Method for processing rubber with high filling formula

By adding filler in step-by-step quantitatively during the rubber kneading process, the uneven mixing and rolling problems in the high-filling formula are solved, the fluidity and dispersion of the rubber are improved, and the stability and safety of the rubber are ensured.

CN118978752APending Publication Date: 2024-11-19GUIZHOU TIRE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411264304.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the rubber mixing process of high-filling formula, there are problems such as difficulty in eating rubber, uneven mixing, rolling off when the mixer is turned on, and local heating is fast, resulting in scorching and scrapping, operational safety and quality risks.

Method used

By quantitatively adding fillers in steps at different kneading stages, it can play a role in wetting vulcanization system and rubber, improving the fluidity and dispersion of the rubber, and avoiding roll removal problems caused by uneven kneading. The specific steps include the first stage of kneading, second stage of kneading and final stage of carbon black addition, which are added according to the rules of different stages to optimize the dispersion effect and temperature control.

Benefits of technology

The rubber is quickly entered the dispersion and kneading stage, which improves the dispersion uniformity and stability of the rubber, avoids the roll removal problem caused by uneven mixing, and ensures the quality and safety of the rubber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978752A_ABST
    Figure CN118978752A_ABST
Patent Text Reader

Abstract

The invention provides a rubber processing method with a high filling formula. The rubber processing method comprises the following steps: mixing 100 parts by mass of rubber, 55-70 parts by mass of carbon black, an anti-aging agent, resin, a softening agent and an activating agent to prepare a section of master batch; mixing the first-stage rubber master batch with 10-20 parts by mass of carbon black to prepare second-stage rubber master batch; and mixing the second-stage rubber master batch with 2-10 parts by mass of carbon black, sulfur, an accelerant and a scorch retarder to prepare final mixed rubber. According to the rubber processing method disclosed by the invention, the filler is quantitatively added step by step in different mixing stages, so that the filler can achieve the effect of wetting a vulcanization system and rubber during mixing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] The invention relates to the field of rubber processing, and in particular to a method for processing rubber with a high filling formula. Background Art

[0004] Rubber processing can be divided into two stages according to the process: plasticizing and mixing (synthetic rubber formula generally does not have a plasticizing stage). The mixing stage is further divided into a masterbatch stage and a final mixing stage. The masterbatch stage is generally carried out under a high temperature environment, and fillers, processing aids, etc. are mixed with rubber in an internal mixer or an open mixer to achieve the best dispersion effect. The final mixing of rubber mainly involves mixing and dispersing the masterbatch with the vulcanization system at a low temperature.

[0005] The rubber mixing process is generally divided into three stages, namely the wetting stage, the dispersion stage, and the kneading stage. The wetting stage is mainly to eliminate the air adsorbed by the compounding agent, and the raw rubber molecules gradually enter the gaps of the carbon black aggregates to form autolytic rubber molecules; the dispersion stage is that under the action of a certain mechanical force, the carbon black aggregates are gradually and evenly dispersed in the raw rubber. As the mixing proceeds, the effective volume of the carbon black gradually decreases, and the combined rubber is generated. The elasticity begins to gradually increase, and the rubber begins to be pressed; the kneading stage is the basic dispersion of the filler and the compounding agent. Under a certain temperature, with the shearing action of the rotor, the dispersant and the filler are further evenly distributed in the rubber, which can further improve the dispersion uniformity of various additives in the rubber.

[0006] However, it is found in the prior art that in the mixing process of rubber with a high filling formula, there will be problems such as difficulty in rubber absorption, uneven mixing, roll slipping when the sheet is discharged from the mixing mill, and rapid local temperature rise in the final rubber production process. This situation will lead to scorching and scrapping, and there are operational safety risks and quality risks.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0009] The object of the present invention is to provide a rubber processing method with a high filling formula. The rubber processing method adds fillers quantitatively and step by step at different mixing stages so that the fillers can wet the vulcanization system and the rubber during mixing, thereby improving the fluidity of the rubber in an internal mixer in the early stage, making the power and temperature reach an ideal state more quickly, and the rubber can quickly enter the dispersion and kneading stage, so that the dispersion of the compounding agent in the mixed rubber is more uniform and the quality is more stable, and at the same time, the problem of roller debonding caused by uneven mixing is solved.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The present invention provides a method for processing a rubber with a high filling formula, comprising the following steps: 100 parts by weight of rubber, 55-70 parts by weight of carbon black, an antioxidant, a resin, a softener, and an activator are mixed to form a masterbatch; Then, the first-stage masterbatch and 10-20 parts by mass of carbon black are mixed to prepare a second-stage masterbatch; The second-stage masterbatch, 2-10 parts by mass of carbon black, sulfur, an accelerator and a scorch retarder are mixed to prepare a final rubber mix.

[0011] When adding carbon black, the rule is to add the largest amount in the first mixing stage, then add a medium amount in the second mixing stage, and finally add the least amount in the final mixing. The reason for adding according to this rule is that if more is added in the first stage, it can be parked after the second mixing, which is equivalent to improving the dispersion effect through crushing and shearing. The residence time in the final mixing is short, the friction effect will not be very good, and the temperature will not be too high and the rotation speed will not be too fast as the mixing process progresses. Therefore, if the amount of carbon black added later is too large, the shear force will be poor, and poor dispersion will affect the quality of the mixed rubber.

[0012] Of course, although it is added according to this rule, the mass fraction of carbon black added in each stage is also the optimal value explored according to specific practice, because in addition to considering the amount of carbon black added, it is also necessary to consider the final performance of the processed rubber with a high filling formula, because carbon black originally plays a reinforcing role. If the amount added in each stage is not enough, the performance of the final processed rubber will also be affected. Therefore, the optimal addition amount of each section is optimized by balancing the uneven mixing, scorching problems and the processing performance of the mixed rubber. The prior art generally adopts a method of adding all the carbon black at once, but the resulting rubber will be harder and less dispersed. The friction and slippage during the mixing process will cause a relatively high temperature rise, which will also affect the dispersibility of sulfur and easily cause scorching problems. The scheme of the present invention solves the above-mentioned technical defects and effectively avoids the occurrence of safety and quality problems.

[0013] In a mixing process, the amount of carbon black added can also be 57 parts by mass, 59 parts by mass, 62 parts by mass, 63 parts by mass, 64 parts by mass, 65 parts by mass, 66 parts by mass, 67 parts by mass, 68 parts by mass, and 69 parts by mass.

[0014] During the second-stage mixing process, the amount of carbon black added can also be 11 parts by mass, 12 parts by mass, 13 parts by mass, 14 parts by mass, 15 parts by mass, 16 parts by mass, 17 parts by mass, 18 parts by mass, 19 parts by mass, and so on.

[0015] During the final refining process, the amount of carbon black added can also be 3 parts by mass, 4 parts by mass, 5 parts by mass, 6 parts by mass, 7 parts by mass, 8 parts by mass, 9 parts by mass, etc.

[0016] The total amount of rubber used in the whole process is calculated as 100 parts by mass, and the total amount of carbon black used is calculated as 67-100 parts by mass. The carbon black used is one or more of the high-structure carbon blacks, and the specific surface area of ​​the carbon black is 68-150×103m² / kg

[0017] Preferably, as a further feasible solution, during the one-stage mixing process, the antioxidant is one or more of quinoline, p-phenylenediamine and naphthylamine.

[0018] Preferably, as a further feasible solution, the resin is one or more of phenolic resin, petroleum resin and styrene resin.

[0019] Preferably, as a further feasible solution, the softener is one or more of a petroleum plasticizer, a coal tar plasticizer, a pine oil plasticizer, and a fatty oil plasticizer.

[0020] Preferably, as a further feasible solution, the activator is one or more of metal oxides and stearic acid.

[0021] Preferably, as a further feasible scheme, the accelerator is one or more of thiazoles, sulfenamides, thiurams, thioureas, disulfurized carbamates, aldehyde amines, guanidines, and xanthates.

[0022] Preferably, as a further feasible solution, the anti-scorching agent is one or more of sulfur and nitrogen, organic acid, phthalic anhydride, and nitroso compounds.

[0023] Preferably, as a further feasible scheme, the sulfur is one or more of soluble sulfur, insoluble sulfur, sulfur, etc.

[0024] Preferably, as a further implementable scheme, in a mixing process, 100 parts by mass of rubber, 55-70 parts by mass of carbon black, as well as antioxidants, resins, softeners, and activators are mixed at a speed of 45-60 rad / min and a pressure of 15-17 MPa, 2-8 parts by mass of oil are added when the temperature reaches 120°C-140°C, the speed is reduced to 25-40 rad / min, mixing is carried out under the condition of a pressure of 15-17 MPa, and the rubber is discharged when the temperature reaches 165°C-175°C.

[0025] Preferably, as a further implementable solution, during the two-stage mixing process, the first-stage masterbatch is mixed with 10-20 parts by mass of carbon black at a rotation speed of 45-55 rad / min and a pressure of 15-17 MPa, and the masterbatch is discharged at 165° C.-175° C.

[0026] Preferably, as a further feasible solution, during the final refining process, the second-stage masterbatch and 2-10 parts by mass of carbon black, as well as sulfur, accelerator and scorch retarder are mixed at a rotation speed of 20-30 rad / min and a pressure of 14-16 MPa, and the mixture is discharged at 110-125°C.

[0027] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention adds carbon black quantitatively in a stepwise manner in a high-filling formula, so that the carbon black wets the vulcanization system and rubber in the early stage of mixing, thereby solving the problem of poor fluidity and uneven mixing in the early stage of mixing caused by a large filling amount.

[0028] (2) The rubber processing method of the present invention has simple steps and operations, and the processed rubber has good dispersibility and excellent indicators. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] By reading the detailed description of the preferred embodiment below, various other advantages and benefits will become clear to those of ordinary skill in the art. The accompanying drawings are only used for the purpose of illustrating the preferred embodiment and are not considered to be limitations of the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings.

[0031] Figure 1 This is a product photo of the rubber material after rubber processing in Example 1 of the present invention; Figure 2 This is a product photo of the rubber material after rubber processing in Example 2 of the present invention; Figure 3 This is a product picture of the rubber material after rubber processing in Comparative Example 1 of the present invention; Figure 4 This is a product picture of the rubber material after rubber processing in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0033] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0034] The equipment and formula sources used in the following examples and comparative examples are as follows, and the amounts of the various components involved are all in parts by mass: Raw materials: Butadiene rubber: China National Petroleum Corporation Southwest Sales Branch 20# Natural Rubber: SRI TRANG INTERNATIONL PTE LTD N375 carbon black: Guizhou Qianjin New Materials Co., Ltd. Phenolic tackifying resin: Shanghai Tongcheng Chemical Co., Ltd. Zinc oxide: Shijiazhuang Zhiyi Zinc Industry Co., Ltd. Aromatic oil: Guiyang Nanming Jiarun Petrochemical Co., Ltd. Stearic acid: Guizhou Pengcheng Gold Chemical Co., Ltd. Antioxidant 6PPD: Shandong Shangshun Chemical Co., Ltd. Antioxidant TMQ: Ningbo Haili Chemical Co., Ltd. Homogenizer: Jiangsu Ruiba New Material Technology Co., Ltd. Paraffin wax: Guizhou Pengcheng Gold Chemical Co., Ltd. Sulfur: Guangxi Fangchenggang Wuxing Environmental Protection Technology Co., Ltd. Accelerator CZ: Kemai Chemical Co., Ltd. Anti-scorch agent CTP: Shandong Oxidation Huatai Co., Ltd.; Equipment: Internal mixer XM370, XM370, Dalian Rubber Machinery Example 1 Basic formula: 65 parts of butadiene rubber; 35 parts of 20# natural rubber; 100 parts of N375 carbon black; 6 parts of phenolic tackifying resin; 5 parts of zinc oxide; 3.5 parts of stearic acid; 10 parts of aromatic oil; 2 parts of antioxidant 6PPD; 1.8 parts of antioxidant TMQ; 6 parts of homogenizer; 5 parts of paraffin wax; 1.5 parts of sulfur; 3 parts of accelerator CZ; 0.2 parts of anti-scorch agent CTP Preparation process: Mixing with internal mixer, XM370 1. The first master batching stage: 65 parts of butadiene rubber, 35 parts of 20# natural rubber, 70 parts of N375 carbon black, 6 parts of phenolic tackifying resin, 5 parts of zinc oxide, 3.5 parts of stearic acid, 2 parts of antioxidant 6PPD, 1.8 parts of antioxidant TMQ, 6 parts of homogenizer, and 5 parts of paraffin are added to the internal mixer at the same time, and mixed at a speed of 55rad / min and a pressure of 17Mpa. When the temperature reaches 120℃, 10 parts of aromatic oil are added, the speed is reduced to 30rad / min, and the pressure is maintained at 17Mpa for 20 seconds. The top bolt is lifted to its place, and the bolt is mixed again. When the temperature reaches 170℃, the rubber is discharged to prepare a first master batch; 2. Second stage master batching: The first stage master batch and 20% N375 carbon black are added to the internal mixer at the same time. At a speed of 55rad / min and a pressure of 17Mpa, the plug is pressed and mixed for 50 seconds. The top plug is lifted and put into place, and then the top plug is pressed. Mix at 30rad / min and discharge the glue at 165℃. 3. Final mixing stage: Add the second-stage masterbatch, 10 parts of N375 carbon black, 1.5 parts of sulfur, 3 parts of accelerator CZ and 0.2 parts of anti-scorch agent CTP into the internal mixer at the same time, mix at a speed of 25ad / min and a pressure of 15Mpa, and discharge the glue when the mixing temperature reaches 115℃. See the specific picture. Figure 1 .

[0035] Example 2 Basic formula: 65 parts of butadiene rubber; 35 parts of 20# natural rubber; 67 parts of N375 carbon black; 6 parts of phenolic tackifying resin; 5 parts of zinc oxide; 3.5 parts of stearic acid; 10 parts of aromatic oil; 2 parts of antioxidant 6PPD; 1.8 parts of antioxidant TMQ; 6 parts of homogenizer; 5 parts of paraffin wax; 1.5 parts of sulfur; 3 parts of accelerator CZ; 0.2 parts of anti-scorch agent CTP Preparation process: Mixing with internal mixer, XM370 1. The first master batching stage: 65 parts of butadiene rubber, 35 parts of 20# natural rubber, 55 parts of N375 carbon black, 6 parts of phenolic tackifying resin, 3.5 parts of stearic acid, 2 parts of antioxidant 6PPD, 1.8 parts of antioxidant TMQ, 6 parts of homogenizer, and 5 parts of paraffin are added to the internal mixer at the same time, and mixed at a speed of 55 rad / min and a pressure of 17 MPa. When the temperature reaches 120°C, 10 parts of aromatic oil are added, the speed is reduced to 30 rad / min, and the pressure is maintained at 17 MPa for 20 seconds. The top bolt is lifted to its place, and the bolt is mixed again. When the temperature reaches 170°C, the rubber is discharged to prepare a first master batch; 2. Second stage master batching: The first stage master batch and 10% N375 carbon black are added to the internal mixer at the same time. At a speed of 55rad / min and a pressure of 17Mpa, the plug is pressed and mixed for 50 seconds. The top plug is lifted and put into place, and then the top plug is pressed. Mix at 30rad / min and discharge the glue at 165℃. 3. Final refining stage: Add the second-stage masterbatch, 2 parts of N375 carbon black, 5 phr of zinc oxide, 1.5 parts of sulfur, 3 parts of accelerator CZ and 0.2 parts of anti-scorch agent CTP into the internal mixer at the same time, mix at a speed of 25 ad / min and a pressure of 15 MPa, and discharge the glue when the mixing temperature reaches 115 ° C. See the specific picture. Figure 2 .

[0036] Comparative Example 1 Basic formula: 65 parts of butadiene rubber; 35 parts of 20# natural rubber; 100 parts of N375 carbon black; 6 parts of phenolic tackifying resin; 5 parts of zinc oxide; 3.5 parts of stearic acid; 10 parts of aromatic oil; 2 parts of antioxidant 6PPD; 1.8 parts of antioxidant TMQ; 6 parts of homogenizer; 5 parts of paraffin wax; 1.5 parts of sulfur; 3 parts of accelerator CZ; 0.2 parts of anti-scorch agent CTP Preparation process: Mixing is done by internal mixer, XM370; 1. The first master batching stage: 65 parts of butadiene rubber, 35 parts of 20# natural rubber, 75phr of N375 carbon black, 6 parts of phenolic tackifying resin, 5phr of zinc oxide, 3.5 parts of stearic acid, 2 parts of antioxidant 6PPD, 1.8 parts of antioxidant TMQ, 6 parts of homogenizer, and 5 parts of paraffin are added to the internal mixer at the same time, and mixed at a speed of 55rad / min and a pressure of 17Mpa. When the temperature reaches 120℃, 10 parts of aromatic oil are added, the speed is reduced to 30rad / min, and the pressure is maintained at 17Mpa for 20 seconds. The top bolt is lifted to its place, and the bolt is mixed again. When the temperature reaches 170℃, the rubber is discharged to prepare a first master batch; 2. Second stage master batching: add the first stage master batch and 25 parts of N375 carbon black into the internal mixer, mix for 50 seconds at a speed of 55rad / min and a pressure of 17Mpa, lift the top bolt into place, press the top bolt again, mix at 30rad / min, and discharge the glue at 165℃; 3. Final mixing stage: Add the second-stage masterbatch, 1.5 parts of sulfur, 3 parts of accelerator CZ and 0.2 parts of anti-scorch agent CTP into the internal mixer at the same time, mix at a speed of 25ad / min and a pressure of 15Mpa, and discharge the glue when the mixing temperature reaches 115℃. See the specific picture. Figure 3 .

[0037] Comparative Example 2 Basic formula: 65 parts of butadiene rubber; 35 parts of 20# natural rubber; 100 parts of N375 carbon black; 6 parts of phenolic tackifying resin; 5 parts of zinc oxide; 3.5 parts of stearic acid; 10 parts of aromatic oil; 2 parts of antioxidant 6PPD; 1.8 parts of antioxidant TMQ; 6 parts of homogenizer; 5 parts of paraffin wax; 1.5 parts of sulfur; 3 parts of accelerator CZ; 0.2 parts of anti-scorch agent CTP Preparation process: Mixing with internal mixer, XM370 1. The first master batching stage: 65 parts of butadiene rubber, 35 parts of 20# natural rubber, 60phr of N375 carbon black, 6 parts of phenolic tackifying resin, 5phr of zinc oxide, 3.5 parts of stearic acid, 2 parts of antioxidant 6PPD, 1.8 parts of antioxidant TMQ, 6 parts of homogenizer, and 5 parts of paraffin are added to the internal mixer at the same time, and mixed at a speed of 55rad / min and a pressure of 17Mpa. When the temperature reaches 120℃, 10 parts of aromatic oil are added, the speed is reduced to 30rad / min, and the pressure is maintained at 17Mpa for 20 seconds. The top bolt is lifted to its place, and the bolt is mixed again. When the temperature reaches 170℃, the rubber is discharged to prepare a first master batch; 2. Second stage master batching: add the first stage master batch and 40 parts of N375 carbon black into the internal mixer, mix for 50 seconds at a speed of 55rad / min and a pressure of 17Mpa, lift the top bolt into place, press the top bolt again, mix at 30rad / min, and discharge the glue at 165℃; 3. Final mixing stage: Add the second-stage masterbatch, 1.5 parts of sulfur, 3 parts of accelerator CZ and 0.2 parts of anti-scorch agent CTP into the internal mixer at the same time, mix at a speed of 25ad / min and a pressure of 15Mpa, and discharge the glue when the mixing temperature reaches 115℃. See the specific picture. Figure 4 .

[0038] From the product pictures of the rubber materials obtained by processing the above-mentioned embodiments and comparative examples, it can be seen that the rubber materials of embodiments 1-2 have good dispersibility, the rubber material of comparative example 1 does not form sheets in the first stage because too much filler is added, and the rubber material of comparative example 2 does not form sheets in the second stage because too much filler is added in the second stage.

[0039] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. A method for processing rubber with a highly filled formula, It is characterized in that The steps include: 100 parts by weight of rubber, 55-70 parts by weight of carbon black, an antioxidant, a resin, a softener, and an activator are mixed to form a masterbatch; Then, the first-stage masterbatch and 10-20 parts by mass of carbon black are mixed to prepare a second-stage masterbatch; The second-stage masterbatch, 2-10 parts by mass of carbon black, sulfur, an accelerator and a scorch retarder are mixed to prepare a final rubber mix.

2. The rubber processing method according to claim 1, It is characterized in that In the one-stage mixing process, the antioxidant is one or more of quinoline, p-phenylenediamine and naphthylamine.

3. The rubber processing method according to claim 1, It is characterized in that The resin is one or more of phenolic resin, petroleum resin and styrene resin.

4. The rubber processing method according to claim 1, It is characterized in that The softener is one or more of a petroleum plasticizer, a coal tar plasticizer, a pine oil plasticizer, and a fatty oil plasticizer.

5. The rubber processing method according to claim 1, It is characterized in that The activator is one or more of metal oxide and stearic acid.

6. The rubber processing method according to claim 1, It is characterized in that The accelerator is one or more of thiazoles, sulfenamides, thiurams, thioureas, disulfurized carbamates, aldehyde amines, guanidines, and xanthates.

7. The rubber processing method according to claim 1, It is characterized in that The anti-scorching agent is one or more of sulfur and nitrogen, organic acid, phthalic anhydride, and nitroso compounds.

8. The rubber processing method according to any one of claims 1 to 7, It is characterized in that In a mixing process, 100 parts by weight of rubber, 55-70 parts by weight of carbon black, antioxidant, resin, softener and activator are mixed at a speed of 45-60 rad / min and a pressure of 15-17 MPa. When the temperature reaches 120°C-140°C, 2-8 parts by weight of oil are added, the speed is reduced to 25-40 rad / min, mixing is carried out under the condition of a pressure of 15-17 MPa, and the rubber is discharged when the temperature reaches 165°C-175°C.

9. The rubber processing method according to any one of claims 1 to 7, It is characterized in that During the second-stage mixing process, the first-stage masterbatch is mixed with 10-20 parts by mass of carbon black at a rotation speed of 45-55 rad / min and a pressure of 15-17 MPa, and the masterbatch is discharged at 165°C-175°C.

10. The rubber processing method according to any one of claims 1 to 7, It is characterized in that During the final refining process, the second-stage masterbatch and 2-10 parts by mass of carbon black, as well as sulfur, accelerator and anti-scorch agent are mixed at a speed of 20-30 rad / min and a pressure of 14-16 MPa, and the rubber is discharged at 110-125°C.