Ratio electrochemical aptamer sensor based on HCR signal amplification and application

By using AuNPs@Ni Co-MOF composite and HCR reaction to identify bisphenol A in the electrochemical sensor, the problems of complex operation, high cost and poor sensitivity of bisphenol A detection in the existing technology are solved, and high sensitivity and Specific test results.

CN118731124APending Publication Date: 2024-10-01SHANXI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410894174.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing bisphenol A detection technology has problems such as complex operation, high cost, and poor sensitivity. Moreover, electrochemical sensors are susceptible to signal interference, resulting in low stability and low reproducibility of detection results.

Method used

A ratiometric electrochemical aptasensor based on HCR signal amplification is used, by modifying AuNPs@Ni Co-MOF composite and ssDNA-Apt on the modified electrode, using hybridization chain reaction (HCR) and methylene blue (MB) signal amplification It will recognize bisphenol A and improve the sensitivity and specificity of detection.

Benefits of technology

It achieves highly sensitive and specific detection of bisphenol A, enhances the anti-interference ability, simplifies the detection process, reduces costs, and improves the reproducibility and reliability of detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731124A_ABST
    Figure CN118731124A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of food detection, and particularly relates to a ratio electrochemical aptamer sensor based on HCR reaction and application of the ratio electrochemical aptamer sensor. In order to improve the sensitivity and selectivity of the sensor for detecting bisphenol A, 2D Ni Co-MOF and Au NPs materials are prepared firstly, then an Au NPs and Ni Co-MOF composite material is synthesized, and then the Au NPs and Ni Co-MOF composite material is dispensed on the surface of GCE. The method comprises the following steps: dropwise coating ssDNA-Apt with a double-chain structure on the surface of a modified electrode for incubation, washing, dropwise coating an MCH solution, dropwise adding a to-be-detected sample solution to the ssDNA-Apt modified electrode on the modified electrode, and dropwise adding a DNA hairpin solution to form long double-chain DNA on the surface of the electrode; after an MB solution is dropwise added, MB can be loaded on the long double-chain structure, and electrochemical detection is carried out on BPA by measuring the peak current ratio of MB to Fc as an output signal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of food detection, and in particular relates to a ratio electrochemical aptamer sensor based on HCR signal amplification and application thereof. Background Art

[0002] Bisphenol A (BPA) is a synthetic monomer for materials such as polycarbonate resin and epoxy resin. It is widely used in the production of food packaging and medical devices such as plastic packaging bags, bottles and coated cans. Studies have shown that BPA is a typical environmental hormone compound that can cause serious environmental pollution. At the same time, BPA penetrates into food under heating and alkaline conditions, and then is absorbed by the gastrointestinal tract, interacts with a variety of biological receptors, interferes with the function of the body's endocrine system, and endangers human health. There are many analytical detection methods for BPA, such as high performance liquid chromatography (HPLC), gas chromatography (GC) and mass spectrometry (MS). These methods have the disadvantages of complex operation, high cost, time-consuming and inefficient, and poor sensitivity. In contrast, electrochemical sensors have the advantages of simple operation, low cost, and sensitive detection, and are widely used in food, environment, medicine and other fields.

[0003] In biosensing systems, it is very important to have accurate signal response intensity. Many factors can interfere with the electrochemical sensor's recognition of detection signal molecules, resulting in false negative or false positive results, leading to poor stability and low reproducibility of detection results. In order to overcome the above problems, the ratio method is introduced into electrochemical biosensor. Through its built-in correction mechanism, external interference is eliminated to a certain extent, improving the reproducibility and reliability of detection.

[0004] Metal-organic frameworks (MOFs) are one of the ideal candidate materials for the construction of electrochemical sensors. MOFs are crystalline porous materials composed of coordination bonds between metal ions or clusters and organic ligands. They have been studied in many fields due to their controllable structure and size, high porosity, and high active sites. However, traditional MOFs are generally considered to be inferior electrocatalysts due to their low conductivity and limited explosive active sites. Two-dimensional (2D) MOF materials have the characteristics of both MOFs and 2D nanomaterials. Due to their thinner 2D structure, they can provide sufficient nanoparticle anchoring sites, reduce the agglomeration of nanoparticles during the reaction, and control their content. In addition, the mass and ion transport processes are enhanced, and they have higher conductivity, overcoming the shortcomings of traditional MOFs. 2D Ni-Co MOFs have the characteristics of both MOFs and 2D nanomaterials. Their 2D structure can provide sufficient nanoparticle anchoring sites, reduce the agglomeration of nanoparticles during the reaction, and enhance the mass and ion transport processes. The synergistic effect between Ni and Co and the strong interaction in MOF nanosheets overcome the shortcomings of traditional MOFs.

[0005] However, the low conductivity of 2D MOF is still a challenge. 2D MOF has a high specific surface area of ​​nanoparticles (such as Pd, Au, Ru and Pt), which increases the conductivity and amplifies the signal. 2D MOF can also avoid the agglomeration of metal nanoparticles. Among all metal nanoparticles, gold nanoparticles (AuNPs) have excellent properties such as large specific surface area, good conductivity, easy preparation, low cost, high stability, excellent biocompatibility, and convenient surface performance. Therefore, noble metal nanoparticles with high electrochemical activity: Au NPs are introduced and composited with 2D Ni Co-MOF nanosheets, so that 2D MOF has a high specific surface area of ​​nanoparticles, which increases the conductivity and amplifies the signal, and can effectively avoid the agglomeration of AuNPs. In addition, the hybridization chain reaction (HCR) is introduced, which is an isothermal enzyme-free nucleic acid amplification technology. The principle is that the target sequence recognizes and initiates two DNA hairpins H 1 and H 2 The crossover opens to form a long double-stranded DNA, and the resulting biological structure can carry more electroactive small molecules, such as methylene blue (MB).

[0006] The ratiometric electrochemical aptamer sensor based on HCR signal amplification constructed in the present invention can realize high-sensitivity and high-specificity detection of bisphenol A, greatly enhance the anti-interference ability and detection sensitivity, and effectively solve the problem of easy signal interference in existing electrochemical detection technology. Summary of the invention

[0007] In view of the shortcomings and bottleneck problems of existing bisphenol A detection technology, the purpose of the present invention is to provide a simple, low-cost, highly sensitive and highly selective ratio electrochemical aptamer sensor based on HCR signal amplification for detecting bisphenol A.

[0008] The present invention firstly uses a simple solvothermal method and a sodium citrate reduction method to prepare 2D Ni Co-MOF and Au NPs materials respectively, and synthesizes the AuNPs@Ni Co-MOF composite material by using the principle of electrostatic adsorption, and then uses a drop coating method to modify the Au NPs@NiCo-MOF composite material on the GCE surface. ssDNA-Apt with a double-stranded structure {one end of Apt is labeled with an electroactive substance ferrocene (Fc)} is drop coated on the surface of the modified electrode for incubation, and after rinsing, MCH is drop coated to prevent non-specific binding, and then different concentrations of BPA (diluted by binding buffer) are dropped onto the ssDNA-Apt modified electrode on the modified electrode. Since Apt and BPA have a stronger affinity, BPA is detached from the electrode, and then a DNA hairpin solution (H 1 and H 2 ), ssDNA can be combined with H 1 and H 2The complementary HCR reaction is triggered to form a long double-stranded DNA on the electrode surface. After the MB solution is added, MB is loaded on the long double-stranded structure. The peak current ratio of MB and Fc (I MB / I Fc ) is used as the output signal to perform electrochemical detection of BPA. This detection method has the advantages of simple operation, fast response speed and high sensitivity.

[0009] To achieve the above object, the present invention adopts the following technical solutions:

[0010] The present invention provides a ratio electrochemical aptamer sensor based on HCR signal amplification, wherein a Pt electrode is used as a counter electrode, Ag / AgCl is used as a reference electrode, and a modified electrode is used as a working electrode, wherein the preparation of the modified electrode comprises the following steps:

[0011] Step 1, preparation of modified materials: preparation of AuNPs@Ni Co-MOF composite materials;

[0012] Step 2, preparation of modified material dispersion: dispersing the Au NPs@Ni Co-MOF composite material in a solution consisting of anhydrous ethanol and ultrapure water;

[0013] Step 3, AuNPs@Ni Co-MOF / GCE preparation: droplets of AuNPs@Ni Co-MOF composite material dispersion were applied onto the clean GCE surface, and the electrode was naturally dried;

[0014] Step 4, preparation of ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE: drop-coat the ssDNA@Fc-Apt solution on the surface of AuNPs@Ni Co-MOF / GCE, cap and incubate;

[0015] Step 5, MCH / ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE preparation: drop the MCH solution onto the surface of ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE, rinse and dry;

[0016] Step 6, preparation of modified electrode: drop bisphenol A solution of different concentrations onto the surface of MCH / ssDNA@Fc-Apt / AuNPs@NiCo-MOF / GCE, rinse and dry, then drop TNaK buffer onto the electrode surface, rinse and dry, and finally drop MB solution onto the electrode surface, rinse and dry.

[0017] Further, in step 1, the method for preparing the AuNPs@Ni Co-MOF composite material is:

[0018] Step 1.1, preparation of 2D Ni Co-MOF:

[0019] Will Co(NO 3 ) 2 6H 2 O and Ni (NO 3 ) 2 6H 2 O is completely dissolved in a mixed solution containing ultrapure water, ethanol and dimethylformamide by ultrasound; 2-methylimidazole is added to the mixed solution and completely dissolved under ultrasound; a heating reaction is performed, and after the reaction is completed, the mixture is cooled to room temperature, and the product is collected by centrifugation and alternately washed with ethanol and dried to obtain 2D NiCo-MOF;

[0020] Step 1.2, preparation of AuNPs solution:

[0021] HAuCl 4 The aqueous solution was heated vigorously to boiling; under constant temperature stirring, the sodium citrate solution was quickly added to the HAuCl 4 In aqueous solution, until the solution reaches wine red, continue to stir at a constant speed until it reaches room temperature, and then the AuNPs solution can be obtained;

[0022] Step 1.3, preparation of AuNPs@Ni Co-MOF composite material:

[0023] The 2D Ni Co-MOF was dissolved in water to obtain a 2D Ni Co-MOF aqueous solution. In a dark environment, the 2D NiCo-MOF aqueous solution was stirred with the Au NPs solution, centrifuged, washed and dried multiple times to obtain an AuNPs@Ni-Co MOF composite material.

[0024] Furthermore, in the step 1.1, the volume ratio of ultrapure water, ethanol and dimethylformamide is 10 mL: 10 mL: 10 mL, the heating reaction temperature is 160 ° C, the heating reaction time is 12 h, the drying temperature is 70 ° C, the drying time is 12 h, and the molar ratio of Ni to Co in 2D Ni Co-MOF is 0 to 0.5: 1;

[0025] In step 1.2, HAuCl 4 The mass fraction of aqueous solution is 0.01%, the mass fraction of sodium citrate solution is 1%, and the mass fraction of HAuCl 4 The volume ratio of the aqueous solution to the sodium citrate solution is 100 mL:4 mL;

[0026] In the step 1.3, the concentration of the 2D Ni Co-MOF aqueous solution is 50 mg / mL, the volume ratio of the 2D Ni Co-MOF aqueous solution to the Au NPs solution is 1 mL:0-7.5 mL, the drying temperature is 70° C., and the drying time is 6 h.

[0027] Furthermore, in step 2, the volume ratio of aqueous ethanol to ultrapure water is 700 μL:300 μL, and the mass concentration of the modified material dispersion is 0.5 mg / mL.

[0028] Furthermore, in step 4, the incubation temperature is 4° C., the time is 10 h, the molar concentration of the ssDNA@Fc-Apt solution is 2 μM, and the volume ratio of ssDNA to Fc-Apt is 3:1 to 1:3;

[0029] The sequence of the ssDNA is:

[0030] 5′-SH-TTTTTTAAAGGCCATACGCGGAACGCTATCCCACCTGAC-3′;

[0031] The sequence of the Fc-Apt is:

[0032] 5′-Fc-CCGGTGGGTGGTCAGGTGGGATAGCGTTCCGCGTATGGCCCAGCGCATCACGGGTTTCGCACCA-3′.

[0033] Further, in step 5, the molar concentration of the MCH solution is 2 mM.

[0034] Furthermore, in step 6, bisphenol A solutions of different concentrations are dripped onto the surface of MCH / ssDNA@Fc-Apt / AuNPs@NiCo-MOF / GCE and incubated for 30 to 70 minutes, TNaK buffer is dripped onto the electrode surface and incubated for 60 to 180 minutes, and methylene blue solution is dripped onto the electrode surface and incubated for 5 to 50 minutes.

[0035] Furthermore, in step 6, the molar concentration of TNaK buffer is 20 mM, pH = 7.4, and contains 2 μM H 1 , 2 μM H 2 , 20mM Tris-HCl, 140mM NaCl, 5mM KCl;

[0036] The H 1 The sequence is:

[0037] 5′-ACGCGGAACGCTATCCCACCTGACATAGCGTGGTCAGGTGGGATAG CGTTCCGCGTATGGCCCA-3′;

[0038] The H 2 The sequence is:

[0039] 5′-CACGCTATGTCAGGTGGGATAGCGTTCCGCGTTGGGCCATACGCGG AACGCTATCCCACCTGAC-3′;

[0040] The molar concentration of the MB solution was 2 nM.

[0041] The present invention also provides an application of a ratiometric electrochemical aptamer sensor based on HCR signal amplification for detecting bisphenol A, and its linear detection range is ×10 -15 M~1×10 -12 M.

[0042] Compared with the prior art, the present invention has the following advantages:

[0043] (1) This invention is the first to apply 2D Ni Co-MOF to the field of electrochemical biosensing and construct a ratiometric electrochemical aptamer sensor for detecting bisphenol A based on the HCR reaction. This method focuses on solving the shortcomings of the current bisphenol A detection method based on chromatography technology, such as cumbersome sample pretreatment process, expensive instruments, and complex operations. It enriches the application of MOF in the field of sensing and provides new ideas and methods for the construction of highly sensitive and specific AuNPs@Ni Co-MOF electrochemical biosensors.

[0044] (2) The present invention uses Au NPs@Ni Co-MOF as a modified electrode material, and the synthesized composite material has excellent electrochemical properties, and is further used as a modified electrode layer of an electrochemical biosensor for the highly sensitive and highly selective determination of BPA. Since the sheet structure of Ni Co-MOF has a large specific surface area, it can adsorb more AuNPs and prevent them from aggregating, and the composite material shows a better current response. In this sensor, Fc-labeled single-stranded DNA and MB act as signal tags. In order to improve the sensing detection performance, a hybridization chain reaction (HCR) strategy is adopted. When BPA is present, Fc-apt binds to BPA, triggering the hairpin DNA (H 1 , H 2 ) to form a longer double-stranded DNA structure, load more methylene blue (MB), and use I MB / I Fc To quantify BPA, the analytical determination of trace amounts of bisphenol A in samples is achieved, providing ideas and methods for electrochemical biosensors. The present invention can achieve high-sensitivity and high-specificity detection of bisphenol A in actual samples. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The figure is a flow chart of the preparation of the ratio electrochemical aptamer sensor based on HCR signal amplification of the present invention;

[0046] Figure 2 This is a graph showing the CV test results for different Ni addition amounts in Ni Co-MOF in Example 5;

[0047] Figure 3 This is a graph showing the CV test results of different amounts of AuNPs added to Au NPs@Ni-Co MOF in Example 5;

[0048] Figure 4 The electrophoresis experiment result diagram in Example 6;

[0049] Figure 5 CV test result diagram of different electrode modification processes in Example 7;

[0050] Figure 6 Graph showing the EIS test results of different electrode modification processes in Example 7;

[0051] Figure 7 This is a graph showing the DPV test results of ssDNA and Fc-Apt at different volume ratios in Example 8;

[0052] Figure 8 This is a graph showing the DPV test results for different BPA incubation times in Example 9;

[0053] Fig. 9 This is a graph showing the DPV test results for different HCR incubation times in Example 10;

[0054] Fig.10 This is a graph showing the DPV test results for different MB incubation times in Example 11;

[0055] Fig.11 A standard curve is drawn for the current value of the electrochemical sensor in Example 12 versus the logarithmic value of the BPA concentration;

[0056] Fig.12 is the linear equation of the fluorescence response value of the electrochemical sensor and the BPA concentration in Example 12;

[0057] Fig.13 This is a graph showing the specificity experimental results of the electrochemical sensor in Example 13. DETAILED DESCRIPTION

[0058] In order to further illustrate the technical solution of the present invention, the present invention is further described below through embodiments.

[0059] Example 1

[0060] like Figure 1 As shown, a method for preparing a ratio electrochemical aptamer sensor based on HCR signal amplification in this embodiment includes the following steps:

[0061] Step 1, preparation of modified materials: preparation of AuNPs@Ni Co-MOF composite materials, the specific steps are as follows:

[0062] Step 1.1, preparation of 2D Ni Co-MOF:

[0063] 1.323 mmol Co(NO 3 ) 2 6H 2 O and 0.397mmol Ni(NO 3 ) 2 6H 2 O was completely dissolved in a mixed solution containing 10 mL of ultrapure water, 10 mL of ethanol and 10 mL of dimethylformamide (DMF) by ultrasound; 0.2504 g of 2-methylimidazole (2-MI) was added to the mixed solution and completely dissolved under ultrasound; it was moved to a 50 mL stainless steel autoclave lined with Teflon and heated in an oven at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, and the product was collected by centrifugation and washed alternately with ethanol three times and dried to obtain a pale purple powder 2D Ni Co-MOF. The molar ratio of Ni to Co in the 2D Ni Co-MOF was 0.3:1, and the total metal molar amount was 1.72 mmol.

[0064] Step 1.2, prepare AuNPs solution by sodium citrate reduction method:

[0065] HAuCl purchased from Shanghai Aladdin Co., Ltd. 4 Dilute to a mass fraction of 0.01% HAuCl 4 The aqueous solution was heated vigorously to boiling; 4 mL of 1% sodium citrate solution was quickly added to the HAuCl solution under constant temperature stirring. 4 The aqueous solution was stirred at a constant temperature for 10 min until the solution reached wine red color, and then the stirring was continued at a constant speed until the solution reached room temperature to obtain the AuNPs solution. The volume was adjusted to 100 mL and the solution was transferred to a brown bottle and stored at 4°C for use.

[0066] Step 1.3, preparation of AuNPs@Ni Co-MOF composite material:

[0067] 2D Ni Co-MOF was dissolved in water to obtain a 50 mg / mL 2D Ni Co-MOF aqueous solution; in a dark environment, 1 mL of the 2D Ni Co-MOF aqueous solution was stirred with 2.5 mL of AuNPs solution for 15 h, centrifuged and washed multiple times, and dried at 70 °C for 6 h to obtain an AuNPs@Ni-Co MOF composite material.

[0068] Step 2, preparation of modified material dispersion: 0.5 mg Au NPs@Ni Co-MOF composite material was placed in a centrifuge tube, 700 μL anhydrous ethanol and 300 μL ultrapure water were added, and ultrasonic dispersion was performed for 20 min to obtain 0.5 mg / mL Au NPs@Ni-Co MOF dispersion.

[0069] Step 3, preparation of AuNPs@Ni Co-MOF / GCE: a drop of AuNPs@Ni Co-MOF composite material dispersion is applied to a clean GCE surface, and the electrode is dried naturally, specifically comprising the following steps:

[0070] Step 3.1: Sprinkle a small amount of aluminum oxide polishing powder on the suede, wet the suede with distilled water, rinse the electrode surface with ultrapure water after polishing, and then add 5mM Fe(CN) 6 3+ / 4+ Measure CV and control it at 80-100mV.

[0071] In step 3.2, 8 μL of the prepared 0.5 mg / mL AuNPs@Ni-Co MOF dispersion was pipetted and drop-coated on the polished GCE electrode surface and dried naturally to obtain the AuNPs@Ni-Co MOF modified electrode.

[0072] Step 4, preparation of ssDNA@Fc-Apt / Au NPs@Ni Co-MOF / GCE: 8 μL of 2 μM ssDNA@Fc-Apt solution was drop-coated on the surface of AuNPs@Ni Co-MOF / GCE, capped and incubated at 4 °C for 10 h, and the unbound ssDNA@Fc-Apt on the surface was washed with TNaK buffer;

[0073] The specific steps for preparing 2μM ssDNA@Fc-Apt are as follows:

[0074] (1) Prepare 4 μM ssDNA using 50 nM TNaK buffer (containing 2.0 mM TCEP);

[0075] (2) Prepare 4 μM Fc-Apt using 50 nM TNaK buffer;

[0076] (3) ssDNA and Fc-Apt were prepared in a volume ratio of 1:3 to 3:1, mixed, incubated at 37°C for 30 min, and then transferred to a refrigerator and incubated in the dark at 4°C for 1 h.

[0077] Step 5, preparation of MCH / ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE: 8 μL of 2 mM MCH solution was dropped onto the surface of ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE for 30 min, rinsed and dried.

[0078] Step 6, preparation of modified electrode: different concentrations of bisphenol A solution (diluted by binding buffer) were dropped onto the surface of MCH / ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE and incubated for 30-70 min, rinsed and dried, and then 8 μL of TNaK buffer (20 mM, pH = 7.4, containing 2 μM H 1 , 2 μM H 2 , 20mM Tris-HCl, 140mM NaCl, 5mM KCl) was dropped onto the electrode surface and incubated for 60-180min (HCR incubation), rinsed and dried, and finally 8μL 2nM methylene blue solution was dropped onto the electrode surface and incubated for 5-50min, rinsed and dried.

[0079] Step 7, preparation of the sensor: using a Pt electrode as a counter electrode, Ag / AgCl as a reference electrode, and a modified electrode as a working electrode, an electrochemical biosensor for bisphenol A detection was prepared.

[0080] Example 2

[0081] The difference from Example 1 is:

[0082] Step 1.1, preparation of 2D Ni Co-MOF:

[0083] 1.6381mmol Co(NO 3 ) 2 6H 2 O and 0.0819mmol Ni(NO 3 ) 2 6H 2 O was completely dissolved in a mixed solution containing 10 mL of ultrapure water, 10 mL of ethanol and 10 mL of dimethylformamide (DMF) by ultrasound; 0.2504 g of 2-methylimidazole (2-MI) was added to the mixed solution and completely dissolved under ultrasound; it was moved to a 50 mL stainless steel autoclave lined with Teflon and heated in an oven at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, and the product was collected by centrifugation and washed alternately with ethanol three times and dried to obtain a pale purple powder 2D Ni Co-MOF, in which the molar ratio of Ni to Co in the 2D Ni Co-MOF was 0.05:1, and the total metal molar amount was 1.72 mmol.

[0084] Step 1.3, preparation of AuNPs@Ni Co-MOF composite material:

[0085] 2D Ni Co-MOF was dissolved in water to obtain a 50 mg / mL 2D Ni Co-MOF aqueous solution; in a dark environment, 1 mL of the 2D Ni Co-MOF aqueous solution was stirred with 5 mL of AuNPs solution for 15 h, centrifuged and washed multiple times, and dried at 70 °C for 6 h to obtain an AuNPs@Ni-Co MOF composite material.

[0086] Example 3

[0087] The difference from Example 1 is:

[0088] Step 1.1, preparation of 2D Ni Co-MOF:

[0089] 1.72 mmol Co(NO 3 ) 2 6H 2 O and 0mmol Ni(NO 3 ) 2 6H 2 O was completely dissolved in a mixed solution containing 10 mL of ultrapure water, 10 mL of ethanol and 10 mL of dimethylformamide (DMF) by ultrasound; 0.2504 g of 2-methylimidazole (2-MI) was added to the mixed solution and completely dissolved under ultrasound; it was moved to a 50 mL stainless steel autoclave lined with Teflon and heated in an oven at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, and the product was collected by centrifugation and washed alternately with ethanol three times and dried to obtain a pale purple powder 2D Ni Co-MOF, in which the molar ratio of Ni to Co in the 2D Ni Co-MOF was 0:1, and the total metal molar amount was 1.72 mmol.

[0090] Step 1.3, preparation of AuNPs@Ni Co-MOF composite material:

[0091] 2D Ni Co-MOF was dissolved in water to obtain a 50 mg / mL 2D Ni Co-MOF aqueous solution; in a dark environment, 1 mL of the 2D Ni Co-MOF aqueous solution was stirred with 0 mL of AuNPs solution for 15 h, centrifuged and washed multiple times, and dried at 70 °C for 6 h to obtain an AuNPs@Ni-Co MOF composite material.

[0092] Example 4

[0093] The difference from Example 1 is:

[0094] Step 1.1, preparation of 2D Ni Co-MOF:

[0095] 0.573 mmol Co(NO 3 ) 2 6H 2 O and 1.147mmol Ni(NO 3 ) 2 6H 2 O was completely dissolved in a mixed solution containing 10 mL of ultrapure water, 10 mL of ethanol and 10 mL of dimethylformamide (DMF) by ultrasound; 0.2504 g of 2-methylimidazole (2-MI) was added to the mixed solution and completely dissolved under ultrasound; it was moved to a 50 mL stainless steel autoclave lined with Teflon and heated in an oven at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, and the product was collected by centrifugation and washed alternately with ethanol three times and dried to obtain a pale purple powder 2D Ni Co-MOF, in which the molar ratio of Ni to Co was 0.5:1 and the total metal molar amount was 1.72 mmol.

[0096] Step 1.3, preparation of AuNPs@Ni Co-MOF composite material:

[0097] 2D Ni Co-MOF was dissolved in water to obtain a 50 mg / mL 2D Ni Co-MOF aqueous solution; in a dark environment, 1 mL of the 2D Ni Co-MOF aqueous solution was stirred with 7.5 mL of AuNPs solution for 15 h, centrifuged and washed multiple times, and dried at 70 °C for 6 h to obtain an AuNPs@Ni-Co MOF composite material.

[0098] In the above Examples 1 to 4, the sequence of the ssDNA is: 5′-SH-TTTTTTAAAGGCCATACGCGGAACGCTATCCCACCTGAC-3′; the sequence of the Fc-Apt is: 5′-Fc-CCGGT GGGTGGTCAGGTGGGATAGCGTTCCGCGTATGGCCCAGCGCATCACGGGT TCGCACCA-3′; the H 1 The sequence is: 5′-ACGCGGAACGCTATCCCACCTGAC ATAGCTGGTCAGGTGGGATAGCGTTCCGCGTATGGCCCA-3′; H 2 The sequence is: 5′-CACGCTATGTCAGGTGGGATAGCGTTCCGCGTTGGGCCATACGCGGAAC GCTATCCCACCTGAC-3′.

[0099] Example 5

[0100] In a Chenhua CHI 830D electrochemical workstation, a three-electrode system consisting of a platinum electrode as a counter electrode, an Ag / AgCl electrode as a reference electrode, and a modified Au NPs@Ni-Co MOF / GCE electrode as a working electrode was used to test the different addition amounts of Ni in Ni Co-MOF and the addition amounts of Au NPs in Au NPs@Ni-Co MOF. The electrolyte was a 0.1 M PBS (pH 7.4) buffer solution containing 5 mM [Fe(CN) 6 ] 3- / 4- and 0.1M KCl solution. At -200~600mV; scanning rate: 50mV·s -1 . Through CV test results ( Figure 2 ) showed that when the addition amount of Ni in Ni Co-MOF was 30%, the Ni Co-MOF / GCE electrode showed a high current response; when the addition amount of Au NPs was 2.5mL, the AuNPs@Ni Co-MOF / GCE electrode showed a high current response ( Figure 3 ).

[0101] Example 6

[0102] The HCR reaction of steps 4 to 6 in Example 1 was subjected to agarose gel electrophoresis experiment:

[0103] The HCR reactions from step 4 to step 6 were incubated in a centrifuge tube for agarose gel electrophoresis. The results showed that ( Figure 4 Band a: SH-ssDNA; Band b: Fc-Apt; Band c: SH-ssDNA+Fc-Apt; Band d: H 1 ; Band e: H 2 ; Band F: H 1 +H 2 ; Band g: ssDNA+Fc-Apt+H 1 +H 2 ; Band h: ssDNA+Fc-Apt+H 1 +H 2 + BPA), when BPA is absent, the hairpin DNA structure H 1 , H 2 It cannot be opened, HCR is interrupted, and only short SH-ssDNA@Fc-Apt double strands exist; when BPA is present, Fc-Apt is taken away by BPA, and the exposed part of SH-ssDNA is bound to H 1 Complement and turn it on, the H 1 And H 2 The two proteins are complementary to each other, thus forming a long double-stranded structure such as band h, which is as long as 2000 bp.

[0104] Example 7

[0105] The modification process of steps 1 to 6 in Example 1 was tested:

[0106] CV and EIS tests were performed on different modification processes. In 5.0 mM [Fe(CN) 6 ] 3- / 4- The test results in solution are as follows Figure 5 and 6 As shown, among them: (a) bare GCE, (b) AuNPs@Ni-Co MOF / GCE, (c) Fc-Apt@ssDNA / AuNPs@Ni-Co MOF / GCE, (d) MCH / Fc-Apt@ssDNA / AuNPs@Ni-Co MOF / GCE, (e) BPA / MCH / Fc-Apt@ssDNA / AuNPs

[0107] @Ni-Co MOF / GCE, (f)H 1 -H 2 / BPA / MCH / Fc-Apt@ssDNA / AuNPs@Ni-Co MOF / GCE, (g)MB / H 1 -H 2 / BPA / MCH / Fc-Apt@ssDNA / AuNPs@Ni-Co MOF / GCE.

[0108] The results show that ( Figure 5 ), the current of Au NPs@Ni-Co MOF loaded on the GCE electrode surface decreased accordingly, which was caused by the poor conductivity of MOF. AuNPs also improved the current response, but it still did not exceed that of bare GCE. Fc-Apt@ssDNA was immobilized on the AuNPs@Ni-Co MOF / GCE electrode. Due to the combination with the electrode Au-S, the electron transfer on the electrode surface was blocked. After the introduction of BPA, Fc-Apt was taken away from the electrode surface, and the peak current increased. The introduction of H 1 , H 2 , the peak current decreases due to its non-electroactive substance; after double-stranded DNA adsorbs MB, the peak current decreases. EIS results ( Figure 6 )If the CVs are consistent, it indicates that the sensor was successfully constructed.

[0109] Example 8

[0110] Perform DPV detection on step 4 in Example 1:

[0111] DPV tests were performed on ssDNA and Fc-Apt at different concentration ratios. The results showed that ( Figure 7 ), when C ssDNA :C Fc-Apt When the ratio is 1:2, IMB / I Fc The value of I is the lowest, at which point as many Fc-Apt as possible hybridizes and complements with ssDNA; with the increase of ssDNA concentration, there will be less Fc-Apt in the same volume of solution. When a certain amount of BPA is introduced, I Fc The signal will decrease, making I MB / I Fc The value of increases.

[0112] Example 9

[0113] DPV tests were performed on different BPA incubation times in step 6 of Example 1. The results showed that ( Figure 8 ), when incubated for 40 min, Fc-Apt and BPA specific binding and stripping were completed. MB / I Fc Stay steady.

[0114] Example 10

[0115] DPV test was performed on different HCR incubation times in step 6 of Example 1. The results showed that ( Fig. 9 ), with the increase of HCR incubation time, I MB / I Fc It increases continuously and reaches the maximum value when incubated for 120 min, and remains unchanged with further incubation.

[0116] Embodiment 11

[0117] DPV test was performed on different MB incubation times in step 6 of Example 1. The results showed that ( Fig.10 ), with the increase of MB breeding time, I MB / I Fc It increases continuously and reaches the maximum value after 30 min of incubation, and remains unchanged with further incubation.

[0118] Example 12

[0119] A standard curve of a ratiometric electrochemical aptamer sensor for detecting bisphenol A based on HCR reaction was established, and the specific steps are as follows:

[0120] (1) The concentrations are 0M, 1×10 -15 M, 5×10 -15 M, 1×10 -14 M, 1×10 -13 M, 1×10 -12 M, 1×10 -13 M of BPA solution, each added to step 6 of Example 1;

[0121] (2) The three-electrode system was used for testing, with Pt electrode as the counter electrode, Ag / AgCl as the reference electrode, and MB / H 1 -H 2 / BPA / MCH / Fc-Apt@ssDNA / Au NPs@Ni-Co MOF / GCE electrode was used as the working electrode. In a 0.1 M PBS (pH 7.4) buffer solution containing 5 mM [Fe(CN) 6 ] 3- / 4- and 0.1M KCl solution, the voltage was -600~900nm for DPV test; and the current value of the electrochemical sensor was used to measure 1×10 -15 M~1×10 -12 A standard curve was drawn using the logarithmic values ​​of BPA concentration within the range of M.

[0122] (3) The results are as follows Fig.11 and 12 As shown in the figure, the fluorescence response value of the constructed sensor is proportional to the logarithm of BPA concentration in the range of 1×10 -15 M~1×10 -12 There is a good linear relationship within the range of M, and the linear equation is: y = 0.925lgC BPA +15.270, correlation coefficient R 2 =0.994.

[0123] Embodiment 13

[0124] A specific detection experiment of ratiometric electrochemical aptasensor for bisphenol A based on HCR reaction

[0125] By measuring 1.0×10 -12 M BPA and its structural analogs (BPB, BPC and BPAF, concentration 1.0×10 - 10 M)I MB / I Fc The selectivity of the ratiometric electrochemical aptasensor based on dual signal amplification was investigated. Fig.13 As shown, the sensor of the present invention is specific for BPA detection.

Claims

1. A ratiometric electrochemical aptamer sensor based on HCR signal amplification, characterized in that: The Pt electrode is used as the counter electrode, Ag / AgCl is used as the reference electrode, and the modified electrode is used as the working electrode. The preparation of the modified electrode includes the following steps: Step 1, preparation of modified materials: preparation of AuNPs@Ni Co-MOF composite materials; Step 2, preparation of modified material dispersion: dispersing the Au NPs@Ni Co-MOF composite material in a solution consisting of anhydrous ethanol and ultrapure water; Step 3, AuNPs@Ni Co-MOF / GCE preparation: droplets of AuNPs@Ni Co-MOF composite material dispersion were applied onto the clean GCE surface, and the electrode was naturally dried; Step 4, preparation of ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE: drop-coat the ssDNA@Fc-Apt solution on the surface of AuNPs@Ni Co-MOF / GCE, cap and incubate; Step 5, MCH / ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE preparation: drop the MCH solution onto the surface of ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE, rinse and dry; Step 6, preparation of modified electrode: drop bisphenol A solution of different concentrations onto the surface of MCH / ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE, incubate, rinse and dry, then drop TNaK buffer onto the electrode surface, incubate, rinse and dry, and finally drop methylene blue solution onto the electrode surface, incubate, rinse and dry.

2. A ratiometric electrochemical aptamer sensor based on HCR signal amplification according to claim 1, characterized in that: In step 1, the method for preparing the AuNPs@Ni Co-MOF composite material is: Step 1.1, preparation of 2D Ni Co-MOF: Co(NO3)2·6H2O and Ni(NO3)2·6H2O are completely dissolved in a mixed solution containing ultrapure water, ethanol and dimethylformamide by ultrasound; 2-methylimidazole is added to the mixed solution and completely dissolved under ultrasound; heating reaction is performed, and after the reaction is completed, the mixture is cooled to room temperature, and the product is collected by centrifugation and alternately washed with ethanol and dried to obtain 2D Ni Co-MOF; Step 1.2, preparation of AuNPs solution: The HAuCl4 aqueous solution is heated vigorously to boiling; under constant temperature stirring, the sodium citrate solution is quickly added to the HAuCl4 aqueous solution until the solution reaches wine red, and the solution is stirred at a constant speed until it reaches room temperature, thereby obtaining the AuNPs solution; Step 1.3, preparation of AuNPs@Ni Co-MOF composite material: The 2D Ni Co-MOF was dissolved in water to obtain a 2D Ni Co-MOF aqueous solution. In a dark environment, the 2D Ni Co-MOF aqueous solution was stirred with the Au NPs solution, centrifuged, washed and dried multiple times to obtain an AuNPs@Ni-Co MOF composite material.

3. The ratio electrochemical aptamer sensor based on HCR signal amplification according to claim 2, characterized in that: In the step 1.1, the volume ratio of ultrapure water, ethanol and dimethylformamide is 10 mL: 10 mL: 10 mL, the heating reaction temperature is 160 ° C, the heating reaction time is 12 h, the drying temperature is 70 ° C, the drying time is 12 h, and the molar ratio of Ni to Co in 2D Ni Co-MOF is 0 to 0.5: 1; In the step 1.2, the mass fraction of the HAuCl4 aqueous solution is 0.01%, the mass fraction of the sodium citrate solution is 1%, and the volume ratio of the HAuCl4 aqueous solution to the sodium citrate solution is 100 mL:4 mL; In the step 1.3, the concentration of the 2D Ni Co-MOF aqueous solution is 50 mg / mL, the volume ratio of the 2D Ni Co-MOF aqueous solution to the AuNPs solution is 1 mL:0-7.5 mL, the drying temperature is 70° C., and the drying time is 6 h.

4. The ratiometric electrochemical aptamer sensor based on HCR signal amplification according to claim 1, characterized in that: In the step 2, the volume ratio of aqueous ethanol to ultrapure water is 700 μL:300 μL, and the mass concentration of the modified material dispersion is 0.5 mg / mL.

5. The ratiometric electrochemical aptamer sensor based on HCR signal amplification according to claim 1, characterized in that: In step 4, the incubation temperature is 4° C., the time is 10 h, the molar concentration of the ssDNA@Fc-Apt solution is 2 μM, and the volume ratio of ssDNA to Fc-Apt is 3:1 to 1:3; The sequence of the ssDNA is: 5′-SH-TTTTTTAAAGGCCATACGCGGAACGCTATCCCACCTGAC-3′; The sequence of the Fc-Apt is: 5′-Fc-CCGGTGGGTGGTCAGGTGGGATAGCGTTCCGCGTATGGCCCAGC GCATCACGGGTTTCGCACCA-3′.

6. The ratiometric electrochemical aptasensor based on HCR signal amplification according to claim 1, characterized in that: In step 5, the molar concentration of the MCH solution is 2 mM.

7. The ratiometric electrochemical aptamer sensor based on HCR signal amplification according to claim 1, characterized in that: In step 6, bisphenol A solutions of different concentrations are dripped onto the surface of MCH / ssDNA@Fc-Apt / AuNPs@Ni Co-MOF / GCE and incubated for 30 to 70 minutes, TNaK buffer is dripped onto the electrode surface and incubated for 60 to 180 minutes, and methylene blue solution is dripped onto the electrode surface and incubated for 5 to 50 minutes.

8. The ratiometric electrochemical aptamer sensor based on HCR signal amplification according to claim 7, characterized in that: In step 6, the molar concentration of the TNaK buffer is 20 mM, pH = 7.4, and contains 2 μM H1, 2 μM H2, 20 mM Tris-HCl, 140 mM NaCl, and 5 mM KCl; The sequence of H1 is: 5′-ACGCGGAACGCTATCCCACCTGACATAGCGTGGTCAGGTGGGATAG CGTTCCGCGTATGGCCCA-3′; The sequence of H2 is: 5′-CACGCTATGTCAGGTGGGATAGCGTTCCGCGTTGGGCCATACGCGG AACGCTATCCCACCTGAC-3′; The molar concentration of the methylene blue solution is 2 nM.

9. The use of a ratio electrochemical aptamer sensor based on HCR signal amplification according to claim 1, characterized in that: Used to detect bisphenol A.

10. The use of a ratio electrochemical aptamer sensor based on HCR signal amplification according to claim 9, characterized in that: The linear detection range is 1×10 -15 M~1×10 -12 M.

Citation Information

Cited By

  • AuNPs (at) CTS (at) NiCo2O4 composite material, preparation method and application

    CN120044105A