Alkali-activated concrete salt crystallization erosion test device and test method

By designing a test device including a box, a thermohygrometer and a salinity meter, the real simulation and monitoring of alkali-induced concrete salt crystallization erosion is realized, which solves the problem that the existing test device cannot effectively observe and control alkali-induced concrete salt crystallization. process problems, improve the reliability and accuracy of test results, and prevent the deterioration of mechanical properties and durability caused by salt corrosion.

CN118730871AActive Publication Date: 2024-10-01SHANGHAI JIAOTONG UNIV

Patent Information

Application Number
CN202410741808.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

The existing test equipment cannot effectively observe and control the alkali-induced salt crystallization erosion process of concrete, especially the physical corrosion mechanism of salt crystallization. Moreover, the existing test methods have unreasonable contact methods, different dry-wet cycle patterns from the natural environment, and complex structures leading to inaccuracies. The problem of reliable results.

Method used

A test device including a box, a thermohygrometer, a salinity meter and a salt solution sealing box was designed. The alkali-stimulated concrete test strips were suspended in a semi-immersion method, and the salt solution was monitored and replenished in real time to control the relative humidity and salt solution concentration. The image recording device is used to record the apparent morphology changes of the test strip and simulate the salt crystallization process in the natural environment.

Benefits of technology

It achieves a true reflection of alkali-induced salt crystallization erosion of concrete, improves the reliability and accuracy of test results, and can effectively prevent the degradation of mechanical properties and durability caused by salt erosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118730871A_ABST
    Figure CN118730871A_ABST
Patent Text Reader

Abstract

The invention provides an alkali-activated concrete salt crystallization erosion test device and test method, the device comprises: a test mechanism, which comprises a box body, a hygrothermograph, a salinity meter and a salt solution sealing box, the box body contains a saturated salt solution and is provided with a first liquid level meter, and the first liquid level meter is provided with a water inlet and a water outlet; the salt solution sealing box is suspended in the box body, contains a corrosion salt solution and is provided with a second liquid level meter, and a sealing box water inlet is formed in the second liquid level meter; the salinity meter is used for measuring the concentration and the pH value of the saturated salt solution; the supporting mechanism comprises a horizontal rod and a suspension rope, one end of the suspension rope is connected with the horizontal rod, the alkali-activated concrete test strip is suspended and fixed at the other end of the horizontal rod, and the alkali-activated concrete test strip is inserted into the salt solution sealing box and is half soaked in the corrosive salt solution; the testing mechanism further comprises an image recording device which is used for recording the apparent morphology change of the test strip in the salt crystallization process. According to the method, the salt crystallization process of the alkali-activated concrete in a natural environment can be more truly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of civil engineering, and in particular to an alkali-induced concrete salt crystallization corrosion test device and a test method. Background Art

[0002] Alkali-activated cementitious materials are cementitious materials that are mixed with strong alkaline chemicals such as NaOH and Na2SiO3 as activators and volcanic ash active materials or potential hydraulic raw materials such as fly ash, slag, and metakaolin as matrix materials. They have stable hydration products and dense microstructures and exhibit good mechanical properties and durability. At the same time, alkali-activated cementitious materials are also regarded as green and environmentally friendly materials due to their low carbon emissions during the production process. In the context of the current global efforts to achieve the goal of "zero carbon emissions by 2050", alkali-activated cementitious materials are likely to partially or completely replace cement and become the most promising building material in the construction of concrete structures.

[0003] However, whether it is made of ordinary Portland cement or alkali-activated cementitious materials, concrete structures are easily corroded by salts in natural service environments, which leads to the production of expansive substances inside the concrete and damage, and the concrete surface becomes powdery and peeled, which ultimately affects the appearance and performance of the concrete structure. At present, there have been a lot of studies on the problem of concrete resistance to salt erosion at home and abroad, and relevant test standards and evaluation methods have been formulated. However, most of these evaluation indicators are aimed at chemical salt attack, and there are fewer studies on physical salt attack (salt crystallization).

[0004] In fact, in the natural service environment, concrete damage caused by salt crystallization is very common, and the degree of damage is far more serious than chemical erosion. Unfortunately, for a long time, people have classified salt crystallization as chemical erosion, and have not paid attention to the problem of salt crystallization in concrete. It was not until the 1990s that foreign scholars began to gradually realize the destructive effect of salt crystallization on concrete. Among them, representative foreign scholars include Carlos Rodriguez Navarro (1996), George Scherer (1999), David Benavente (2001), Robert J. Flatt (2002), Harvey Haynes (2008), Giovanni Castellazzi (2013), etc.; representative domestic scholars include Yang Quanbing (2007), Ma Kunlin (2007), Deng Dehua (2011), etc. In 2011, the American Concrete Institute officially classified salt crystallization as physical erosion. In recent years, in order to study the salt crystallization erosion of ordinary concrete and alkali-activated concrete, a series of tests have been conducted and certain results have been achieved. However, at present, there is still no unified test standard for salt crystallization erosion of alkali-activated concrete at home and abroad, and the existing test equipment / test methods have the following problems to be solved:

[0005] First, the contact mode between concrete and salt solution significantly affects the salt crystallization process. Commonly used immersion modes include full immersion, horizontal semi-immersion and vertical semi-immersion. Many tests failed to adopt reasonable immersion modes, resulting in the inability to effectively observe the salt crystallization erosion phenomenon. Second, in order to reduce the test cycle of salt crystallization erosion, dry-wet cycle accelerated tests are often used. However, the salt crystallization mode under dry-wet cycle is different from the salt crystallization mode under capillary adsorption in the natural environment, resulting in the test results being unable to reflect the real salt crystallization process. Third, some test methods require high-temperature pre-drying of concrete samples, which causes the microstructure of hydration products in concrete to shrink and produce microcracks, significantly affecting the salt crystallization process. Finally, unlike ordinary concrete, alkali-activated concrete has a very complex salt crystallization process due to its complex chemical composition, and the salt crystallization process is related to many factors such as salt type, salt concentration, ambient temperature, humidity, etc. However, many existing test devices are too complicated to safely and effectively control the above influencing factors (for example, some devices control relative humidity by injecting high pressure into the working box, which will destroy the internal structure of concrete), resulting in unreliable salt crystallization test results.

[0006] After searching, the Chinese invention patent with application publication number CN103217377A discloses a rapid determination device and method for concrete salt corrosion resistance, which aims to accelerate the corrosion process of concrete in salt solution to capture the final state after corrosion, but cannot observe the changes in the apparent state of concrete during salt erosion in real time; the device does not consider how to regulate the relative humidity in the working box, so it cannot strictly control the important influencing factors of the salt erosion process, which is ultimately not conducive to obtaining reliable test results. In addition, the device fixes the installation method and size of the concrete specimen, and the flexibility of the applicable scenarios is insufficient.

[0007] The Chinese invention patent with application publication number CN101144807A discloses a test device for concrete resistance to salt solution crystallization erosion and destruction performance. The device controls the pressure in a glass box and visually observes an external reading tube to infer the rate at which the salt solution enters the concrete. In reality, the transmission of the salt solution in concrete gradually transitions from a non-steady state to a steady state, and the test method is not accurate enough. In addition, it is necessary to inject high pressure into the glass box during the test, which is a dangerous operation. The device is too simple and does not have a corresponding safety protection mechanism. It does not take into account the concentration loss caused by the evaporation of the salt solution in the working box, which can easily cause errors in the salt crystallization test results.

[0008] The Chinese utility model patent with the authorization announcement number CN207366416U discloses a test device for the salt crystallization damage performance of concrete under dry-wet cycles, which involves high-temperature drying and rapid cooling of the test piece. This process will cause the supersaturation of the concrete pore solution to rise rapidly, increase the crystallization pressure, destroy the concrete microstructure, and affect the accuracy of the salt crystallization test; the salt crystallization process is accelerated by dry-wet cycles, but the salt crystallization pattern under dry-wet cycles is different from the salt crystallization pattern under capillary adsorption in the natural environment, so it cannot reflect the actual salt crystallization process under actual conditions. The patent requires high-temperature drying of concrete samples, which is likely to cause CSH gel shrinkage and microcracks in the concrete, thereby significantly interfering with the salt crystallization process.

[0009] In summary, there is an urgent need for a test device and a corresponding test method for salt crystallization erosion of alkali-activated concrete, so as to truly reflect the salt crystallization process of alkali-activated concrete, and thus prevent the adverse effects of deterioration of mechanical properties and durability of alkali-activated concrete due to salt erosion. Summary of the invention

[0010] In view of the defects in the prior art, the object of the present invention is to provide an alkali-induced concrete salt crystallization corrosion test device and a test method.

[0011] According to one aspect of the present invention, there is provided an alkali-induced concrete salt crystallization corrosion test device, the device comprising:

[0012] A testing mechanism, comprising a box, a thermometer and hygrometer, a salinity meter and at least one sealed box for a salt solution;

[0013] The box contains a saturated salt solution and is provided with a first liquid level gauge for measuring the liquid level of the saturated salt solution. The box is provided with a water inlet and a water outlet, and the water inlet is connected to the saturated salt solution storage device. The salt solution sealing box is suspended in the box and is located above the saturated salt solution. The salt solution sealing box contains a corrosive salt solution and is provided with a second liquid level gauge for measuring the liquid level of the corrosive salt solution. The salt solution sealing box is provided with a sealed box water inlet connected to the corrosive salt solution storage device. The thermometer and hygrometer are arranged inside the box. The salinometer is used to measure the concentration and pH value of the saturated salt solution flowing out of the water outlet.

[0014] The supporting mechanism comprises a horizontal rod and a suspension rope, wherein the horizontal rod is horizontally arranged inside the box and both ends are respectively fixedly connected to the inner wall of the box, one end of the suspension rope is connected to the horizontal rod, and the alkali-activated concrete test strip is suspended and fixed at the other end of the horizontal rod, and the alkali-activated concrete test strip is inserted into the salt solution sealing box and half immersed in the corrosive salt solution; the testing mechanism also comprises an image recording device, which is located outside the box and is used to record the apparent morphological changes of the alkali-activated concrete test strip during the salt crystallization process.

[0015] Optionally, the box body is provided with a bracket at the bottom, a mesh pad is provided above the bracket, and the salt solution sealing box is located on the mesh pad.

[0016] Optionally, paraffin is provided between the interface between the alkali-activated concrete test strip and the salt solution sealing box.

[0017] Optionally, the water outlet is connected to a water outlet valve, and the water inlet is connected to the saturated salt solution storage via a first hose, and the first hose is provided with a water inlet valve.

[0018] Optionally, the water inlet of the sealing box is connected to the corrosive salt solution storage device through a second hose, and the second hose is provided with a sealing box water inlet valve.

[0019] Optionally, a stirring device is provided below the box, and the stirring device is used to stir the saturated salt solution to keep the concentration of the saturated salt solution uniform.

[0020] According to another aspect of the present invention, there is provided an alkali-induced concrete salt crystallization corrosion test method, which is implemented using the above-mentioned device, and the method comprises:

[0021] Inject a saturated salt solution into the box and let it stand until the relative humidity in the box stabilizes and reaches the test requirement, and obtain the initial liquid level of the saturated salt solution through a first liquid level meter;

[0022] Provide alkali-activated concrete test strips in moisture equilibrium state and measure their mass;

[0023] Inject a corrosion salt solution of the required concentration value of the experiment into the salt solution sealing box, install the alkali-activated concrete test strip, make the alkali-activated concrete test strip half immersed in the corrosion salt solution, let it stand, and obtain the initial liquid level of the corrosion salt solution through the second liquid level meter;

[0024] Monitor the temperature and humidity in the box through a thermometer and hygrometer to ensure that the test requirements are met;

[0025] The liquid level of the saturated salt solution is monitored by a first liquid level meter, and the concentration change of the saturated salt solution is monitored by a salinometer, and when the liquid level or concentration changes, the saturated salt solution is replenished until the concentration and relative humidity return to an initial state;

[0026] The liquid level of the corrosive salt solution is monitored by a second liquid level gauge, and when the liquid level drops, the corrosive salt solution is replenished until the liquid level returns to an initial state;

[0027] The surface morphology changes of the alkali-activated concrete test strips during the salt crystallization process were recorded by an image recording device;

[0028] After the alkali-activated concrete test strips are immersed for a specified time, the alkali-activated concrete test strips are taken out for analysis to obtain the salt crystallization erosion test results of the alkali-activated concrete test strips.

[0029] Optionally, the length of the alkali-activated concrete test strip immersed in the corrosive salt solution accounts for 10% to 20% of the entire test strip length.

[0030] Optionally, the number of the salt solution sealed boxes is determined according to test requirements, and deionized water is injected into one of the salt solution sealed boxes to serve as a control group during the test.

[0031] Optionally, the method further comprises: retaining one of the salt solution sealed boxes, coating all sides of the alkali-activated concrete test strip therein with paraffin for waterproof sealing, not replenishing the liquid level during the test, continuously observing and recording the drop in the liquid level as the test proceeds, and calculating the capillary water absorption rate according to the following formula:

[0032]

[0033] Where h is the height of the corrosive salt solution, in meters; S is the capillary absorption rate, in meters per second. 0.5 ; t is the adsorption time, in seconds; b is the fitting parameter.

[0034] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0035] 1. The alkali-stimulated concrete salt crystallization corrosion test device provided by the present invention suspends the alkali-stimulated concrete test strips through horizontal rods and suspension ropes, realizing a semi-immersion contact mode of the alkali-stimulated concrete, which can effectively increase the corrosion rate of the salt solution; monitoring is performed through a thermometer, a salinometer, a liquid level meter, etc., and saturated salt solution and corrosive salt solution are replenished at any time during the test, which can stably control the relative humidity and the concentration of the corrosive salt solution in the test box without disturbing the state of the alkali-stimulated concrete test strips being tested. The device provided by the present invention has a simple structure, reasonable functions, simple operation and low cost. Compared with the dry-wet cycle accelerated test, the present invention can more realistically restore the salt crystallization process of alkali-stimulated concrete in a natural environment.

[0036] 2. By using the device and method provided by the present invention, various performance parameters of alkali-activated concrete after salt crystallization erosion can be obtained, which is helpful to clarify the salt crystallization mechanism and performance degradation process in concrete, thereby preventing the deterioration of mechanical properties and durability of alkali-activated concrete caused by salt erosion in actual engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0038] Figure 1 It is a schematic diagram of the structure of an alkali-induced concrete salt crystallization corrosion test device in one embodiment of the present invention;

[0039] The corresponding reference numerals in the figure are: 1-box, 2-salt solution sealing box, 3-thermohygrometer, 4-image recording device, 5-salinity meter, 6-controller, 7-saturated salt solution, 8-water outlet, 9-water outlet valve, 10-first liquid level meter, 11-water inlet, 12-saturated salt solution storage, 13-water inlet valve, 14-first hose, 15-bracket, 16-mesh pad, 17-corrosive salt solution, 18-second liquid level meter, 19-sealed box water inlet, 20-corrosive salt solution storage, 21-sealed box water inlet valve, 22-second hose, 23-alkali-activated concrete test strip, 24-paraffin, 25-data cable, 26-stirring device, 27-base, 28-horizontal rod, 29-suspension rope. DETAILED DESCRIPTION

[0040] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0041] Reference Figure 1 As shown, it is a schematic diagram of the structure of an alkali-induced concrete salt crystallization erosion test device provided in one embodiment of the present invention. The alkali-induced concrete salt crystallization erosion test device includes a test mechanism and a support mechanism, and the test mechanism includes a box 1, a thermometer and hygrometer 3, a salinity meter 5 and at least one salt solution sealing box 2; the box 1 contains a saturated salt solution 7 to stabilize the humidity in the box 1 within the experimental requirements, wherein a saturated MgCl2 solution is recommended when low humidity is required, and a saturated KCl solution is recommended when high humidity is required, and a first liquid level gauge 10 for measuring the liquid level of the saturated salt solution 7 is provided in the box 1, and a water inlet 11 and a water outlet 8 are provided on the box 1, and the water inlet 11 and the water outlet 8 are respectively located on two opposite side walls, as shown in FIG. Figure 1The bottom of the left side wall of the box body 1 is provided with a water outlet 8, and the right side wall of the box body 1 is provided with a water inlet 11. The water inlet 11 is connected with a saturated salt solution storage 12 outside the box body 1. The concentration of the saturated salt solution is supplemented by the saturated salt solution storage 12 to stabilize the relative humidity in the box body 1; the salt solution sealing box 2 is suspended in the box body 1 and is located above the saturated salt solution 7. The salt solution sealing box 2 contains a corrosive salt solution 17 and is provided with a second liquid level gauge 18 for measuring the liquid level of the corrosive salt solution 17. The corrosive salt solution 17 and the saturated salt solution 7 in the box body 1 are independent of each other and do not interfere with each other. The salt solution sealing box 2 is provided with a sealed box water inlet 19 connected with a corrosive salt solution storage 20 outside the box body 1. The concentration of the corrosive salt solution is supplemented by the corrosive salt solution storage 20 to stabilize it at the experimental set value; the thermometer and hygrometer 3 is arranged inside the box body 1 to monitor the temperature and humidity during the experiment; the salinity meter 5 is used to measure the flow from the water outlet 8. The concentration and pH value of the saturated salt solution 7 obtained are measured; the supporting mechanism includes a horizontal rod 28 and a suspension rope 29, the horizontal rod 28 and the suspension rope 29 are used to suspend and fix the tested component, namely the alkali-activated concrete test strip 23, to achieve a semi-immersion corrosion mode; specifically, the horizontal rod 28 is horizontally arranged inside the box 1 and both ends are fixedly connected to the inner wall of the box 1, one end of the suspension rope 29 is connected to the horizontal rod 28, the alkali-activated concrete test strip 23 is suspended and fixed at the other end of the horizontal rod 28, and the alkali-activated concrete test strip 23 is inserted into the salt solution sealing box 2 and semi-immersed in the corrosive salt solution 17; the testing mechanism also includes an image recording device 4, the image recording device 4 is located outside the box 1, and is used to record the apparent morphological changes of the alkali-activated concrete test strip 23 during the salt crystallization process. Since salt crystallization will cause white powdery substances to be generated on the surface of the sample, the influence of salt crystallization on the concrete surface can be intuitively reflected by observing the apparent morphological changes of the alkali-activated concrete test strip 23.

[0042] The device provided by the embodiment of the present invention suspends the alkali-activated concrete test strip 23 by means of a horizontal rod 28 and a suspension rope 29, thereby realizing a semi-immersion contact mode of the alkali-activated concrete, and can effectively improve the corrosion rate of the salt solution; through monitoring by means of a thermohygrometer 3, a salinometer 5, a liquid level meter, etc., the changes in the apparent state of the alkali-activated concrete test strip 23 during the salt erosion process can be observed in real time, and the saturated salt solution 7 and the corrosive salt solution 17 can be replenished at any time during the test, and the relative humidity and the concentration of the corrosive salt solution 17 in the box 1 can be stably controlled without disturbing the state of the alkali-activated concrete test strip 23 being tested. The device provided by the embodiment of the present invention has a simple structure, reasonable functions, simple operation and low cost. Compared with the dry-wet cycle accelerated test, the embodiment of the present invention can more realistically restore the salt crystallization process of the alkali-activated concrete in the natural environment.

[0043] To facilitate observation during the test, in some embodiments, the box 1 is a transparent box, exemplarily, a plexiglass box, and the box 1 is a sealed rectangular parallelepiped structure to facilitate the arrangement of multiple salt solution sealed boxes 2. A base 27 for supporting the box 1 is provided below the box 1 to ensure the stability of the device during the test.

[0044] In some embodiments, a bracket 15 is provided at the bottom of the box body 1, a mesh pad 16 is provided above the bracket 15, and the salt solution sealing box 2 is located on the mesh pad 16. Through the bracket 15 and the mesh pad 16, the salt solution sealing box 2 is suspended above the saturated salt solution 7 in the box body 1.

[0045] In the embodiment of the present invention, the alkali-activated concrete test strip 23 is half-immersed in the corrosive salt solution 17 by a hanging method, which can be applicable to test strips of various shapes and sizes. The alkali-activated concrete test strip 23 is pretreated before starting the salt crystallization test. For example, the test strip is placed in an environment with a humidity of 50±5% for 3 days to achieve a humidity equilibrium state. Since the pretreatment does not use a drying box to dry the test strip, it will not affect the structure of the test strip, thereby not interfering with the salt crystallization process, which is conducive to improving the reliability of the test results.

[0046] In some embodiments, paraffin 24 is provided between the interface of the alkali-activated concrete test strip 23 and the salt solution sealing box 2 to seal the gap between the test strip and the salt solution sealing box 2, so as to minimize the moisture exchange and transmission between the box 1 and the salt solution sealing box 2, which is beneficial to improve the accuracy of the test results.

[0047] In some embodiments, the water outlet 8 is connected to the water outlet valve 9, and a salinometer 5 is arranged near the water outlet 8 through the water outlet 8 and the water outlet valve 9. During the test, the saturated salt solution 7 can be sampled from the box 1 at any time and the concentration and pH value of the saturated salt solution 7 can be measured by the salinometer 5. The water inlet 11 is connected to the saturated salt solution storage 12 through the first hose 14. Exemplarily, the first hose 14 is a silicone hose, and the first hose 14 is provided with a water inlet valve 13 to facilitate the replenishment of the saturated salt solution 7 into the box 1.

[0048] In some embodiments, the sealed box water inlet 19 is connected to the corrosive salt solution storage 20 via a second hose 22 . Exemplarily, the second hose 22 is a silicone tube, and a sealed box water inlet valve 21 is provided on the second hose 22 to facilitate the replenishment of the corrosive salt solution 17 into the salt solution sealed box 2 .

[0049] Under normal circumstances, the amount of liquid level drop in the storage device and the change value of the corresponding level gauge in the salt solution box should be consistent. However, in fact, the salt solution adsorbed in the test strip may also reflux due to the concentration imbalance of the pore solution in the test strip, resulting in a slight error between the amount of supplemented salt solution and the actual amount of adsorbed salt solution. In order to accurately obtain the volume of the saturated salt solution 7 and the corrosive salt solution 17 supplemented during the test, the saturated salt solution storage device 12 and the corrosive salt solution storage device 20 are marked with high-precision scales. The scales on the storage device can assist in observing the liquid level changes and complement the level gauge. Two different means are used to monitor the liquid level changes, and the test error is controlled as much as possible, thereby improving the accuracy and reliability of the measurement results. In addition, the first level gauge 10 and the second level gauge 18 are both highly sensitive electronic water level sensors, which are conducive to improving the accuracy of the test results.

[0050] In some embodiments, a stirring device 26 is provided below the box 1, and the stirring device 26 is used to stir the saturated salt solution 7 to keep the concentration of the saturated salt solution 7 uniform. Exemplarily, the stirring device 26 is a magnetic stirrer.

[0051] In some embodiments, the image recording device 4 is a video cassette recorder (VCR), which can record the surface morphology changes of the alkali-activated concrete test strip 23 during the salt crystallization process during the experiment.

[0052] In the above embodiment, in order to meet the temperature requirement during the test, the temperature of the environment where the box 1 is located, that is, the temperature of the laboratory, can be stabilized at room temperature by controlling the indoor air-conditioning temperature to meet the requirements of the salt crystallization erosion experiment.

[0053] In order to realize automatic control of the test device, the above device also includes a controller 6. The salinometer 5, the thermometer and hygrometer 3, the image recording device 4, etc. are respectively connected to the controller 6 through a data line 25. The controller 6 can store and process relevant data observed during the salt crystallization process to reduce errors caused by manual measurement.

[0054] Based on the same inventive concept, another embodiment of the present invention provides an alkali-induced concrete salt crystallization corrosion test method implemented by the above-mentioned device, and further reference is made to Figure 1 , the method comprising:

[0055] S1. Before the test begins, inject a saturated salt solution 7 into the box 1 and let it stand for a period of time until the relative humidity in the box 1 stabilizes and reaches the test requirement, and obtain the initial liquid level of the saturated salt solution 7 through the first liquid level meter 10;

[0056] S2. Before the test, the alkali-activated concrete test strip 23 is pretreated to reach a moisture equilibrium state, and its mass is measured, recorded as m0 (kg), for calculating the mass loss rate of the alkali-activated concrete test strip 23 under the action of salt crystallization; the test strip may be cylindrical, rectangular or other shapes, and the height of the test strip is greater than 3 times the cross-sectional width or diameter. For example, the size of the test strip may be 50 mm×50 mm×150 mm;

[0057] S3, injecting a corrosive salt solution 17 of the concentration required by the experiment into the salt solution sealed box 2, installing the alkali-activated concrete test strip 23, making the alkali-activated concrete test strip 23 half-immersed in the corrosive salt solution 17, leaving it to stand for a period of time, and obtaining the initial liquid level of the corrosive salt solution 17 through the second liquid level meter 18; preferably, using paraffin 24 to treat the interface between the salt solution sealed box 2 and the alkali-activated concrete test strip 23 to minimize moisture exchange and transmission between the box 1 and the salt solution sealed box 2;

[0058] The immersion depth of the bottom of the test strip is determined according to the height of the prepared test strip. For example, the length of the alkali-activated concrete test strip 23 immersed in the corrosive salt solution 17 from the bottom accounts for about 10% to 20% of the entire test strip length. Specifically, for the above-mentioned test strip with a length of 150 mm, the bottom immersion length can be 20 mm. As a typical vertical semi-immersion contact mode, the immersion length in the embodiment of the present invention can enhance the capillary adsorption effect without affecting the evaporation rate of the specimen surface, thereby accelerating the salt crystallization corrosion test process.

[0059] S4. During the test, the temperature and humidity in the box 1 are monitored by the thermometer and hygrometer 3 to ensure that the test requirements are met;

[0060] S5. During the test, the liquid level of the saturated salt solution 7 in the box 1 is monitored by the first liquid level meter 10 to control the humidity in the box 1 to remain stable, and the concentration change of the saturated salt solution 7 is monitored by the salinity meter 5. When the liquid level or concentration changes, the saturated salt solution 7 is replenished in time until the concentration and relative humidity return to the initial state;

[0061] Specifically, during the test, the saturated salt solution 7 is sampled from the water outlet 8 at regular intervals, and the concentration change is monitored by the salinometer 5. If the liquid level or concentration decreases, the water inlet valve 13 is opened to replenish the saturated salt solution 7 until the concentration and relative humidity return to the initial state;

[0062] S6. During the test, the liquid level of the corrosive salt solution 17 in the salt solution sealing box 2 is monitored by the second liquid level meter 18. When the liquid level drops, the sealing box water inlet valve 21 is opened to replenish the corrosive salt solution 17 until the liquid level returns to the initial state;

[0063] S7, during the test, the image recording device 4 records the surface morphology changes of the alkali-activated concrete test strip 23 during the salt crystallization process;

[0064] S8. After the alkali-activated concrete test strip 23 is immersed for a specified time, the alkali-activated concrete test strip 23 is taken out for analysis to obtain the salt crystallization corrosion test result of the alkali-activated concrete test strip 23.

[0065] Specifically, the alkali-activated concrete test strip 23 is taken out, the salt crystallization state of the test strip is observed, and the mass of the test strip after the salt crystallization is measured, which is recorded as m t (kg), combined with the initial mass measured in S2, the mass loss rate of the alkali-activated concrete test strip 23 under the action of salt crystallization can be calculated. The calculation formula is:

[0066]

[0067] Where Δm is the mass loss rate of the test strip under the action of salt crystallization, and t is the capillary adsorption time or the elapsed time of the test strip immersed in the salt solution.

[0068] Furthermore, samples were taken from the test bars for XRD analysis to determine the composition of the crystallized products after salt attack, to measure the pH value and concentration of various ions in the pore solution, and to determine the pore structure and mechanical properties of the alkali-activated concrete.

[0069] In the embodiment of the present invention, the number of the salt solution sealed boxes 2 is determined according to the test requirements, and deionized water is injected into one of the salt solution sealed boxes 2 to serve as a control group during the test.

[0070] In some embodiments, the method in the above embodiment further includes: retaining one of the salt solution sealing boxes 2, coating all sides of the alkali-activated concrete test strip 23 therein with paraffin for waterproof sealing, not replenishing the liquid level during the test, continuously observing and recording the liquid level drop as the test proceeds, and calculating the capillary water absorption rate according to the following formula:

[0071]

[0072] Where h is the height of the corrosive salt solution falling, that is, the adsorption height of the corrosive salt solution in the alkali-activated concrete test strip, in meters; S is the capillary absorption rate, in meters per second. 0.5 ; t is the adsorption time, in seconds; b is the fitting parameter.

[0073] By fitting the adsorption height and time of alkali-activated concrete at different times according to the above formula, the capillary water absorption rate of the measured alkali-activated concrete strip can be calculated. According to the size of the capillary absorption rate S, it can be preliminarily judged that for alkali-activated concrete strips with the same porosity, those with larger S values ​​tend to weather on the surface of the strips, i.e., surface salt crystallization (efflorescence), while those with smaller S values ​​tend to have internal salt crystallization (subflorescence) inside the strips and near the drying front.

[0074] The device and method provided in the above-mentioned embodiments of the present invention can obtain various performance parameters of alkali-activated concrete after salt crystallization erosion, which is helpful to clarify the salt crystallization mechanism and performance degradation process in concrete, thereby preventing the deterioration of mechanical properties and durability of alkali-activated concrete caused by salt erosion in actual engineering applications.

[0075] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various modifications or variations within the scope of the claims, which does not affect the essence of the present invention. The above preferred features can be used in any combination without conflicting with each other.

Claims

1. An alkali-induced concrete salt crystallization corrosion test device, It is characterized in that include: A testing mechanism, comprising a box, a thermometer and hygrometer, a salinity meter and at least one sealed box for a salt solution; The box contains a saturated salt solution and is provided with a first liquid level gauge for measuring the liquid level of the saturated salt solution. The box is provided with a water inlet and a water outlet, and the water inlet is connected to the saturated salt solution storage device. The salt solution sealing box is suspended in the box and is located above the saturated salt solution. The salt solution sealing box contains a corrosive salt solution and is provided with a second liquid level gauge for measuring the liquid level of the corrosive salt solution. The salt solution sealing box is provided with a sealed box water inlet connected to the corrosive salt solution storage device. The thermometer and hygrometer are arranged inside the box. The salinometer is used to measure the concentration and pH value of the saturated salt solution flowing out of the water outlet. The supporting mechanism comprises a horizontal rod and a suspension rope, wherein the horizontal rod is horizontally arranged inside the box and both ends are respectively fixedly connected to the inner wall of the box, one end of the suspension rope is connected to the horizontal rod, and the alkali-activated concrete test strip is suspended and fixed at the other end of the horizontal rod, and the alkali-activated concrete test strip is inserted into the salt solution sealing box and half immersed in the corrosive salt solution; the testing mechanism also comprises an image recording device, which is located outside the box and is used to record the apparent morphological changes of the alkali-activated concrete test strip during the salt crystallization process.

2. The alkali-induced concrete salt crystallization corrosion test device according to claim 1, It is characterized in that The box body is provided with a bracket at the bottom, a mesh pad is provided above the bracket, and the salt solution sealing box is located on the mesh pad.

3. The alkali-induced concrete salt crystallization corrosion test device according to claim 1, It is characterized in that Paraffin is arranged between the interface of the alkali-activated concrete test strip and the salt solution sealing box.

4. The alkali-induced concrete salt crystallization corrosion test device according to claim 1, It is characterized in that The water outlet is connected to the water outlet valve, and the water inlet is connected to the saturated salt solution storage via a first hose, and the first hose is provided with a water inlet valve.

5. The alkali-induced concrete salt crystallization corrosion test device according to claim 1, It is characterized in that The water inlet of the sealing box is connected to the corrosive salt solution storage device through a second hose, and the second hose is provided with a water inlet valve of the sealing box.

6. The alkali-induced concrete salt crystallization corrosion test device according to claim 1, It is characterized in that A stirring device is provided below the box body, and the stirring device is used to stir the saturated salt solution to keep the concentration of the saturated salt solution uniform.

7. A method for testing alkali-induced concrete salt crystallization corrosion, implemented using the device according to any one of claims 1 to 6, It is characterized in that include: Inject a saturated salt solution into the box and let it stand until the relative humidity in the box stabilizes and reaches the test requirement, and obtain the initial liquid level of the saturated salt solution through a first liquid level meter; Provide alkali-activated concrete test strips in moisture equilibrium state and measure their mass; Inject a corrosion salt solution of the required concentration value of the experiment into the salt solution sealing box, install the alkali-activated concrete test strip, make the alkali-activated concrete test strip half immersed in the corrosion salt solution, let it stand, and obtain the initial liquid level of the corrosion salt solution through the second liquid level meter; Monitor the temperature and humidity in the box through a thermometer and hygrometer to ensure that the test requirements are met; The liquid level of the saturated salt solution is monitored by a first liquid level meter, and the concentration change of the saturated salt solution is monitored by a salinometer, and when the liquid level or concentration changes, the saturated salt solution is replenished until the concentration and relative humidity return to an initial state; The liquid level of the corrosive salt solution is monitored by a second liquid level gauge, and when the liquid level drops, the corrosive salt solution is replenished until the liquid level returns to an initial state; The surface morphology changes of the alkali-activated concrete test strips during the salt crystallization process were recorded by an image recording device; After the alkali-activated concrete test strips are immersed for a specified time, the alkali-activated concrete test strips are taken out for analysis to obtain the salt crystallization erosion test results of the alkali-activated concrete test strips.

8. The alkali-induced concrete salt crystallization corrosion test method according to claim 7, It is characterized in that The length of the alkali-activated concrete test strip immersed in the corrosive salt solution accounts for 10% to 20% of the entire test strip length.

9. The alkali-induced concrete salt crystallization corrosion test method according to claim 7, It is characterized in that The number of the salt solution sealed boxes is determined according to the test requirements, and deionized water is injected into one of the salt solution sealed boxes, which serves as a control group during the test.

10. The alkali-induced concrete salt crystallization corrosion test method according to claim 7, It is characterized in that The method also includes: retaining one of the salt solution sealed boxes, applying paraffin wax on all sides of the alkali-activated concrete test strips therein for waterproof sealing, not replenishing the liquid level during the test, continuously observing and recording the drop in the liquid level as the test proceeds, and calculating the capillary water absorption rate according to the following formula: Where h is the height of the corrosive salt solution, in meters; S is the capillary absorption rate, in meters per second. 0.5 ; t is the adsorption time, in seconds; b is the fitting parameter.

Citation Information

Patent Citations

  • Concrete salt-resistant solution physical crystal erosion destruction performance test device

    CN101144807A

  • Rapid determination device of salt corrosion resistance performance of concrete and determination method thereof

    CN103217377A

  • Salt corrosion-resisting testing device

    CN107860704A

  • Concrete semi-immersion test device

    CN110376119A

  • Method for testing sulfate corrosion resistance of tunnel lining concrete

    CN110426459A

Cited By

  • Device and method for testing water absorption characteristic of alkali-activated mortar

    CN121558555A