg more alkali is recovered per ton of pulp; the recovery cost of one ton of alkali is reduced by 1.5 tons of steam. Therefore, the preparation process of the present invention reduces the cost of producing the same tonnage of pulp, saves the amount of steam and the amount of plant fiber raw materials, and improves the pulp quality (reduces the lignin content and increases the fiber polymerization degree).

[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An alkali pulping process with a slow release of alkali concentration, characterized in that: include: The plant fiber raw materials are chopped or divided into silks, and the sodium carbonate recovered from the alkali recovery boiler is mixed evenly with the shredded raw materials and put into the digester; at the same time, according to the chemical proportional reaction of quicklime and sodium carbonate, quicklime or slaked lime is measured and put into the digester, and then the plant fiber raw materials in the digester are supplied with heat energy according to the cooking liquid ratio for high-temperature cooking, and black liquor is extracted after the cooking is completed.

2. The alkaline pulping process with slow-release alkali concentration as claimed in claim 1, characterized in that: In the digester, oxygen is introduced, and one or more of magnesium sulfate, magnesium hydroxide, a chelating agent, anthraquinone and a protective agent are also added.

3. The alkaline pulping process with slow-release alkali concentration according to claim 1, characterized in that: In the digester, sodium sulfide is added thereto.

4. The alkaline pulping process with slow-release alkali concentration according to claim 1 or 2, characterized in that: It also includes the use of sodium hydroxide to replenish the sodium ions lost in the alkali recovery boiler and black liquor extraction process.

5. The alkaline pulping process with slow-release alkali concentration according to claim 1 or 3, characterized in that: It also includes the use of sodium sulfate to replenish the sodium ions and sulfur ions lost in the alkali recovery boiler and black liquor extraction process.

6. The alkaline pulping process with slow-release alkali concentration according to claim 1, characterized in that: The cooking temperature is greater than or equal to 100° C. to 185° C., the cooking time is greater than or equal to 20 minutes, and the cooking liquid ratio is 1:2 to 1:

5.

7. The alkaline pulping process with slow-release alkali concentration according to claim 1, characterized in that: The amount of quicklime or slaked lime used is higher than the amount chemically reacted with sodium carbonate in equal proportion, and the amount of lime exceeding the amount chemically reacted is 1% to 10% of the amount chemically reacted.