Au / 2D-MOF / GCE electrode, electrochemical aptamer sensor manufactured by using Au / 2D-MOF / GCE electrode and preparation method of electrochemical aptamer sensor

By compositing two-dimensional copper metal-organic framework nanosheets Cu-THQ onto a glassy carbon electrode and covering them with AuNP, and combining them with an LPS aptamer, a bioelectrochemical aptamer sensor was constructed. This solved the problems of insufficient sensitivity and selectivity in traditional LPS detection methods, and achieved high-sensitivity and widely applicable LPS detection.

CN118731129APending Publication Date: 2024-10-01GUANGDONG NO 2 PROVINCIAL PEOPLES HOSPITAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410735780.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing traditional LPS detection methods require skilled technicians, are time-consuming and labor-intensive, and are easily affected by sample sampling. They also lack sensitivity and anti-interference performance. Traditional nanomaterials have limited design flexibility and multifunctionality, making it difficult to achieve high-sensitivity and selective LPS detection.

Method used

A bioelectrochemical aptamer sensor was constructed using an Au/2D-MOF/GCE electrode. This sensor was created by compositing two-dimensional copper metal-organic framework nanosheets (Cu-THQ) onto a glassy carbon electrode and uniformly covering them with AuNP structures. Combined with an LPS aptamer, the sensor was then detected using differential pulse voltammetry.

Benefits of technology

It achieves high-sensitivity detection of LPS with a dissociation constant KD of 3.25 fg/mL, a linear range of 1 fg/mL to 100 pg/mL, and a detection limit LOD of 0.15 fg/mL, which is significantly better than traditional methods. It has good selectivity and anti-interference ability and is suitable for sensitive detection of a variety of targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731129A_ABST
    Figure CN118731129A_ABST
Patent Text Reader

Abstract

The invention discloses an Au / 2D-MOF / GCE electrode and a specific preparation method of the bioelectrochemical aptamer sensor. According to the bioelectrochemical aptamer sensor manufactured by the electrode, the detection target of the biosensor can be easily changed by changing the modified aptamer, and the bioelectrochemical aptamer sensor is widely applicable to detection of various detection targets, such as LPS detection of gram-negative bacteria. The inventor particularly finds that when the 2D-MOF is specifically Cu-THQ, an unexpected technical effect is achieved. When the bioelectrochemical aptamer sensor is used for carrying out LPS detection, the dissociation constant KD of the LPS is 3.25 fg / mL, the linear range is 1 fg / mL to 100 pg / mL, the detection limit LOD is as low as 0.15 fg / mL, various indexes are far superior to those of a traditional detection method, and the bioelectrochemical aptamer sensor is a huge technical breakthrough in the industry. The Cu-THQ nanosheet shows a flatter form and has a redox ligand and denser Cu redox sites, further, the 3D flower-shaped Au nanostructure AuNP uniformly deposits and covers the unique microstructure formed by Cu-THQ / GCE, and a series of excellent microcosmic electrochemical characteristics of the electrode are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an Au / 2D-MOF / GCE electrode and an electrochemical aptamer sensor made using the same and a preparation method thereof, and belongs to the field of medical detection. Background Art

[0002] Infectious diseases such as meningitis, pneumonia, and diarrhea are caused by Gram-negative bacteria. LPS is a key component of the outer membrane of Gram-negative bacteria, a complex composed of lipids and polysaccharides. Dead Gram-negative bacteria release lipopolysaccharide (LPS) from their outer membrane, and the concentration of LPS in serum is proportional to the number of Gram-negative bacteria. At the same time, LPS is an endotoxin, which is released when bacteria die and exerts its effect by binding to the TLR4 receptor on animal cells, triggering an inflammatory response. Therefore, rapid and sensitive detection of LPS in serum is essential for timely diagnosis, evaluation of infection sources, identification of bacterial infections, and promotion of treatment. Traditional diagnostic methods such as the horseshoe crab amoeba lysate (LAL) assay rely mainly on bacterial culture methods. However, although this method is sensitive, these methods require skilled technicians and involve complex sample preparation protocols, which are not only time-consuming and labor-intensive, but also easily affected by specimen sampling, which may lead to false positives or false negatives. The assay also exhibits relatively low sensitivity, a narrow linear range (about 10 -2 ~1EU / mL, equivalent to 1pg / mL--0.1ng / mL) and insufficient anti-interference performance.

[0003] Electrochemical sensors are an effective means of detecting lipopolysaccharide (LPS), using aptamers and nanomaterials to improve the sensitivity and selectivity of detection. Among them, the combination of recognition elements and electrodes is crucial for the construction of electrochemical sensors; however, the limited design flexibility and versatility of traditional nanomaterials have hindered its development.

[0004] Recently, two-dimensional metal-organic frameworks (2D-MOFs) with excellent conductivity have been gradually applied to electrochemical biosensors due to their redox properties and planar metal ligand networks with highly delocalized π electrons. This aptasensor achieved sensitive and selective detection of LPS in serum samples of patients with bacterial infection and showed good applicability. This simple and effective strategy of introducing conductive 2D-MOFs in electrochemical biosensors provides a powerful approach to develop superior electrochemical detection platforms.

[0005] However, there are many types of 2D-MOF materials, and the performance of products obtained by using different 2D-MOF materials cannot be accurately predicted, and may vary greatly. Cu-TCPP and Cu-THQ are two specific 2D-MOF materials that the inventors focus on in the present invention. Although Cu-TCPP is used for electrochemical sensor detection in some known studies, there are many types and structures of electrochemical sensors. The types, structures and principles of sensors using Cu-TCPP in known studies are different from those of the present invention, and are not used for LPS detection; and the related applications of Cu-THQ are even rarer. Summary of the invention

[0006] The first aspect of the present invention is to provide an Au / 2D-MOF / GCE electrode, which has a two-dimensional copper metal organic framework nanosheet layer composited on an underlying GCE glassy carbon electrode, and the two-dimensional copper metal organic framework nanosheet layer 2D-MOF is composited with nanostructured AuNP, and the whole contains an Au / 2D-MOF / GCE structure.

[0007] Furthermore, the two-dimensional copper metal organic framework nanosheet layer 2D-MOF is specifically a Cu-TCPP and Cu-THQ nanosheet layer.

[0008] Preferably, the Cu-THQ nanosheet layer is used. The AuNP structure is evenly covered on the Cu-THQ nanosheet layer. The Cu-THQ nanosheet layer is composited on the bottom GCE glassy carbon electrode.

[0009] Furthermore, the Au nanostructure AuNP is in a 3D flower shape and is uniformly deposited and covers the Cu-THQ / GCE to form an Au / Cu-THQ / GCE electrode.

[0010] Furthermore, the electroactive surface area of ​​the Au / Cu-THQ / GCE electrode is 0.1551 cm 2 The electroactive surface area of ​​Au / Cu-TCPP / GCE electrode is 0.1257 cm 2 .

[0011] Furthermore, the Au atomic percentage on the surface of the Au / Cu-THQ / GCE electrode is greater than 80%, specifically greater than 83%, and more specifically greater than 84.96%.

[0012] The second aspect of the present invention is to provide a bioelectrochemical aptamer sensor, which is an Apt / Au / 2D-MOF / GCE structure obtained by combining the Au / 2D-MOF / GCE electrode mentioned above with the aptamer Apt, and can obtain a bioelectrochemical aptamer sensor that responds specifically to a specific detection object.

[0013] Furthermore, the aptamer Apt is an aptamer of lipopolysaccharide LPS (Lipopolysaccharide), and a bioelectrochemical aptamer sensor that responds specifically to the concentration of LPS can be obtained.

[0014] Furthermore, the two-dimensional copper metal organic framework nanosheet layer 2D-MOF is a Cu-THQ nanosheet layer. When differential pulse voltammetry (DPV) is used for LPS detection, the dissociation constant of LPS is KD=3.25fg / mL, the linear range is 1fg / mL to 100pg / mL, and the detection limit LOD (Limit of Detection) is 0.15fg / mL.

[0015] The third aspect of the present invention is to provide a method for preparing the bioelectrochemical aptamer sensor described above, comprising the steps of: preparing a dispersion system of Cu-THQ nanosheets with a first concentration, depositing it on a bare GCE glassy carbon electrode with a diameter of 3 mm, and the Cu-THQ deposition amount is 6-10 μL, more specifically 7-9 μL, and more specifically 8 μL; or preparing a dispersion system of Cu-TCPP nanosheets with a first concentration, and depositing it on a bare GCE by drop coating, and the Cu-TCPP deposition amount is 8-12 μL, more specifically 9-11 μL, and more specifically 10 μL.

[0016] Furthermore, the preparation method of the aforementioned bioelectrochemical aptamer sensor comprises preparing a dispersion system of Cu-THQ nanosheets with a first concentration of 1 mg / mL, or preparing a dispersion system of Cu-TCPP nanosheets with a first concentration of 1 mg / mL.

[0017] Further, the method comprises the steps of depositing Cu-THQ nanosheets on bare GCE to obtain a Cu-THQ / GCE structure, drying and immersing the structure in a 0.1% HAuCl4 solution, and electro-depositing Au on the electrode surface at -0.2V for a deposition time of 120-270s, more specifically 180-240s, and more specifically 210s to obtain an Au / Cu-THQ / GCE structure.

[0018] Further, in the scheme of depositing Cu-THQ nanosheets on bare GCE, the steps are included: 1) synthesizing two-dimensional Cu-THQ nanosheets; 2) making an electrochemical biosensor, wherein step 2) includes: polishing a bare GCE with a diameter of 3 mm using 0.3 and 0.05 μm alumina slurries until a mirror-like gloss is obtained; then, the bare GCE is ultrasonically treated in ultrapure water, ethanol and ultrapure water in sequence, and then dried with nitrogen vapor; then 8 μL of Cu-THQ nanosheets (first concentration 1 mg / mL) are deposited on the surface of the GCE; after complete drying, the modified electrode is immersed in 0. 1% HAuCl4 solution; AuNPs were electrodeposited on the electrode surface at -0.2V and then dried at room temperature to form Au / Cu-THQ / GCE; subsequently, the prepared Au / Cu-THQ / GCE was incubated with 0.25μM Apt and reduced with 1mM TCEP and incubated at 37°C for 30 min; after rinsing and drying, the electrode was incubated with 1mM 6-mercapto-1-hexanol for 30 min to prevent nonspecific adsorption and block blank sites; after rinsing, Apt / Au / Cu-THQ / GCE was incubated with LPS solution at 37°C for 40 min.

[0019] Beneficial technical effects

[0020] The present invention discloses an Au / 2D-MOF / GCE electrode and an electrochemical aptamer sensor made using the same and a preparation method thereof. The bioelectrochemical aptamer sensor made by the electrode can easily change the detection target of the biosensor by changing the modified aptamer, and is widely applicable to the detection of a variety of detection targets, such as LPS detection of Gram-negative bacteria. The inventors particularly found that when the 2D-MOF is specifically Cu-THQ, an unexpected technical effect is achieved. When the bioelectrochemical aptamer sensor is used for LPS detection, the dissociation constant KD of LPS is 3.25fg / mL, the linear range is 1fg / mL to 100pg / mL, and the detection limit LOD is as low as 0.15fg / mL. All indicators are far superior to traditional detection methods, which is a huge technological breakthrough in the industry. This may be due to the flatter morphology of Cu-THQ nanosheets, the presence of redox ligands and denser Cu redox sites, the unique micromorphology formed by the uniform deposition of 3D flower-like Au nanostructures AuNPs covering Cu-THQ / GCE, and a series of excellent microelectrochemical properties of the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The scheme of the present invention and its beneficial technical effects are described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0022] Figure 1:(A) Construction of Apt / Au / 2D-MOFs / GCE sensing platform. (B) Schematic diagram of electrochemical biosensor for detecting LPS.

[0023] Figure 2 : (A) XPS spectrum of Cu-TCPP, (B) O1s, (C) C1s, and (D) high-resolution XPS spectra of Cu2p.

[0024] Figure 3 :(A) XPS spectrum of Cu-THQ. (B) High-resolution XPS spectra of O1s, (C) C1s, and (D) Cu2p.

[0025] Figure 4 : Transmission electron microscopy (TEM) images of (A) Cu-TCPP nanosheets and (B) Cu-THQ nanosheets; powder XRD patterns of (C) Cu-TCPP nanosheets and (D) Cu-THQ nanosheets.

[0026] Figure 5 :(A, B) EIS graphs of Au / Cu-THQ / GCE(a), Au / Cu-TCPP / GCE(b), Au / GCE(c), GCE(d), Cu-THQ / GCE(e), Cu-TCPP / GCE(f). (C) DPV curves of GCE, Au / GCE, Au / Cu-TCPP / GCE, Au / Cu-THQ / GCE. (D) Comparison of DPV current peaks of electrodes (n=3).

[0027] Figure 6 :(A) Comparison of different Cu-THQ nanosheet volumes and different electrodeposition times of the prepared sensor CV current peaks (n = 3), a histogram of the effects of Cu-THQ nanosheet volume and electrodeposition time was obtained. (B)(C)(D)(E) Represent the CV cyclic voltammograms of 5μL, 8μL, 10μL, 15μL Cu-THQ nanosheet volumes and different HAuCl4 electrodeposition times of 30-270s. The optimal volume of Cu-THQ was finally optimized to be 8μL: and the optimal Au electrodeposition time was 210s, with a maximum current of about 230μA.

[0028] Figure 7:(A) Comparison of CV current peaks of different Cu-TCPP nanosheet volumes and different electrodeposition times of the prepared sensors (n=3); a histogram of the effects of Cu-TCPP nanosheet volume and electrodeposition time was obtained. (B)(C)(D)(E) Represent the CV cyclic voltammograms of 5μL, 8μL, 10μL, 15μL Cu-TCPP nanosheet volumes and different HAuCl4 electrodeposition times of 30-270s. The optimal volume of Cu-TCPP was finally optimized to be 10μL: and the optimal Au electrodeposition time was 240s, with a maximum current of about 180μA.

[0029] Figure 8 : (A) CV graphs and (B) histograms of Au / GCE electrodes at different electrochemical deposition times, with the maximum current being approximately 150 μA.

[0030] Fig. 9 : SEM images of (A) Au / GCE, (B) Au / Cu-TCPP / GCE and (C) Au / Cu-THQ / GCE.

[0031] Fig.10 : SEM images of (A) GCE, (B) Cu-TCPP / GCE and (C) Cu-THQ / GCE.

[0032] Fig.11 : EDS analysis of Au / Cu-TCPP / GCE.

[0033] Fig.12 : EDS analysis of Au / Cu-THQ / GCE.

[0034] Fig.13 :(A) and (B) represent the CV curves and current peak comparison diagrams of GCE, Au / GCE, Au / Cu-TCPP / GCE and Au / Cu-THQ / GCE, respectively, wherein the data of (B) are expressed as mean ± SD (n = 3). (C) DPV curves and (D) EIS spectra corresponding to Au / Cu-THQ / GCE, Apt / Au / Cu-THQ / GCE and Apt / Au / Cu-THQ / GCE with LPS (0.1 pg / mL).

[0035] Fig.14: CV graphs obtained at different scan rates from 10 to 100 mV / s for (A) Au / GCE, (C) Au / Cu-TCPP / GCE and (E) Au / Cu-THQ / GCE in a solution of 5.0 mM K3Fe(CN)6 / K4Fe(CN)6 and 0.1 M KCl. And the peak current versus scan rate graphs for (B) Au / GCE, (D) Au / Cu-TCPP / GCE and (F) Au / Cu-THQ / GCE (n=3).

[0036] Fig.15 :(A) The corresponding DPVs were obtained by incubation with different concentrations of DNA aptamers (n=3), (B) The average difference of DPVs before and after using 0.25μM and 0.5μM Apt (n=3).

[0037] Fig.16 : DPV peak current of the biosensor after incubation with LPS (0.1 pg / mL) for different time periods (n=3).

[0038] Fig.17 :(A) Using different concentrations (ag): 0, 1×10 -15 , 1×10 -14 , 1×10 -13 , 1×10 -12 , 1×10 -11 and 1×10 -10 DPV curves recorded for Glu, IgG, HSA, AST, ALT and LPS at 0.1 pg / mL. (B) Linear fit of peak current and cLPS logarithm. Error bars represent standard deviation of three independent experiments. (C and D) Responses of Apt / Au / Cu-THQ / GCE in the presence of Glu, IgG, HSA, AST, ALT and LPS. The concentration of LPS and interfering molecules was 0.1 pg / mL. Data in (B) and (D) are shown as mean ± SD (n = 3).

[0039] Fig.18 : Langmuir analysis of LPS binding, error bars represent standard deviation of three independent experiments.

[0040] Fig.19 : Corresponding DPV peak currents obtained with LPS (0.1 pg / mL) and without LPS (control group) in (A) 1× PBS buffer and (B) serum (n=3). DETAILED DESCRIPTION

[0041] In order to make the invention purpose, technical solution and beneficial technical effects of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific implementation methods described in this specification are only for explaining the present invention, not for limiting the present invention.

[0042] The research and development process of the present invention is described in detail below.

[0043] 1. Experimental part

[0044] 1.1 Reagents and instruments

[0045] Copper nitrate trihydrate (Cu(NO3)2·3H2O), trifluoroacetic acid, polyvinylpyrrolidone (PVP, average molecular weight 40,000), H4TCPP (97%), N,N-dimethylformamide (DMF, 99.8%), ethanol (99%), Cu(CH3COO)2·H2O, ethylenediamine (99%), THQ, iron (III) chloride hexahydrate (K3[Fe(CN)6]), iron (II) chloride hexahydrate (K4[Fe(CN)6]), potassium chloride (KCl), tri(2-carboxyethyl)phosphine (TCEP, 99%), and chloroauric acid (HAuCl4) were purchased from Aladdin (Shanghai, China). 10×TM buffer, sterile phosphate buffer, and 6-mercapto-1-hexanol were provided by Sangon Biotechnology Co., Ltd. (Shanghai, China). LPS was purchased from Sigma (USA). Glucose (Glu) was purchased from Adamas (Shanghai, China), human immunoglobulin (IgG) was purchased from Meilun Biotechnology (Liaoning, China), human serum albumin (HSA) was purchased from Sigma-Aldrich (USA), glutamate aminotransferase (AST) was purchased from Acmec (Shanghai, China) and alanine aminotransferase (ALT) from Biowamp (Wuhan, China). LPS aptamer (Apt: 5'-(CH2)6-CTTCTGCCCGCCTCCT TCCTAGCCGGATCGCGCTGGCCAGATGATATAAAGGGTCAGCCCCCCAGGAGACGAGATAGGCGGACACT-3') was synthesized by Sangon Biotech Co., Ltd. (Shanghai, China) and HPLC purified. For the preparation of solutions, ultrapure water (18.2 MΩ·cm) was used.

[0046] Electrochemical measurements were performed using an RST5100F electrochemical workstation (Suzhou Ruisaite Instrument Co., Ltd., Suzhou, China). Scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS) images were captured using a field emission scanning electron microscope (Gemini500, Germany). Transmission electron microscopy (TEM) images were obtained using a transmission electron microscope (JEM1400, Japan), and powder X-ray diffraction (PXRD) patterns were obtained using a PANalytical instrument (Empyrean, the Netherlands) to analyze the MOF crystalline phase. X-ray photoelectron spectroscopy (XPS, Nexsa, ThermoFisherScientific, USA) was used to examine the surface composition and valence state. In addition, the WB-80 microbial rapid dynamic monitoring system (Beijing Jinshanchuan Company) was used to determine the LPS concentration in real serum samples.

[0047] 1.2 Synthesis of Cu-MOF nanosheets

[0048] Synthesis of Cu-TCPP nanosheets: Cu(NO3)2·3H2O (7.2 mg, 0.03 mmol), trifluoroacetic acid (1.6 μL) and polyvidone (PVP) (20.0 mg) were dissolved in a mixture of 24 mL of dimethylformamide (DMF) and ethanol (v:v=3:1) and placed in a 50 mL capped vial. Subsequently, TCPP (8.0 mg, 0.005 mmol) was added to a mixture of 8 mL of DMF and ethanol (v:v=3:1) while stirring. The two solutions were then mixed and ultrasonically treated for 10 minutes. The solution was then transferred to a reactor, heated to 80°C and maintained for 3 hours to obtain red nanosheets. The resulting red nanosheets were then washed with ethanol and centrifuged at 8000 rpm for 10 minutes to collect the nanosheets. Finally, the obtained Cu-TCPP nanosheets were redispersed in 10 mL of ethanol.

[0049] Synthesis method of Cu-THQ nanosheets: Under N2 protection, tetrahydroxy-1,4-benzoquinone hydrate (THQ) (50 mg) was first dissolved in 17 ml of degassed water to prepare a THQ solution. Subsequently, a mixture containing Cu(CH3COO)2·H2O (77 mg) and ethylenediamine (40 μL) was added to the THQ solution under vigorous stirring. The reaction mixture was reacted under stirring for 12 hours at room temperature. The resulting product was filtered and washed twice with H2O (17 mL) and twice with acetone (9 mL). After centrifugation at 6000 rpm, the product was collected and then dried in an oven at 60°C overnight for further processing.

[0050] 1.3 Fabrication of electrochemical biosensor

[0051] A bare GCE with a diameter of 3 mm was polished using 0.3 and 0.05 μm alumina slurries until a mirror-like gloss was obtained. Subsequently, the bare GCE was ultrasonically treated in ultrapure water, ethanol, and ultrapure water, and then dried with nitrogen vapor. An appropriate volume of 2D-MOF nanosheets (specifically Cu-TCPP nanosheets and Cu-THQ nanosheets) was then deposited on the GCE surface, wherein the concentration of the 2D-MOF nanosheets was the first concentration, and the first concentration was specifically 1 mg / mL. After complete drying, the modified electrode was immersed in a 0.1% HAuCl4 solution. Au was deposited on the electrode surface at -0.2 V by different electrodeposition times and dried at room temperature to form Au / 2D-MOF / GCE. Subsequently, the prepared Au / 2D-MOF / GCE was incubated with 0.25 μM Apt, reduced with 1 mM TCEP, and incubated at 37 ° C for 30 minutes. After rinsing and drying, the electrode was incubated with 1 mM 6-mercapto-1-hexanol for 30 min to prevent nonspecific adsorption and block blank sites. After rinsing, Apt / Au / 2D-MOF / GCE was incubated with different concentrations of LPS at 37 °C for 40 min. The electrode was then carefully cleaned and used for electrochemical measurements.

[0052] 1.4 Electrochemical measurements

[0053] Electrochemical measurements were performed using an RST5100F electrochemical workstation equipped with a conventional three-electrode system. GCE or modified GCE was used as the working electrode. The reference electrode used was a saturated calomel electrode, and a platinum wire was used as the counter electrode. EIS, CV, and DPV measurements were performed in an electrolyte containing K3[Fe(CN)6] / K4[Fe(CN)6](5mM) and KCl(0.5M). For EIS, the experimental parameters included an amplitude of 5mV, a bias potential of 0.224V, and a frequency range of 0.1-10kHz. The conditions for CV scanning were a scan rate of 0.1V / s in the range of -0.2 to 0.6V. The conditions for DPV measurement were a pulse amplitude of 50mV, a potential increment of 4mV, a pulse width of 40ms, a pulse period of 0.1s, and a voltage range of 0-0.6V.

[0054] 2. Results and Discussion

[0055] 2.1 Principle of the proposed electrochemical aptasensor

[0056] First, GCE was coated with 2D-MOF nanosheets (Cu-TCPP or Cu-THQ) as a support material and electroactive layer for Au deposition. Subsequently, Au was in situ electrodeposited onto the GCE coated with MOF nanosheets, and then the LPS aptamer was covalently bound to the Au nanostructures via Au-S bonds. In the presence of LPS, the aptamer effectively captured the LPS molecules with high efficiency and selectivity, resulting in an increased hindrance to the diffusion process and a decrease in the DPV current. Therefore, the DPV technique can be used to sensitively and selectively detect the concentration of LPS.

[0057] 2.2 Characterization of synthesized 2D Cu-MOF nanosheets

[0058] To examine the construction of aptasensors, Cu-TCPP and Cu-THQ were used. Both MOF structures consist of two-dimensional stacked layers composed of planar tetracoordinated Cu 2+ ions and oxygen chelating ligands. Although Cu-TCPP has been used for electrochemical sensor detection in previous studies, Cu-THQ is rare in such applications. The synthesized Cu-TCPP and Cu-THQ nanosheets were characterized by SEM, TEM, XPS and PXRD. As shown in the TEM image ( Figure 4 A, B), both samples showed 2D nanosheet morphology characterized by surface wrinkles and folds. The PXRD patterns of Cu-TCPP and Cu-THQ nanosheets are similar to those reported previously in the literature. The chemical state and elemental composition of Cu-TCPP and Cu-THQ were analyzed using XPS. The XPS spectra of Cu-TCPP and Cu-THQ showed different peaks corresponding to Cu2p, O1s, and C1s, such as Figure 2 and 3 As shown. In the Cu2p region, Cu-TCPP and Cu-THQ nanosheets exhibit two peaks at about 932-934 eV and 931-933 eV, corresponding to Cu2p3 / 2 and Cu2p1 / 2, respectively. These results confirm the successful synthesis of phase-pure Cu-TCPP and Cu-THQ nanosheets.

[0059] EIS can be used to evaluate the electrochemical performance of interfaces. The charge transfer resistance (Rct) is represented by the semicircular diameter of the electrochemical impedance. The EIS graph of Rct can clearly show the effects of various electrode surfaces on diffusion limitation and electron transfer limitation. Figure 5The EIS graphs of GCE modified with Cu-TCPP (i.e., Cu-TCPP / GCE) and GCE modified with Cu-THQ (i.e., Cu-THQ / GCE) in a solution containing 5 mM K3Fe(CN)6 / K4Fe(CN)6 are shown. Analysis of the corresponding data in the graph shows that the Rct of Cu-TCPP / GCE is about 1330Ω, which exceeds the Rct of Cu-THQ / GCE (725Ω). These findings indicate that the conductivity of Cu-THQ is significantly higher than that of Cu-TCPP.

[0060] 2.3 Preparation and characterization of Au / 2D-MOF / GCE

[0061] Although Cu-TCPP and Cu-THQ provide abundant active sites and electrocatalytic activity, they exhibit limitations such as semiconductivity and nonspecific electrochemical responses, making them unsuitable for stand-alone use. To address these limitations, a promising strategy is to composite 2D-MOFs with metal nanostructures to achieve optimal interfacial interactions, thereby improving conductivity, electron transfer rate, and electrocatalytic activity. In addition, AuNPs can easily bind to aptamers through Au-S bonds. Therefore, AuNPs were used for electrochemical deposition onto 2D-MOFs. An electrochemical deposition voltage of -0.2 V and a HAuCl4 concentration of 0.1% were used to prepare the AuNP-modified electrodes. Other preparation parameters, such as the electrodeposition time and the amount of MOF modification on the GCE, were optimized ( Figure 6 and 7 In addition, AuNPs were directly deposited on GCE (Au / GCE) for comparative experiments ( Figure 8 ).like Figure 6 and 7 As shown, after Cu-THQ or Cu-TCPP is deposited by drop coating (according to the inventor's research, electrodeposition is not suitable), the Figure 8 ), the current was significantly improved, and the deposited Cu-THQ was much better than the deposited Cu-TCPP. The specific deposition time and MOF modification amount profoundly affected the CV current and electrochemical response. The Cu-THQ modified electrode showed the highest electrochemical response when the volume was 8μL (1mg / mL) and the gold deposition time was 210s ( Figure 6 Meanwhile, the optimized volume and optimized gold deposition time of Cu-TCPP were 10 μL and 240 s, respectively. Figure 7 ).

[0062] The active surface and morphology of the support material are key factors for AuNP deposition. In addition, the distribution and morphology of AuNPs on the electrode significantly affect the electrochemical performance and detection performance. Therefore, the morphologies of different 2D-MOF / GCE and Au / 2D-MOF / GCE were examined. Cu-TCPP and Cu-THQ were uniformly distributed on GCE and maintained their original morphology, as shown in Figure 2. Fig.10 However, after AuNPs were deposited on 2D-MOF / GCE, AuNPs were not uniformly deposited on Cu-TCPP / GCE ( Fig. 9 B and Fig.11 ), while they are uniformly deposited and completely cover Cu-THQ / GCE( Fig. 9 C and Fig.12 ). The AuNPs on Au / Cu-THQ / GCE exhibited a relatively complex morphology, coexisting with smaller gold nanomaterials to form a nanoflower-like 3D structure. In contrast, the morphology of Au / GCE is that on bare GCE, relatively large and smooth AuNPs are loosely deposited on the electrode, with visible gaps between the AuNPs ( Fig. 9 A). In addition, the EDS curves of Au / Cu-THQ / GCE and Au / Cu-TCPP / GCE show obvious peaks corresponding to the Au element ( Fig.11 , 12 ). Furthermore, the Au atomic percentage on the surface of Au / Cu-THQ / GCE (84.96%, Fig.12 ) was significantly higher than Au / Cu-TCPP / GCE (48.26%, Fig.11 ), the uniformity of the deposits was significantly improved, achieving unexpected technical results. The improvement in the deposition of AuNPs on Cu-THQ / GCE compared to Cu-TCPP can be attributed to the morphology and excellent conductivity of Cu-THQ. Figure 4 As shown in Figures B and 10B, Cu-TCPP exhibits folded and wrinkled morphology on GCE, which makes it challenging to electrodeposit AuNPs uniformly and in large quantities and hinders electron transfer. Cu-THQ nanosheets exhibit a flatter morphology with redox ligands and more densely packed Cu redox sites ( Fig.10 C), which is beneficial to improve the electrodeposition of AuNPs ( Fig. 9 C). These results indicate that Cu-THQ is an excellent supporting material for the fabrication of Au / 2D-MOF / GCE biosensors.

[0063] 2.4 Electrochemical Characterization of Au / 2D-MOF / GCE

[0064] The electrocatalytic activity of the electrode is significantly affected by its surface morphology and composition. Therefore, CV, EIS, and DPV are used to evaluate the electrochemical properties of the electrode, including conductivity, electrochemistry activity, and electroactive surface area. The CV curves of various electrodes under the optimal experimental conditions are shown in Fig.13 Figure A. The CV peak current increases in the following order: GCE < Au / GCE < Au / Cu-TCPP / GCE < Au / Cu-THQ / GCE. Compared with the bare GCE, the CV peak currents of Au / Cu-THQ / GCE, Au / Cu-TCPP / GCE, and Au / GCE increase by 77%, 48%, and 25%, respectively, as shown in Fig.13 Figure B. The presence of fast redox-active copper sites in the 2D-MOF nanosheets leads to these improvements, and the peaks are generated by Cu 2+ / Cu + and Cu + / Cu 0 as well as the electrocatalytic activity of AuNPs. Due to the excellent deposition of AuNPs on the surface of Cu-THQ and its enhanced electrocatalytic activity and conductivity, the current response of Au / Cu-THQ / GCE significantly exceeds that of Au / Cu-TCPP / GCE, achieving unexpected technical effects.

[0065] After modifying Cu-TCPP and Cu-THQ on GCE, Rct increases, as shown in Figure 5 Figure A and Figure 5B. After depositing Au nanostructures, the impedance spectrum is similar to a straight line, indicating that the composite nanomaterials can enhance the electron transfer ability. This is particularly obvious on Cu-THQ / GCE due to its excellent electrocatalytic activity and conductivity. Rct increases in the following order: Au / Cu-THQ / GCE < Au / Cu-TCPP / GCE < Au / GCE < GCE. To more intuitively observe the signal, DPV is used. As shown in Figure 5 Figure C and Figure 5D, after modifying with 2D-MOF and AuNP, the DPV current of the modified GCE shows a significant increase. The differential pulse voltammetry (DPV) current of the electrode increases correspondingly with its Rct. These findings indicate that Au / Cu-THQ / GCE exhibits excellent conductivity and promotes electron transfer.

[0066] The Randled-Sevcik equation (Equation 1) is used to determine the electroactive surface area ( Fig.14 ) of CV at different scan rates. The electroactive surface area of the Au / Cu-THQ / GCE electrode is calculated to be 0.1551 cm 2 , which is significantly larger than that of Au / Cu-TCPP / GCE (0.1257 cm 2 ) and Au / GCE (0.1008 cm 2), achieving unexpected technical results. The active surface area of ​​the modified electrode exceeds that of the bare GCE (0.0871 cm 2 ). Even when AuNPs were deposited only on bare GCE, the electroactive surface area was already slightly increased. Moreover, the introduction of 2D-MOF nanosheets with abundant active sites on their defect-rich surface further facilitated the deposition of AuNPs and increased the electroactive surface area. Notably, the sufficient deposition of AuNPs on Cu-THQ / GCE resulted in a significantly larger electroactive surface area.

[0067] I p =(2.69×10 5 )AD 1 / 2 n 3 / 2 γ 1 / 2 C (Equation 1)

[0068] The above results show that Au / Cu-THQ / GCE exhibits excellent electrochemical performance compared with Au / Cu-TCPP / GCE, Au / GCE and bare GCE for the following reasons: (1) the fast redox active copper sites of Cu-THQ contribute to the increase of peak CV current; (2) the good conductivity of Cu-THQ enhances the electron transport capacity; (3) the abundant deposition of AuNPs with unique 3D nanoflower morphology on Cu-THQ / GCE promotes electron transfer and may be beneficial for aptamer modification. Therefore, the Au / Cu-THQ / GCE platform is expected to be an excellent candidate for the development of highly sensitive electrochemical biosensors.

[0069] Preparation and electrochemical characterization of 2.5Apt / Au / Cu-THQ / GCE

[0070] LPSApt was modified onto the optimized Au / Cu-THQ / GCE surface via Au-S bonds to achieve a specific response to LPS. DPV and EIS were used to verify whether Apt modification was successful. Fig.13 As shown in C, significantly smaller signals were observed in the presence of Apt immobilization and LPS treatment compared to the negative control (without Apt and LPS). In addition, the electron transfer resistance increased significantly after Apt modification ( Fig.13 D) These findings are attributed to the high insulating and negative charge of Apt, suggesting a target-responsive reaction.

[0071] The amount of Apt modified on the electrode plays a key role in LPS detection because the binding of LPS to the electrode surface hinders the diffusion process and reduces the DPV current. Therefore, the concentration of the Apt solution used for modification was optimized by evaluating the current changes before and after incubation with LPS. First, Au / Cu-THQ / GCE was incubated with different concentrations of Apt at 37°C for 40 min. The modified electrode was then incubated with LPS (10 fg / mL) and subsequently detected by DPV. Fig.15 As shown, the maximum current change was observed when the Apt concentration was 0.25 μM. Therefore, 0.25 μM was selected as the optimal Apt concentration for modification. In addition, the incubation time of the LPS solution was optimized to 40 min, which resulted in the maximum current change ( Fig.16 ).

[0072] 2.6 LPS detection performance of Apt / Au / Cu-THQ / GCE

[0073] After the successful preparation of Apt / Au / Cu-THQ / GCE and optimization of the conditions, the developed aptasensor was used for LPS detection using the DPV method. The peak current decreased with the increase of LPS concentration (ag), as shown in Fig.17 A. A linear correlation was observed between the peak current (Ip) and the logarithm of LPS concentration ( Fig.17 B), represented by the linear equation Ip = 37.26lgcLPS + 313.1 (R2 = 0.9992). Langmuir analysis of LPS binding yielded a dissociation constant KD = 3.25fg / mL ( Fig.18 ), indicating that the electrode has a strong affinity for LPS. The KD value of LPS has not been reported in the electrochemical sensing detection literature. However, compared with other electrochemical sensing electrodes for protein detection, the KD value of this sensor is significantly lower, indicating that it has rapid responsiveness. The linear range is 1fg / mL to 100pg / mL, and the calculated LOD is 0.15fg / mL (S / N=3). As shown in Table 1, the biosensor proposed in the present invention exhibits a wide linear range and the lowest LOD value, achieving an order of magnitude breakthrough, highlighting its satisfactory sensitivity for early diagnosis of bacterial infection, and achieving unprecedented and breakthrough progress.

[0074] Table 1 Comparison with previously reported methods

[0075]

[0076]

[0077] Note:

[0078] [1]YangLM,GaoYK,FangK,SunH,SunJT,LiuHY,FengWH,JiangL(2020)Photocatalyt icallyrenewablepeptide-basedelectrochemicalimpedancemethodforsensinglipopolysac charide,MicrochimActa187(6):349.https: / / doi.org / 10.1007 / s00604-020-04321-8.

[0079] [2]XieSB,ZhangJ,TengLM,YuanW,TangY,PengQ,TangQC(2019)Electrochemicaldete ctionoflipopolysaccharidebasedonrollingcircleamplificationassistedformationofcoppe rnanoparticlesforenhancedresistancegeneration,Sens.ActuatorsB:Chem.301:127072.https: / / doi.org / 10.1016 / j.snb.2019.127072.

[0080] [3]ChenTJ,ShengAZ,HuY,MaoDS,NingLM,ZhangJ(2019)Modularizationofthree-dim ensionalgoldnanoparticles / ferrocene / liposomeclusterforelectrochemicalbiosensor,Bio sens.Bioelectron.124-125:115-121.https: / / doi.org / 10.1016 / j.bios.2018.09.101.

[0081] [4]LiZ,DaiG,LuoFF,LuYQ,ZhangJW,ChuZH,HePG,ZhangF,WangQJ(2020)Anelectro chemicalsensorforbacteriallipopolysaccharidedetectionbasedondualfunctionalCu 2+-modifiedmetal-organicframeworknanoparticles,MicrochimActa187(7):415.https: / / doi.org / 10.1007 / s00604-020-04364-x

[0082] [5]WangN,DaiHX,SaiLT,MaHY,LinM(2019)Copperion-assistedgoldnanoparticleaggr egatesforelectrochemicalsignalalamplificationoflipopolysaccharidesensing,Biosens.Bio electron.126:529-534.https: / / doi.org / 10.1016 / j.bios.2018.11.021

[0083] Excellent biosensors must have excellent selectivity, reproducibility, and long-term stability. The selectivity of the biosensor was confirmed by evaluating the response of DPV to various potential biomolecule interferences such as Glu, IgG, HSA, AST, and ALT. Fig.17 As shown in Figures C and 17D, the signal decreased only in the presence of LPS, while the signal showed minimal changes in the presence of Glu, IgG, HSA, AST and ALT, which confirmed the excellent selectivity. Subsequently, the reproducibility was confirmed by measuring the response of DPV to 1pg / mL LPS using five Au / Cu-THQ / GCE biosensors under the same test conditions. As shown in Table 2, the relative standard deviation (RSD) of the DPV peak current obtained from five parallel tests was 3.98% (n=5), indicating that the biosensor has good reproducibility. The prepared biosensor was stored at 4°C for 15 days to evaluate its stability. The response of DPV to 1pg / mL of LPS was then measured, and the current reduction was maintained at 85.7% of the initial current (Table 3, n=3), showing satisfactory stability. The above satisfactory selectivity, reproducibility and stability highlight the potential for real sample detection.

[0084] Table 2 Relative standard deviation (RSD) of DPV peak current (1 pg / mL LPS, n=5)

[0085]

[0086] Table 3 Stability of biosensors (n=3)

[0087]

[0088] 2.7 Biological sample analysis

[0089] To verify the applicability of the Au / Cu-THQ / GCE biosensor for real sample detection, the DPV response of LPS in 50-fold diluted human serum, which is commonly used in previous reports, was examined. Due to the high sensitivity of this method, diluting the serum sample 50-fold did not affect the accurate determination of the target substance. The simple dilution process effectively mitigated the interference of coexisting components. Clinically, a cutoff value of 10 pg / mL is considered to be associated with LPS, and values ​​above 20 pg / mL are considered to be LPS-positive, i.e., Gram-negative bacterial infection requiring antimicrobial treatment. 1.00×10 13 , 1.00×10 12 and 1.00×10 11 g / mL of LPS to evaluate the detection accuracy. First, the LPS currents recorded in buffer and serum were almost the same ( Fig.19 ), highlighting the excellent anti-interference ability of the biosensor. Subsequently, Apt / Au / Cu-THQ / GCE was used to measure the LPS concentration in the spiked samples. The recovery of our method was within the acceptable range of 98%-108% with a low RSD (≤8.8%), as shown in Table 4. These results indicate that the proposed biosensor can detect LPS in complex biological samples with good anti-interference properties, thus demonstrating the broad prospects of this method in clinical diagnostic applications.

[0090] Table 4 Detection of LPS in diluted human serum (n=3)

[0091]

[0092] Subsequently, to verify the clinical detection performance of Apt / Au / Cu-THQ / GCE, the biosensor was used to detect LPS in human serum samples collected at various stages of clinical cases of sepsis. As shown in Table 5, the LPS concentration in the samples determined by the Apt / Au / Cu-THQ / GCE biosensor was consistent with the results obtained by the standard method using the WB-80 microbial rapid detection instrument (p>0.5) dynamic monitoring system (LOD=5pg / mL). In addition, the Apt / Au / Cu-THQ / GCE biosensor can sensitively detect 1.33pg / mL of LPS in serum, which is much lower than the LOD of the standard method. The excellent sensitivity, selectivity, accuracy and anti-interference ability of the Apt / Au / Cu-THQ / GCE biosensor demonstrate its broad prospects in clinical detection.

[0093] Table 5 Comparison of LPS concentrations in serum samples measured by the proposed biosensor and the WB-80 microbial dynamic monitoring system (n = 3). Statistical significance was calculated using t-test (p > 0.5)

[0094]

[0095]

[0096] 3. Conclusion

[0097] This study constructed a simple electrochemical aptamer sensor by electrodeposition of gold nanostructures on conductive 2D-MOF nanosheets (specifically 2D-MOF is Cu-TCPP and Cu-THQ) modified electrodes and efficient connection of LPS aptamers. The inventors of the present invention particularly found that when 2D-MOF is specifically Cu-THQ, unexpected technical effects are achieved. When the bioelectrochemical aptamer sensor is used for LPS detection, the dissociation constant KD of LPS is 3.25fg / mL, the linear range is 1fg / mL to 100pg / mL, and the detection limit LOD is as low as 0.15fg / mL, showing excellent stability and strong anti-interference ability, and can achieve accurate detection of LPS. All indicators are far superior to traditional detection methods, showing extremely high accuracy, and at the same time having higher sensitivity, which is a huge technological breakthrough in the industry. This may be due to the fact that the Cu-THQ nanosheets exhibit a flatter morphology, have redox ligands and denser Cu redox sites, and further, the unique micromorphology formed by the uniform deposition of 3D flower-like Au nanostructures AuNPs covering Cu-THQ / GCE, as well as a series of excellent microscopic electrochemical properties of the electrode, resulting in enhanced electrocatalytic activity.

[0098] Moreover, changing the modified aptamers can easily change the detection target of this biosensor, highlighting its wide applicability. Few studies have been known to investigate the use of 2D-MOF as a conductive support layer and the comprehensive exploration of two 2D-MOF nanosheets with different redox centers and morphologies. Overall, the approach of integrating redox-active 2D-MOF nanosheets to enhance detection performance has great practical significance, and the proposed biosensor shows great promise in advancing clinical detection and diagnosis.

Claims

1. An Au / 2D-MOF / GCE electrode, characterized in that: A two-dimensional copper metal organic framework nanosheet layer is compounded on the bottom GCE glassy carbon electrode, and nanostructured AuNP is compounded on the two-dimensional copper metal organic framework nanosheet layer 2D-MOF, and the whole contains Au / 2D-MOF / GCE structure.

2. The Au / 2D-MOF / GCE electrode according to claim 1, characterized in that: The two-dimensional copper metal organic framework nanosheet layer 2D-MOF is specifically a Cu-TCPP or Cu-THQ nanosheet layer, preferably a Cu-THQ nanosheet layer, and the Cu-THQ nanosheet layer is evenly covered with AuNP flower-like structures.

3. The Au / 2D-MOF / GCE electrode according to claim 2, characterized in that: The Au atomic percentage on the surface of the Au / Cu-THQ / GCE structure is greater than 80%, specifically greater than 83%, and more specifically greater than 84.96%.

4. A bioelectrochemical aptamer sensor, characterized in that: It is the Apt / Au / 2D-MOF / GCE structure obtained by combining the Au / 2D-MOF / GCE electrode described in claim 1 with the aptamer Apt, and can obtain a bioelectrochemical aptamer sensor that responds specifically to a specific detection object.

5. The bioelectrochemical aptamer sensor according to claim 4, characterized in that: The aptamer Apt is an aptamer of lipopolysaccharide LPS, and a bioelectrochemical aptamer sensor that specifically responds to the concentration of LPS can be obtained.

6. The bioelectrochemical aptamer sensor according to claim 5, characterized in that: The two-dimensional copper metal organic framework nanosheet layer 2D-MOF is a Cu-THQ nanosheet layer. When differential pulse voltammetry DPV is used for LPS detection, the dissociation constant KD of LPS is 3.25 fg / mL, the linear range is 1 fg / mL to 100 pg / mL, and the detection limit LOD is 0.15 fg / mL.

7. A method for preparing a bioelectrochemical aptamer sensor, wherein the sensor is the bioelectrochemical aptamer sensor according to claim 4, characterized in that: Includes steps: Prepare a dispersion system of Cu-THQ nanosheets with a first concentration, and deposit the Cu-THQ nanosheets on a bare GCE glassy carbon electrode with a diameter of 3 mm, wherein the Cu-THQ deposition amount is 6-10 μL, more specifically 7-9 μL, more specifically 8 μL; Alternatively, a dispersion system of Cu-TCPP nanosheets with a first concentration is prepared, and the Cu-THQ nanosheets are deposited on a bare GCE by drop coating, wherein the Cu-TCPP deposition amount is 8-12 μL, more specifically 9-11 μL, and more specifically 10 μL.

8. The method for preparing the bioelectrochemical aptamer sensor according to claim 7, characterized in that: The method comprises the following steps: depositing Cu-THQ nanosheets on bare GCE to obtain a Cu-THQ / GCE structure, drying the electrode of the Cu-THQ / GCE structure and immersing it in a HAuCl4 solution, and electro-depositing AuNP on the electrode surface at -0.2V for a deposition time of 120-270s, more specifically 180-240s, more specifically 210s, to obtain an Au / Cu-THQ / GCE structure.

9. The method for preparing the bioelectrochemical aptamer sensor according to claim 7, characterized in that: In the scheme for depositing Cu-THQ nanosheets on bare GCE, the steps include: 1) synthesizing two-dimensional Cu-THQ nanosheets; 2) making an electrochemical biosensor, wherein step 2) comprises: polishing a bare GCE with a diameter of 3 mm using 0.3 and 0.05 μm alumina slurries until a mirror-like gloss is obtained; then, the bare GCE is ultrasonically treated in ultrapure water, ethanol and ultrapure water in sequence, and then dried with nitrogen vapor; then 8 μL of Cu-THQ nanosheets (1 mg / mL) are deposited on the surface of the GCE; after complete drying, the modified electrode is immersed in a 0.1% HAuCl4 solution; at -0.2 V AuNPs were electrodeposited on the electrode surface and then dried at room temperature to form Au / Cu-THQ / GCE; subsequently, the prepared Au / Cu-THQ / GCE was incubated with 0.25 μM Apt and reduced with 1 mM TCEP at 37°C for 30 min; after rinsing and drying, the electrode was incubated with 1 mM 6-mercapto-1-hexanol for 30 min; after rinsing, Apt / Au / Cu-THQ / GCE was incubated with different concentrations of LPS at 37°C for 40 min.

10. The method for preparing the bioelectrochemical aptamer sensor according to claim 7, characterized in that: A dispersion system of Cu-THQ nanosheets having a first concentration of 1 mg / mL is prepared, or a dispersion system of Cu-TCPP nanosheets having a first concentration of 1 mg / mL is prepared.