High porosity gas diffusion layer carbon paper and preparation method thereof
By spraying modified carbon nanotubes, polytetrafluoroethylene and epoxy polysiloxane onto modified carbon paper in fuel cells, a high porosity gas diffusion layer carbon paper is formed, and the gas diffusion layer is solved. The corrosion problem in high humidity environments achieves higher stability and mechanical properties.
Patent Information
- Application Number
- CN202411229569.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The gas diffusion layer in the existing fuel cells is susceptible to corrosion in a high-humidity environment, affecting the stability of the battery, and it is difficult to prepare a high-porosity gas diffusion layer carbon paper with excellent mechanical properties and stable properties.
Modified carbon nanotubes, modified polytetrafluoroethylene, epoxy polysiloxane and sodium chloride were mixed and sprayed onto modified carbon paper. The high-quality reactions were formed by carbonization, graphitization, oxidation treatment and self-healing reactions. Porosity gas diffusion layer carbon paper improves its stability and mechanical properties.
The stability and mechanical properties of carbon paper with high porosity gas diffusion layer are significantly improved, the binding force with the carbon paper matrix is enhanced, the cross-linking network is formed, and the stability of porosity and current density is improved.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of fuel cells, in particular to high-porosity gas diffusion layer carbon paper and a preparation method thereof. Background Art
[0002] Energy is an indispensable resource for human beings to engage in production and life. With the increase in energy consumption, the storage capacity of traditional energy is constantly decreasing, and it is necessary to explore high-efficiency and low-pollution energy conversion methods. Fuel cells have great potential in terms of efficiency and environmental protection. Compared with traditional internal combustion engines, fuel cells can use hydrogen as fuel to reduce pollution. Fuel cells mainly include: bipolar plates, gas diffusion layers, catalyst layers, proton exchange membranes, current collectors and other components. Among them, the gas diffusion layer plays an important role in supporting the catalyst layer, conducting gas and discharging the reaction product water, but the high humidity environment inside the battery can easily lead to material corrosion and affect the stability of the battery. Therefore, it is necessary to prepare high-porosity gas diffusion layer carbon paper with excellent mechanical properties and stable performance. Summary of the invention
[0003] The object of the present invention is to provide a high-porosity gas diffusion layer carbon paper and a preparation method thereof, so as to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] The high-porosity gas diffusion layer carbon paper is obtained by spraying modified carbon nanotubes, modified polytetrafluoroethylene, epoxy polysiloxane and sodium chloride on the modified carbon paper after mixing them evenly.
[0006] As an optimization, the modified carbon nanotubes are obtained by reacting carbon nanotubes with [3-(trimethoxysilyl)propyl]succinic anhydride and N-(3-aminopropyl)diethanolamine, and then reacting with 2-chloromethylfuran.
[0007] As an optimization, the carbon nanotubes are from Shanghai Lishuo Composite Materials Technology Co., Ltd.
[0008] As an optimization, the modified polytetrafluoroethylene is obtained by reacting activated polytetrafluoroethylene with 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane and N-(2-aminoethyl)maleimide in sequence.
[0009] As an optimization, the polytetrafluoroethylene model is HH2010AFPTOK, which comes from Dongguan Tianyu Chemical Co., Ltd.
[0010] As an optimization, the modified carbon paper is obtained by wet-making short-cut polyacrylonitrile carbon fibers, followed by carbonization, graphitization, and oxidation, and then reacting with 1-aminopyrrole.
[0011] As an optimization, the chopped polyacrylonitrile carbon fiber comes from Lianyungang Rui Innovation Materials Technology Co., Ltd.
[0012] The method for preparing high-porosity gas diffusion layer carbon paper comprises the following preparation steps:
[0013] (1) The short-cut polyacrylonitrile carbon fiber is immersed in a polyethylene oxide aqueous solution with a mass fraction of 0.1-0.2%, ultrasonically dispersed for 30-40 minutes, and papered on a sheet-making machine using a wet papermaking process, and dried at 60-70°C for 2-4 hours to obtain a carbon paper blank; the carbon paper blank is immersed in a phenolic resin alcohol solution with a mass fraction of 6-8% for 20-30 minutes, hot-pressed at 120-130°C for 30-40 minutes using a flat vulcanizer, heated to 165-175°C for curing for 55-65 minutes, and placed in a high-temperature carbonization furnace, heated to 1300-1500°C at a rate of 4-6°C / min, Keep warm for 0.5-1.5h, take out after cooling naturally to room temperature, put into a high-temperature graphitization furnace, heat to 2700-2900°C at a rate of 4-6°C / min under argon atmosphere, keep warm for 55-65min, take out after cooling naturally to room temperature, and obtain graphitized carbon paper; immerse the graphitized carbon paper in the oxidation solution for 4-6min, take out, and let stand at 75-85°C for 4-5h to obtain oxidized carbon paper; immerse the oxidized carbon paper in the reaction solution for 4-6min, take out, let stand at 75-85°C for 1-3h, wash with deionized water 3-5 times, and dry at 55-65°C for 11-13h to obtain modified carbon paper;
[0014] (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:(0.4~0.6):(0.5~0.7):(0.01~0.02), stir at 75~85°C and 200~300 rpm for 4~6 hours, cool naturally to room temperature and filter, wash with chloroform and deionized water for 3~5 times respectively, and dry at 60~70°C for 8~10 hours to obtain pre-modified carbon nanotubes. ; Pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran were mixed in a mass ratio of 1:(1-2):(0.2-0.3):(4-6), stirred at 0-4°C and 100-200rpm for 1-3h in a nitrogen atmosphere, heated to 20-30°C and stirred for 9-11h, filtered, rotary evaporated at 40-50°C for 1-2h, washed with saturated sodium bicarbonate aqueous solution and deionized water for 3-5 times respectively, and dried at 70-80°C for 11-13h to obtain modified carbon nanotubes;
[0015] (3) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing the pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:(1-2):(0.4-0.5):(3-4), stirring for 4-6 hours at 85-95°C and 200-300 rpm in a nitrogen atmosphere, cooling naturally to room temperature and centrifuging, washing with acetone and deionized water for 3-5 times respectively, and drying at 55-65°C. The pre-modified polytetrafluoroethylene and dichloromethane were mixed in a mass ratio of 1:(5-7), stirred at -1-1°C and 400-500rpm for 10-20min, and N-(2-aminoethyl)maleimide in an amount 4-6 times the mass of the pre-modified polytetrafluoroethylene was added at a uniform speed within 5-6h, the mixture was heated to 20-30°C and stirred for 11-13h, then centrifuged, washed with deionized water for 3-5 times, and dried at 60-70°C for 8-10h to obtain modified polytetrafluoroethylene;
[0016] (4) Mix the modified carbon nanotubes, modified polytetrafluoroethylene and anhydrous ethanol in a mass ratio of 1:(0.2~0.3):(0.12~0.13), stir at 20~30℃ and 100~200rpm for 25~35min, then ultrasonicate for 25~35min, repeat the stirring and ultrasonicate for 2~4 times, add 0.06~0.08 times the mass of the modified carbon nanotubes epoxy polysiloxane and 0.01~0.02 times the mass of the modified carbon nanotubes sodium chloride, continue stirring for 10~20min, and spray with a spray gun. Spray it on the modified carbon paper, let it stand for 4~6 hours after spraying, move it into a tubular furnace, heat it to 240~260℃ at a rate of 4~6℃ / min, bake it for 25~35min, continue to heat it to 340~360℃ at a rate of 1~3℃ / min, sinter it for 25~35min, and then cool it to room temperature at a rate of 4~6℃ / min, immerse it in deionized water for ultrasonication for 1~2h, wash it with deionized water 3~5 times, and dry it at 65~75℃ for 8~10h to obtain a high porosity gas diffusion layer carbon paper.
[0017] As an optimization, the oxidizing solution in step (1) is obtained by mixing phosphorus pentoxide, potassium persulfate and 80% sulfuric acid solution in a mass ratio of 1:1.
[0018] As an optimization, the reaction solution in step (1) is obtained by mixing 1-aminopyrrole, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, N-hydroxysuccinimide and deionized water in a mass ratio of 1:0.5:0.4:30.
[0019] As an optimization, the reaction equation of the modified carbon paper in step (1) is:
[0020] .
[0021] As an optimization, the reaction equation of the pre-modified carbon nanotubes in step (2) is:
[0022] .
[0023] As an optimization, the reaction equation for modifying the carbon nanotubes in step (2) is:
[0024] .
[0025] As an optimization, the plasma treatment method in step (3) is: in an argon atmosphere, 35~45V for 250~350s.
[0026] As an optimization, the epoxy polysiloxane model in step (4) is LK-636, which comes from Guangzhou Longkai Chemical Co., Ltd.
[0027] As an optimization, the spraying process in step (4) is as follows: the temperature of the modified carbon paper is 80-90° C. and the spraying thickness is 40-60 μm.
[0028] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0029] When preparing high-porosity gas diffusion layer carbon paper, the present invention comprises the following steps: wet-papering short-cut polyacrylonitrile carbon fibers, followed by carbonization, graphitization and oxidation, and then reacting with 1-aminopyrrole to obtain modified carbon paper; reacting carbon nanotubes with [3-(trimethoxysilyl)propyl]succinic anhydride and N-(3-aminopropyl)diethanolamine, and then reacting with 2-chloromethylfuran to obtain modified carbon nanotubes; plasma-treating polytetrafluoroethylene, followed by reacting with 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane and N-(2-aminoethyl)maleimide to obtain modified polytetrafluoroethylene; and uniformly mixing the modified carbon nanotubes, modified polytetrafluoroethylene, epoxy polysiloxane and sodium chloride, and then spraying the mixture on the modified carbon paper to prepare high-porosity gas diffusion layer carbon paper.
[0030] Firstly, short-cut polyacrylonitrile carbon fibers are wet-papered and then carbonized, graphitized and oxidized in sequence, and then reacted with 1-aminopyrrole to obtain modified carbon paper; carbon nanotubes are reacted with [3-(trimethoxysilyl)propyl]succinic anhydride and N-(3-aminopropyl)diethanolamine and then reacted with 2-chloromethylfuran to obtain modified carbon nanotubes; 1-aminopyrrole is grafted on the carbon paper substrate to introduce pyrrole groups to participate in the self-healing reaction, increase the bonding force between the carbon paper substrate and the coating, and improve the stability of the high-porosity gas diffusion layer carbon paper; long chains containing silane groups are polymerized and grafted on the surface of the carbon nanotubes to increase the bonding effect with the carbon paper substrate and improve the stability of the high-porosity gas diffusion layer carbon paper; 2-chloromethylfuran is then grafted to introduce the furan groups participating in the self-healing reaction and form a secondary amine structure, which can react with epoxy polysiloxane to form a cross-linked network, and further improve the stability and mechanical properties of the high-porosity gas diffusion layer carbon paper.
[0031] Secondly, polytetrafluoroethylene is subjected to plasma treatment and then reacted with 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane and N-(2-aminoethyl)maleimide in sequence to obtain modified polytetrafluoroethylene; modified carbon nanotubes, modified polytetrafluoroethylene, epoxy polysiloxane and sodium chloride are evenly mixed and sprayed on modified carbon paper to prepare high-porosity gas diffusion layer carbon paper; maleic anhydride groups that can participate in self-healing reactions are introduced on polytetrafluoroethylene by grafting N-(2-aminoethyl)maleimide, and secondary amine structures that can react with epoxy polysiloxane to form a cross-linked network are formed, thereby improving the stability and mechanical properties of the high-porosity gas diffusion layer carbon paper; sodium chloride is used to make pores after curing is completed to avoid the influence of self-healing and cross-linking processes on the pore structure, thereby improving the porosity of the high-porosity gas diffusion layer carbon paper. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for preparing a high-porosity gas diffusion layer carbon paper, the method comprising the following preparation steps:
[0035] (1) The short-cut polyacrylonitrile carbon fiber was immersed in a 0.1% by mass polyethylene oxide aqueous solution, ultrasonically dispersed for 30 minutes, and papered on a sheet-making machine using a wet papermaking process. The paper was dried at 60°C for 4 hours to obtain a carbon paper blank. The carbon paper blank was immersed in a 6% by mass phenolic resin alcohol solution for 30 minutes, hot-pressed at 120°C for 40 minutes using a flat vulcanizer, heated to 165°C for curing for 65 minutes, and placed in a high-temperature carbonization furnace, heated to 1500°C at a rate of 4°C / min, and maintained at 400°C for 6 hours. The carbon paper was immersed in the oxidizing solution for 4 minutes, then taken out, and allowed to stand at 75°C for 6 hours to obtain oxidized carbon paper; the oxidized carbon paper was immersed in the reaction solution for 4 minutes, then taken out, allowed to stand at 75°C for 3 hours, washed with deionized water 3 times, and dried at 55°C for 13 hours to obtain modified carbon paper;
[0036] (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:0.4:0.5:0.01, stir at 75°C and 200 rpm for 6 h, cool naturally to room temperature and filter, wash with chloroform and deionized water three times respectively, and dry at 60°C for 10 h to obtain pre-modified carbon nanotubes; Mix pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran in a mass ratio of 1:1:0.2:4, stir at 0°C and 100 rpm for 3 h in a nitrogen atmosphere, heat to 20°C and stir for 11 h, filter, rotary evaporate at 40°C for 2 h, wash with saturated sodium bicarbonate aqueous solution and deionized water three times respectively, and dry at 70°C for 13 h to obtain modified carbon nanotubes;
[0037] (3) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:1:0.4:3, stirring at 85°C and 200 rpm for 6 hours in a nitrogen atmosphere, centrifuging after natural cooling to room temperature, washing with acetone and deionized water for 3 times respectively, and drying at 55°C for 25 hours to obtain pre-modified polytetrafluoroethylene; mixing pre-modified polytetrafluoroethylene and dichloromethane in a mass ratio of 1:5, stirring at -1°C and 400 rpm for 20 minutes, adding N-(2-aminoethyl)maleimide 6 times the mass of pre-modified polytetrafluoroethylene at a uniform rate within 5 hours, heating to 20°C and stirring for 13 hours, and then centrifuging, washing with deionized water for 3 times, and drying at 60°C for 10 hours to obtain modified polytetrafluoroethylene;
[0038] (4) The modified carbon nanotubes, modified polytetrafluoroethylene and anhydrous ethanol were mixed in a mass ratio of 1:0.2:0.12, stirred at 20°C and 100 rpm for 35 min, and then ultrasonicated for 35 min. The stirring and ultrasonication were repeated twice, and 0.06 times the mass of the modified carbon nanotubes and 0.01 times the mass of the modified carbon nanotubes were added. The stirring was continued for 20 min, and the modified carbon paper was sprayed with a spray gun. After the spraying was completed, it was allowed to stand for 6 h, and then moved into a tubular furnace, heated to 260°C at a rate of 4°C / min and baked for 25 min. The temperature was continued to be raised to 360°C at a rate of 1°C / min and sintered for 25 min. Then, it was cooled to room temperature at a rate of 4°C / min, immersed in deionized water for 1 h, ultrasonicated, washed with deionized water 3 times, and dried at 65°C for 10 h to obtain a high porosity gas diffusion layer carbon paper.
[0039] Example 2
[0040] A method for preparing a high-porosity gas diffusion layer carbon paper, the method comprising the following preparation steps:
[0041] (1) The short-cut polyacrylonitrile carbon fiber was immersed in a polyethylene oxide aqueous solution with a mass fraction of 0.15%, ultrasonically dispersed for 35 minutes, and papered on a sheet-making machine using a wet papermaking process. The paper was dried at 65°C for 3 hours to obtain a carbon paper blank. The carbon paper blank was immersed in a phenolic resin alcohol solution with a mass fraction of 7% for 25 minutes, hot-pressed at 125°C for 35 minutes using a flat vulcanizer, heated to 170°C for curing for 60 minutes, and placed in a high-temperature carbonization furnace, heated to 1400°C at a rate of 5°C / min, and maintained at 400°C for 3 hours. The carbon paper was immersed in the oxidizing solution for 5 minutes, then taken out, and allowed to stand at 80°C for 4.5 hours to obtain oxidized carbon paper. The oxidized carbon paper was immersed in the reaction solution for 5 minutes, then taken out, allowed to stand at 80°C for 2 hours, washed with deionized water 4 times, and dried at 60°C for 12 hours to obtain modified carbon paper.
[0042] (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:0.5:0.6:0.015, stir at 80°C and 250 rpm for 5 h, cool naturally to room temperature and filter, wash with chloroform and deionized water four times respectively, and dry at 65°C for 9 h to obtain pre-modified carbon nanotubes; Mix pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran in a mass ratio of 1:1.5:0.25:5, stir at 2°C and 150 rpm for 2 h in a nitrogen atmosphere, heat to 25°C and stir for 10 h, filter, rotary evaporate at 45°C for 1.5 h, wash with saturated sodium bicarbonate aqueous solution and deionized water four times respectively, and dry at 75°C for 12 h to obtain modified carbon nanotubes;
[0043] (3) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:1.5:0.45:3.5, stirring at 90°C and 250rpm for 5 hours in a nitrogen atmosphere, centrifuging after natural cooling to room temperature, washing with acetone and deionized water for 4 times respectively, and drying at 60°C for 24 hours to obtain pre-modified polytetrafluoroethylene; mixing pre-modified polytetrafluoroethylene and dichloromethane in a mass ratio of 1:6, stirring at 0°C and 450rpm for 15 minutes, adding N-(2-aminoethyl)maleimide 5 times the mass of pre-modified polytetrafluoroethylene at a uniform rate within 5.5 hours, heating to 25°C and stirring for 12 hours, centrifuging, washing with deionized water 4 times, and drying at 65°C for 9 hours to obtain modified polytetrafluoroethylene;
[0044] (4) The modified carbon nanotubes, modified polytetrafluoroethylene and anhydrous ethanol were mixed in a mass ratio of 1:0.25:0.125, stirred at 25°C and 150 rpm for 30 min, and then ultrasonicated for 30 min. The stirring and ultrasonication were repeated 3 times. 0.07 times the mass of the modified carbon nanotubes epoxy polysiloxane and 0.015 times the mass of the modified carbon nanotubes sodium chloride were added, and the stirring was continued for 15 min. The modified carbon paper was sprayed with a spray gun. After the spraying was completed, it was allowed to stand for 5 h. The mixture was moved into a tubular furnace, heated to 250°C at a rate of 5°C / min and baked for 30 min. The temperature was continued to be raised to 350°C at a rate of 2°C / min and sintered for 30 min. The mixture was then cooled to room temperature at a rate of 5°C / min. The mixture was immersed in deionized water and ultrasonicated for 1.5 h. The mixture was washed 4 times with deionized water and dried at 70°C for 9 h to obtain a high porosity gas diffusion layer carbon paper.
[0045] Example 3
[0046] A method for preparing high-porosity gas diffusion layer carbon paper, the method for preparing high-porosity gas diffusion layer carbon paper comprising the following preparation steps:
[0047] (1) The short-cut polyacrylonitrile carbon fiber was immersed in a 0.2% by mass polyethylene oxide aqueous solution, ultrasonically dispersed for 40 minutes, and papered on a sheet-making machine using a wet papermaking process. The paper was dried at 70°C for 2 hours to obtain a carbon paper blank. The carbon paper blank was immersed in an 8% by mass phenolic resin alcohol solution for 20 minutes, hot-pressed at 130°C for 30 minutes using a flat vulcanizer, heated to 175°C for curing for 55 minutes, and placed in a high-temperature carbonization furnace, heated to 1300°C at a rate of 6°C / min, and maintained at 400°C for 24 hours. The carbon paper was immersed in the oxidizing solution for 6 minutes, then taken out, and allowed to stand at 85°C for 4 hours to obtain oxidized carbon paper; the oxidized carbon paper was immersed in the reaction solution for 6 minutes, then taken out, allowed to stand at 85°C for 1 hour, washed with deionized water 5 times, and dried at 65°C for 11 hours to obtain modified carbon paper;
[0048] (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:0.6:0.7:0.02, stir at 85°C and 300 rpm for 4 hours, cool naturally to room temperature and filter, wash with chloroform and deionized water for 5 times, and dry at 70°C for 8 hours to obtain pre-modified carbon nanotubes; Mix pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran in a mass ratio of 1:2:0.3:6, stir at 4°C and 200 rpm in a nitrogen atmosphere for 1 hour, heat to 30°C and stir for 9 hours, filter, rotary evaporate at 50°C for 1 hour, wash with saturated sodium bicarbonate aqueous solution and deionized water for 5 times, and dry at 80°C for 11 hours to obtain modified carbon nanotubes;
[0049] (3) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:2:0.5:4, stirring at 95°C and 300rpm for 4 hours in a nitrogen atmosphere, centrifuging after natural cooling to room temperature, washing with acetone and deionized water for 5 times respectively, and drying at 65°C for 23 hours to obtain pre-modified polytetrafluoroethylene; mixing pre-modified polytetrafluoroethylene and dichloromethane in a mass ratio of 1:7, stirring at 1°C and 500rpm for 10 minutes, adding N-(2-aminoethyl)maleimide 4 times the mass of pre-modified polytetrafluoroethylene at a uniform rate within 6 hours, heating to 30°C and stirring for 11 hours, and then centrifuging, washing with deionized water 5 times, and drying at 70°C for 8 hours to obtain modified polytetrafluoroethylene;
[0050] (4) The modified carbon nanotubes, modified polytetrafluoroethylene and anhydrous ethanol were mixed in a mass ratio of 1:0.3:0.13, stirred at 30°C and 200 rpm for 25 min, and then ultrasonicated for 25 min. The stirring and ultrasonication were repeated 4 times. 0.08 times the mass of the modified carbon nanotubes epoxy polysiloxane and 0.02 times the mass of the modified carbon nanotubes sodium chloride were added, and the stirring was continued for 10 min. The modified carbon paper was sprayed with a spray gun. After the spraying was completed, it was allowed to stand for 4 h. The mixture was moved into a tubular furnace, heated to 240°C at a rate of 6°C / min and baked for 35 min. The temperature was continued to be raised to 340°C at a rate of 3°C / min and sintered for 35 min. The mixture was then cooled to room temperature at a rate of 6°C / min. The mixture was immersed in deionized water for 2 h and ultrasonicated. The mixture was washed with deionized water 5 times and dried at 75°C for 8 h to obtain a high porosity gas diffusion layer carbon paper.
[0051] Comparative Example 1
[0052] A method for preparing high-porosity gas diffusion layer carbon paper, the method for preparing high-porosity gas diffusion layer carbon paper comprising the following preparation steps:
[0053] (1) The short-cut polyacrylonitrile carbon fiber was immersed in a polyethylene oxide aqueous solution with a mass fraction of 0.15%, ultrasonically dispersed for 35 minutes, and papered on a sheet-making machine using a wet papermaking process, and dried at 65°C for 3 hours to obtain a carbon paper blank; the carbon paper blank was immersed in a phenolic resin alcohol solution with a mass fraction of 7% for 25 minutes, hot-pressed at 125°C for 35 minutes using a flat vulcanizer, heated to 170°C for curing for 60 minutes, placed in a high-temperature carbonization furnace, heated to 1400°C at a rate of 5°C / min, kept at this temperature for 1 hour, naturally cooled to room temperature and then taken out, placed in a high-temperature graphitization furnace, heated to 2800°C at a rate of 5°C / min in an argon atmosphere, kept at this temperature for 60 minutes, and naturally cooled to room temperature and then taken out to obtain graphitized carbon paper;
[0054] (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:0.5:0.6:0.015, stir at 80°C and 250 rpm for 5 h, cool naturally to room temperature and filter, wash with chloroform and deionized water four times respectively, and dry at 65°C for 9 h to obtain pre-modified carbon nanotubes; Mix pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran in a mass ratio of 1:1.5:0.25:5, stir at 2°C and 150 rpm for 2 h in a nitrogen atmosphere, heat to 25°C and stir for 10 h, filter, rotary evaporate at 45°C for 1.5 h, wash with saturated sodium bicarbonate aqueous solution and deionized water four times respectively, and dry at 75°C for 12 h to obtain modified carbon nanotubes;
[0055] (3) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:1.5:0.45:3.5, stirring at 90°C and 250rpm for 5 hours in a nitrogen atmosphere, centrifuging after natural cooling to room temperature, washing with acetone and deionized water for 4 times respectively, and drying at 60°C for 24 hours to obtain pre-modified polytetrafluoroethylene; mixing pre-modified polytetrafluoroethylene and dichloromethane in a mass ratio of 1:6, stirring at 0°C and 450rpm for 15 minutes, adding N-(2-aminoethyl)maleimide 5 times the mass of pre-modified polytetrafluoroethylene at a uniform rate within 5.5 hours, heating to 25°C and stirring for 12 hours, centrifuging, washing with deionized water 4 times, and drying at 65°C for 9 hours to obtain modified polytetrafluoroethylene;
[0056] (4) The modified carbon nanotubes, modified polytetrafluoroethylene and anhydrous ethanol were mixed in a mass ratio of 1:0.25:0.125, stirred at 25°C and 150 rpm for 30 min, and then ultrasonicated for 30 min. The stirring and ultrasonication were repeated 3 times. 0.07 times the mass of the modified carbon nanotubes epoxy polysiloxane and 0.015 times the mass of the modified carbon nanotubes sodium chloride were added, and the stirring was continued for 15 min. The mixture was sprayed on the graphitized carbon paper with a spray gun. After the spraying was completed, it was allowed to stand for 5 h. The mixture was moved into a tubular furnace, heated to 250°C at a rate of 5°C / min and baked for 30 min. The temperature was continued to be raised to 350°C at a rate of 2°C / min and sintered for 30 min. The mixture was then cooled to room temperature at a rate of 5°C / min. The mixture was immersed in deionized water and ultrasonicated for 1.5 h. The mixture was washed 4 times with deionized water and dried at 70°C for 9 h to obtain a high porosity gas diffusion layer carbon paper.
[0057] Comparative Example 2
[0058] A method for preparing high-porosity gas diffusion layer carbon paper, the method for preparing high-porosity gas diffusion layer carbon paper comprising the following preparation steps:
[0059] (1) The short-cut polyacrylonitrile carbon fiber was immersed in a polyethylene oxide aqueous solution with a mass fraction of 0.15%, ultrasonically dispersed for 35 minutes, and papered on a sheet-making machine using a wet papermaking process. The paper was dried at 65°C for 3 hours to obtain a carbon paper blank. The carbon paper blank was immersed in a phenolic resin alcohol solution with a mass fraction of 7% for 25 minutes, hot-pressed at 125°C for 35 minutes using a flat vulcanizer, heated to 170°C for curing for 60 minutes, and placed in a high-temperature carbonization furnace, heated to 1400°C at a rate of 5°C / min, and maintained at 400°C for 3 hours. The carbon paper was immersed in the oxidizing solution for 5 minutes, then taken out, and allowed to stand at 80°C for 4.5 hours to obtain oxidized carbon paper. The oxidized carbon paper was immersed in the reaction solution for 5 minutes, then taken out, allowed to stand at 80°C for 2 hours, washed with deionized water 4 times, and dried at 60°C for 12 hours to obtain modified carbon paper.
[0060] (2) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:1.5:0.45:3.5, stirring at 90°C and 250rpm for 5 hours in a nitrogen atmosphere, centrifuging after natural cooling to room temperature, washing with acetone and deionized water for 4 times respectively, and drying at 60°C for 24 hours to obtain pre-modified polytetrafluoroethylene; mixing pre-modified polytetrafluoroethylene and dichloromethane in a mass ratio of 1:6, stirring at 0°C and 450rpm for 15 minutes, adding N-(2-aminoethyl)maleimide 5 times the mass of pre-modified polytetrafluoroethylene at a uniform rate within 5.5 hours, heating to 25°C and stirring for 12 hours, centrifuging, washing with deionized water 4 times, and drying at 65°C for 9 hours to obtain modified polytetrafluoroethylene;
[0061] (3) CNTs, modified polytetrafluoroethylene and anhydrous ethanol were mixed in a mass ratio of 1:0.25:0.125, stirred at 25°C and 150 rpm for 30 min, then ultrasonicated for 30 min, repeated stirring and ultrasonication for 3 times, added epoxy polysiloxane (0.07 times the mass of CNTs) and sodium chloride (0.015 times the mass of CNTs), continued stirring for 15 min, sprayed on the modified carbon paper with a spray gun, allowed to stand for 5 h after spraying, moved into a tubular furnace, heated to 250°C at a rate of 5°C / min and baked for 30 min, continued to heat to 350°C at a rate of 2°C / min and sintered for 30 min, then cooled to room temperature at a rate of 5°C / min, immersed in deionized water for 1.5 h, ultrasonicated, washed 4 times with deionized water, and dried at 70°C for 9 h to obtain a high porosity gas diffusion layer carbon paper.
[0062] Comparative Example 3
[0063] A method for preparing high-porosity gas diffusion layer carbon paper, the method for preparing high-porosity gas diffusion layer carbon paper comprising the following preparation steps:
[0064] (1) The short-cut polyacrylonitrile carbon fiber was immersed in a polyethylene oxide aqueous solution with a mass fraction of 0.15%, ultrasonically dispersed for 35 minutes, and papered on a sheet-making machine using a wet papermaking process. The paper was dried at 65°C for 3 hours to obtain a carbon paper blank. The carbon paper blank was immersed in a phenolic resin alcohol solution with a mass fraction of 7% for 25 minutes, hot-pressed at 125°C for 35 minutes using a flat vulcanizer, heated to 170°C for curing for 60 minutes, and placed in a high-temperature carbonization furnace, heated to 1400°C at a rate of 5°C / min, and maintained at 400°C for 3 hours. The carbon paper was immersed in the oxidizing solution for 5 minutes, then taken out, and allowed to stand at 80°C for 4.5 hours to obtain oxidized carbon paper. The oxidized carbon paper was immersed in the reaction solution for 5 minutes, then taken out, allowed to stand at 80°C for 2 hours, washed with deionized water 4 times, and dried at 60°C for 12 hours to obtain modified carbon paper.
[0065] (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:0.5:0.6:0.015, stir at 80°C and 250 rpm for 5 h, cool naturally to room temperature and filter, wash with chloroform and deionized water four times respectively, and dry at 65°C for 9 h to obtain pre-modified carbon nanotubes; Mix pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran in a mass ratio of 1:1.5:0.25:5, stir at 2°C and 150 rpm for 2 h in a nitrogen atmosphere, heat to 25°C and stir for 10 h, filter, rotary evaporate at 45°C for 1.5 h, wash with saturated sodium bicarbonate aqueous solution and deionized water four times respectively, and dry at 75°C for 12 h to obtain modified carbon nanotubes;
[0066] (3) The modified carbon nanotubes, polytetrafluoroethylene and anhydrous ethanol were mixed in a mass ratio of 1:0.25:0.125, stirred at 25°C and 150 rpm for 30 min, and then ultrasonicated for 30 min. The stirring and ultrasonication were repeated 3 times. 0.07 times the mass of the modified carbon nanotubes epoxy polysiloxane and 0.015 times the mass of the modified carbon nanotubes sodium chloride were added, and the stirring was continued for 15 min. The modified carbon paper was sprayed with a spray gun. After the spraying was completed, it was allowed to stand for 5 h. The mixture was moved into a tubular furnace, heated to 250°C at a rate of 5°C / min and baked for 30 min. The temperature was continued to be raised to 350°C at a rate of 2°C / min and sintered for 30 min. The mixture was then cooled to room temperature at a rate of 5°C / min. The mixture was immersed in deionized water and ultrasonicated for 1.5 h. The mixture was washed with deionized water 4 times and dried at 70°C for 9 h to obtain a high porosity gas diffusion layer carbon paper.
[0067] Test Case
[0068] 1. Porosity
[0069] Test method: Take the high-porosity gas diffusion layer carbon paper obtained in each embodiment and the comparative example in size of 10 mm×10 mm, and test the porosity with a mercury intrusion instrument Autopore IV 9500 V 1.09.
[0070] 2. Mechanical properties
[0071] Test method: The high porosity gas diffusion layer carbon paper obtained in each embodiment and the comparative example were cut into sample sizes of 70 mm×10 mm, and the tensile strength was measured using a CMT4000 series tensile universal testing machine at a tensile rate of 10 mm / min.
[0072] 3. Stability
[0073] Test method: The high porosity gas diffusion layer carbon paper obtained in each embodiment and the comparative example are used as working electrodes, graphite plates as counter electrodes, and calomel as reference electrodes, respectively, and two groups of test samples are set up; one group is directly tested for the limiting current density J0 under the conditions of working temperature 80°C and humidity 100%; the other group is placed in a 0.5 mol / L sulfuric acid solution at 1.8 V for 15 hours and then tested for the limiting current density J1, and the current density loss rate = J0-J1 / J0*100% is calculated to judge the stability.
[0074] Table 1 below shows the analysis results of thermal stability, porosity and mechanical properties of high porosity gas diffusion layer carbon papers of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0075] Table 1
[0076] Porosity% Tensile strength MPa Current density loss rate% Example 1 81.5 31.1 27.6 Example 2 81.7 31.5 27.4 Example 3 81.4 31.2 27.7 Comparative Example 1 81.2 30.7 44.6 Comparative Example 2 77.7 19.1 48.9 Comparative Example 3 77.1 18.4 59.1
[0077] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the high-porosity gas diffusion layer carbon paper prepared in the present invention has good thermal stability, porosity and mechanical properties.
[0078] By comparison, the experimental data of the porosity of Examples 1 to 3 and Comparative Examples 1 to 3 show that the high-porosity gas diffusion layer carbon papers prepared by the present invention all have good pore structures, indicating that the use of sodium chloride to make pores after curing is completed avoids the influence of self-repair and cross-linking processes on the pore structure, thereby improving the porosity of the high-porosity gas diffusion layer carbon paper.
[0079] By comparison, the current density loss rate of Examples 1, 2, and 3 is lower than that of Comparative Example 1, which indicates that by grafting 1-aminopyrrole on the carbon paper substrate, pyrrole groups are introduced to participate in the self-repair reaction, thereby increasing the bonding force between the carbon paper substrate and the coating and improving the stability of the high-porosity gas diffusion layer carbon paper.
[0080] By comparison, Examples 1, 2, and 3 have higher tensile strength and lower current density loss rate than Comparative Example 2, which indicates that long chains containing silane groups are polymerized and grafted on the surface of carbon nanotubes to increase the bonding effect with the carbon paper matrix and improve the stability of the high porosity gas diffusion layer carbon paper; 2-chloromethylfuran is then grafted to introduce furan groups that participate in the self-healing reaction and form a secondary amine structure, which can react with epoxy polysiloxane to form a cross-linked network, thereby further improving the stability and mechanical properties of the high porosity gas diffusion layer carbon paper.
[0081] By comparison, Examples 1, 2, and 3 have higher tensile strength and lower current density loss rate than Comparative Example 3, indicating that by grafting N-(2-aminoethyl)maleimide onto polytetrafluoroethylene, maleic anhydride groups that can participate in the self-healing reaction are introduced, and at the same time, a secondary amine structure that can react with epoxy polysiloxane to form a cross-linked network is formed, thereby improving the stability and mechanical properties of the high-porosity gas diffusion layer carbon paper.
[0082] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. Preparation method of high porosity gas diffusion layer carbon paper, It is characterized in that The method comprises the following preparation steps: (1) The short-cut polyacrylonitrile carbon fiber was immersed in a polyethylene oxide aqueous solution with a mass fraction of 0.1-0.2%, ultrasonically dispersed for 30-40 minutes, and papered on a sheet-making machine using a wet papermaking process. The paper was dried at 60-70°C for 2-4 hours to obtain a carbon paper blank. The carbon paper blank was immersed in a phenolic resin alcohol solution with a mass fraction of 6-8% for 20-30 minutes, hot-pressed at 120-130°C for 30-40 minutes using a flat vulcanizer, heated to 165-175°C for curing for 55-65 minutes, placed in a high-temperature carbonization furnace, heated to 1300-1500°C at a rate of 4-6°C / min, kept warm for 0.5-1.5 hours, naturally cooled to room temperature, taken out, placed in a high-temperature graphitization furnace, and heated under argon. In an atmosphere, the temperature is raised to 2700-2900°C at a rate of 4-6°C / min, kept at this temperature for 55-65min, and taken out after being naturally cooled to room temperature to obtain graphitized carbon paper; the graphitized carbon paper is immersed in an oxidizing solution for 4-6min, taken out, and allowed to stand at 75-85°C for 4-5h to obtain oxidized carbon paper; 1-aminopyrrole, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, N-hydroxysuccinimide and deionized water are mixed in a mass ratio of 1:0.5:0.4:30 to obtain a reaction solution; the oxidized carbon paper is immersed in the reaction solution for 4-6min, taken out, allowed to stand at 75-85°C for 1-3h, washed with deionized water for 3-5 times, and dried at 55-65°C for 11-13h to obtain modified carbon paper; (2) Mix carbon nanotubes, [3-(trimethoxysilyl)propyl]succinic anhydride, N-(3-aminopropyl)diethanolamine and fluorobutylsulfonimide in a mass ratio of 1:(0.4-0.6):(0.5-0.7):(0.01-0.02), stir at 75-85°C and 200-300 rpm for 4-6 hours, cool naturally to room temperature and filter, wash with chloroform and deionized water for 3-5 times respectively, and dry at 60-70°C for 8-10 hours to obtain pre-modified carbon nanotubes; Pre-modified carbon nanotubes, 2-chloromethylfuran, triethylamine and tetrahydrofuran were mixed in a mass ratio of 1:(1-2):(0.2-0.3):(4-6), stirred at 0-4°C and 100-200 rpm for 1-3 h in a nitrogen atmosphere, heated to 20-30°C and stirred for 9-11 h, filtered, rotary evaporated at 40-50°C for 1-2 h, washed with saturated sodium bicarbonate aqueous solution and deionized water for 3-5 times respectively, and dried at 70-80°C for 11-13 h to obtain modified carbon nanotubes; (3) Treating polytetrafluoroethylene with a plasma processor to obtain pretreated polytetrafluoroethylene; mixing the pretreated polytetrafluoroethylene, 1-vinyl-3-chloromethyl-1,1,3,3-tetramethyldisiloxane, benzoyl peroxide and chlorobenzene in a mass ratio of 1:(1-2):(0.4-0.5):(3-4), stirring for 4-6 hours at 85-95°C and 200-300 rpm in a nitrogen atmosphere, cooling naturally to room temperature and centrifuging, washing with acetone and deionized water for 3-5 times respectively, and drying at 55-65°C. Dry for 23-25 hours to obtain pre-modified polytetrafluoroethylene; mix the pre-modified polytetrafluoroethylene and dichloromethane in a mass ratio of 1:(5-7), stir at -1-1°C and 400-500rpm for 10-20min, add N-(2-aminoethyl)maleimide 4-6 times the mass of the pre-modified polytetrafluoroethylene at a uniform speed within 5-6 hours, heat to 20-30°C, stir for 11-13 hours, then centrifuge, wash with deionized water 3-5 times, and dry at 60-70°C for 8-10 hours to obtain modified polytetrafluoroethylene; (4) Mix the modified carbon nanotubes, modified polytetrafluoroethylene and anhydrous ethanol in a mass ratio of 1:(0.2~0.3):(0.12~0.13), stir at 20~30℃ and 100~200rpm for 25~35min, then ultrasonicate for 25~35min, repeat the stirring and ultrasonicate for 2~4 times, add 0.06~0.08 times the mass of the modified carbon nanotubes epoxy polysiloxane and 0.01~0.02 times the mass of the modified carbon nanotubes sodium chloride, continue stirring for 10~20min, and spray with a spray gun. Spray it on the modified carbon paper, let it stand for 4~6 hours after spraying, move it into a tubular furnace, heat it to 240~260℃ at a rate of 4~6℃ / min, bake it for 25~35min, continue to heat it to 340~360℃ at a rate of 1~3℃ / min, sinter it for 25~35min, and then cool it to room temperature at a rate of 4~6℃ / min, immerse it in deionized water for ultrasonication for 1~2h, wash it with deionized water 3~5 times, and dry it at 65~75℃ for 8~10h to obtain a high porosity gas diffusion layer carbon paper.
2. The method for preparing the high porosity gas diffusion layer carbon paper according to claim 1, It is characterized in that The oxidizing liquid in step (1) is obtained by adding phosphorus pentoxide and potassium persulfate in a mass ratio of 1:1 into a sulfuric acid solution with a mass fraction of 80% and mixing evenly.
3. The method for preparing the high porosity gas diffusion layer carbon paper according to claim 1, It is characterized in that The reaction equation of the modified carbon paper in step (1) is: 。 4. The method for preparing the high porosity gas diffusion layer carbon paper according to claim 1, It is characterized in that The reaction equation of the pre-modified carbon nanotubes in step (2) is: 。 5. The method for preparing the high porosity gas diffusion layer carbon paper according to claim 1, It is characterized in that The plasma treatment method in step (3) is: in an argon atmosphere, 40V for 300s.
6. The method for preparing the high porosity gas diffusion layer carbon paper according to claim 1, It is characterized in that The spraying process in step (4) is as follows: the temperature of the modified carbon paper is 85° C. and the spraying thickness is 50 μm.
7. A high porosity gas diffusion layer carbon paper prepared according to the method for preparing high porosity gas diffusion layer carbon paper according to any one of claims 1 to 6.