Method for manually detecting metal content in thick oxide layer of silicon wafer

By using a vacuum pen and pipette gun to process the silicon wafer in a clean room environment, the silicon base in ICP-MS detection is removed, the problem of high silicon base interference is solved, the accuracy of ICP-MS analysis is improved, and the thickness of the silicon wafer is measured. Accurate detection of metal content in the oxide layer, suitable for batch detection.

CN118731145APending Publication Date: 2024-10-01杭州中欣晶圆半导体股份有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410745368.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, the water and SiF4 gas generated by the reaction of hydrofluoric acid solution with high silicon content and thick oxide layer cause serious interference in the detection value of Ti element in ICP-MS detection, affecting the detection accuracy.

Method used

Pre-processing is carried out in a class 100 and above clean room environment, using a vacuum pen and pipette gun to process the silicon wafer, evaporating the SiF4 gas generated by the reaction of hydrofluoric acid and silicon dioxide through a heating plate, removing the silicon base in the solution, and reducing the Test for interference and obtain accurate Ti element content via ICP-MS analysis.

Benefits of technology

It improves the accuracy of ICP-MS analysis and achieves accurate detection of metal content in the thick oxide layer of silicon wafers. It is suitable for batch detection and analysis, and is easy to operate and low in cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a method for manually detecting the content of metal in a thick oxide layer of a silicon wafer, which belongs to the technical field of silicon wafer detection, and comprises the following operation steps: 1, the whole operation process is in a dust-free room environment, and the pretreatment work is completed in a ventilation cabinet; 2, putting the box into a ventilation cabinet, sucking the silicon wafer by using a vacuum pen, and putting the silicon wafer on a wafer bearing frame; and 3, transferring the HF solution to the surface of the silicon wafer by using a pipette, and slightly shaking the silicon wafer by using a vacuum chuck. And 4, placing the silicon wafer on the PTFE film above the heating plate to evaporate the liquid drops on the surface of the silicon wafer to dryness. And 5, transferring the scanning liquid drops to the surface of the silicon wafer by using a pipette, and rolling for more than two times at the positions where the metal on the surface of the silicon wafer is extracted and recovered and the hydrofluoric acid solution is evaporated by using a ball method. And 6, carrying out ICP-MS analysis on the extract to obtain the content value of the Ti metal element. The device has the advantages of time and labor saving, convenient operation, low cost and good stability. The ICP-MS analysis accuracy is improved, and the method is applied to batch detection and analysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon wafer detection, and in particular to a method for manually detecting the metal content in a thick oxide layer of a silicon wafer. Background Art

[0002] After the semiconductor silicon wafer goes through the process of crystal pulling, chamfering, grinding, etching, polishing, cleaning and other processes, the surface metal level is controlled within a certain level; some power device substrates require the back of the silicon wafer to be sealed with a low-temperature oxide layer to prevent subsequent high-temperature heat treatment processes, especially the diffusion of doped elements to the wafer surface during the epitaxial process. Therefore, in addition to the uniformity and density requirements of the oxide layer, there are also requirements for the metal content level in the film layer, which needs to be tested.

[0003] The most common method of manual pretreatment is to use high-purity hydrofluoric acid drops to decompose silicon oxide. The decomposed droplets are scanned across the surface of the silicon wafer to collect oxides and trace metals. The collected liquid is analyzed by ICP-MS for trace element analysis. There is a problem with this method: hydrofluoric acid reacts with the thick oxide layer to generate water, and the water content in the solution is extremely high. The reaction product H2SiF6 dissolves in water, preventing further reaction to generate SiF4 gas. Therefore, the collected liquid contains a large amount of silicon base, which is directly detected by ICP-MS, greatly affecting the accuracy of ICP-MS detection.

[0004] For example, in ICP-MS analysis of Ti, the effects of high silicon base on Ti element detection in oxygen mode are as follows: 48 Multi-atomic group interference of Ti: 29 Si 19 F; 48 Ti 16 O multi-atomic group interference: 29 Si 16 O 19 F. Therefore, the detection value of Ti in the oxygen mode of the high silicon matrix has much more interference than the element content itself. Summary of the invention

[0005] The present invention mainly solves the deficiencies in the prior art and provides a method for manually detecting the metal content in the thick oxide layer of a silicon wafer, which has the advantages of saving time and effort, convenient operation, low cost and good stability. By eliminating some test interference factors, the silicon-based content in the heating container is removed and the silicon-based content in the solution is removed, the accuracy of ICP-MS analysis is improved, and it can be applied to batch detection and analysis.

[0006] The above technical problems of the present invention are mainly solved by the following technical solutions:

[0007] A method for manually detecting the metal content in a thick oxide layer of a silicon wafer comprises the following steps:

[0008] Step 1: The entire operation process needs to be carried out in a clean room environment of Class 100 or above. The pre-treatment work is completed in a fume hood. The fume hood requires a Class 10 dust-free environment with sufficient exhaust. The fume hood is in a negative pressure state. The exhaust air is drawn away to keep the surface of the silicon wafer dry. The silicon-based content of the scanning liquid is greatly reduced, thereby obtaining lower test interference.

[0009] Step 2: Place the box containing the thick oxide layer silicon wafers to be tested into the fume hood, open the box cover, use a vacuum pen to suck up the silicon wafers, and place them on the wafer rack with the thick oxide layer facing up.

[0010] Step 3: Use a pipette to transfer 2ml to 5ml of the prepared 20% to 49% HF solution to the surface of the silicon wafer. The thick oxide layer will quickly react with HF. Use a vacuum pen to slightly shake the silicon wafer to allow the droplets to roll over the entire surface of the silicon wafer and stay in the center of the silicon wafer.

[0011] Step 4: Place the silicon wafer on the PTFE film above the heating plate; adjust the temperature of the heating plate to 100-120°C, heat for 30-60 minutes until the droplets on the surface of the silicon wafer evaporate, turn off the heating plate, and cool to room temperature.

[0012] Step 5: Use a pipette to transfer 1-5 ml of 2-10% HF + 2-10% H2O2 to the configured scanning droplet and drop it onto the surface of the silicon wafer. Use the ball rolling method to extract and recover the metal on the surface of the silicon wafer. Roll twice more at the position where the hydrofluoric acid solution evaporates.

[0013] Hydrogen peroxide slightly oxidizes the surface of the silicon wafer to form a thin oxide layer, and hydrofluoric acid reacts with the oxide layer to generate silicon fluoride and water, thereby recovering the metal remaining on the surface of the silicon wafer into the scanning liquid.

[0014] Step 6: The extract is analyzed by ICP-MS to obtain the Ti metal element content. The silicon removal treatment avoids the solution entering the ICP-MS analysis from containing high silicon groups, thus obtaining more accurate Ti element content results.

[0015] Preferably, the fume hood is cleaned and washed to be free of metal, glass and other material contamination. The fume hood is cleaned and the number of air particles with a particle size ≥ 0.5 μm and above is ≤ 1. The 300-500°C ceramic or PTFE-coated heating plate is cleaned and placed in the fume hood. The PTFE film is cleaned and dried with nitrogen and laid on top of the ceramic plate or PTFE-coated plate of the heating plate.

[0016] Preferably, the silicon dioxide is reacted with hydrofluoric acid to generate water-soluble hexafluorodihydrogen silicon, i.e. SiO2+6HF=H2SiF6+2H2O, by evaporation, which is continued to react under heating to generate silicon tetrafluoride gas and HF gas, i.e. H2SiF6=SiF4+2HF, which is volatilized to carry out silicon removal treatment.

[0017] Preferably, the droplets on the silicon wafer are poured into a prepared 100 ml PFA sample bottle, and the sample bottle number is recorded; an equal amount of HF prepared solution is transferred to a prepared 100 ml sample bottle using a pipette, and the sample bottle number is recorded as a blank sample; all PFA sample bottles containing thick oxide layer collection droplets and blank sample bottles are placed on a ceramic or PTFE coated heating plate, the temperature is adjusted to 150-200° C., and heated for about 30 min to 60 min until the liquid in the FPA sample bottle is dried; the heating plate is turned off and the temperature is lowered to room temperature.

[0018] Preferably, use a pipette to transfer 5-10 ml of 2-10% HF + 2-10% H2O2 prepared extraction scanning solution to the evaporated and cooled PFA sample bottle and blank sample PFA bottle, and gently shake the PFA bottle to allow the residual trace elements at the bottom of the bottle to be fully dissolved and extracted with the extraction scanning solution. The method of heating the PFA bottle to drive out silicon can drive out silicon more thoroughly, avoiding the solution entering the ICP-MS analysis containing high silicon groups, thereby obtaining the most accurate Ti element content results.

[0019] As a preferred method, the recovery rate of adding Ti standard solution to the extraction scanning liquid is verified, and Ti standard solution is added to the extraction scanning liquid at a mass ratio of 1:1, and ICP-MS is used to detect and obtain the Ti element content X1; 4 ml of the mixed solution of the extraction liquid and the standard solution is taken into a PFA sample bottle, heated to evaporate and cooled, and then 4 ml of 3-6% dilute nitric acid is used to extract the residual Ti element, and ICP-MS is used to detect and obtain the Ti element content X2; X2 / X1 is calculated as the Ti element recovery rate.

[0020] As a preferred method, the recovery rate of Ti element added to the solution after extraction scanning of the thin oxide layer is verified, Ti standard solution is added to the extraction scanning solution at a mass ratio of 1:1, and the Ti element content X1 is obtained by ICP-MS detection. 4 ml of the extraction scanning solution is added to the surface of the silicon wafer, and the entire surface of the silicon wafer is scanned by the ball method, and then poured into a PFA sample bottle, and ICP-MS is used to detect and obtain the Ti element content X2. X2 / X1 is calculated as the recovery rate of Ti element; the scanning solution is poured into a PFA sample bottle and silicon is added to drive out silicon, and then 4 ml of the scanning solution is used to extract the residual metal, and the Ti element content X3 is obtained by ICP-MS detection, and X3 / X1 is the recovery rate of Ti element after addition.

[0021] As a preferred method, the recovery rate of Ti in the solution after etching the thick oxide layer is verified, Ti standard solution is added to the extraction scanning solution at a mass ratio of 1:1, and ICP-MS is used to detect the Ti element content X1. 10 ml of the extraction scanning solution is added to the surface of the thick oxide layer of the silicon wafer, and the entire surface of the silicon wafer with a thick oxide layer of about 500 nm is etched by the ball method. After the silicon wafer is poured into a PFA sample bottle, the Ti element content X2 is obtained by ICP-MS detection, and X2 / X1 is the Ti recovery rate; the scanning solution is poured into a PFA sample bottle, silicon is added, and then 10 ml of extraction scanning is used to dissolve the residual metal, and the Ti element content X3 is obtained by ICP-MS detection; X3 / X1 is the recovery rate of Ti element after addition.

[0022] The present invention can achieve the following effects:

[0023] The present invention provides a method for manually detecting the metal content in the thick oxide layer of a silicon wafer, which has the advantages of saving time and labor, convenient operation, low cost and good stability compared with the prior art. By eliminating some test interference factors, the silicon-based content in the solution of the heating container is removed, the accuracy of ICP-MS analysis is improved, and it can be applied to batch detection and analysis. DETAILED DESCRIPTION

[0024] The technical solution of the invention is further specifically described below through embodiments.

[0025] Embodiment 1: A method for manually detecting the metal content in a thick oxide layer of a silicon wafer, comprising the following steps:

[0026] Step 1: The entire operation process needs to be carried out in a clean room environment of Class 100 or above. The pre-treatment work is completed in a fume hood. The fume hood requires a Class 10 dust-free environment with sufficient exhaust and a negative pressure state.

[0027] The fume hood has been cleaned and washed, and there is no pollution from materials such as metal and glass. The fume hood is clean, and the number of air particles with a particle size of ≥0.5μm and above is ≤1; the 400℃ ceramic or PTFE-coated heating plate is cleaned and placed in the fume hood, the PTFE film is cleaned and dried with nitrogen, and then laid on the ceramic plate or PTFE-coated plate of the heating plate.

[0028] Step 2: Place the box containing the thick oxide layer silicon wafers to be tested into the fume hood, open the box cover, use a vacuum pen to suck up the silicon wafers, and place them on the wafer rack with the thick oxide layer facing up.

[0029] Step 3: Use a pipette to transfer 3.5 ml of the prepared 33% HF solution to the surface of the silicon wafer. The thick oxide layer will react with HF quickly. Use a vacuum pen to slightly shake the silicon wafer to let the droplet roll over the entire surface of the silicon wafer and stay in the center of the silicon wafer. Do not touch the silicon wafer when pouring the hydrofluoric acid solution, and do not let the droplet fall when changing the ball.

[0030] Step 4: Place the silicon wafer on the PTFE film above the heating plate; adjust the temperature of the heating plate to 100-120°C, heat for 30-60 minutes until the droplets on the surface of the silicon wafer evaporate, turn off the heating plate, and cool to room temperature. Use evaporation to generate water-soluble hexafluorodihydrogen silicon (SiO2+6HF=H2SiF6+2H2O) generated by the reaction of silicon dioxide and hydrofluoric acid, and continue to react under heating to generate silicon tetrafluoride gas and HF gas (H2SiF6=SiF4+2HF), which volatilizes and removes silicon.

[0031] Step 5: Use a pipette to transfer 3 ml of 6% HF + 6% H2O2 to the configured scanning droplet and drop it on the surface of the silicon wafer. Use the ball rolling method to extract and recover the metal on the surface of the silicon wafer. Roll the ball twice more at the position where the hydrofluoric acid solution evaporates.

[0032] Step 6: The extract is subjected to ICP-MS analysis to obtain the Ti metal element content.

[0033] Verify the recovery rate of adding Ti standard solution to the extraction scanning liquid, add Ti standard solution to the extraction scanning liquid at a mass ratio of 1:1, and detect by ICP-MS to obtain the Ti element content X1; take 4 ml of the mixed solution of the extraction liquid and the standard solution into a PFA sample bottle, heat to evaporate and cool, then use 4 ml of 3-6% dilute nitric acid to extract the residual Ti element, and detect by ICP-MS to obtain the Ti element content X2; calculate X2 / X1 as the Ti element recovery rate.

[0034] To verify the recovery rate of Ti element added to the solution after extraction scanning of the thin oxide layer, Ti standard solution was added to the extraction scanning solution at a mass ratio of 1:1, and the Ti element content X1 was obtained by ICP-MS detection. 4 ml of extraction scanning solution was added to the surface of the silicon wafer, and the entire surface of the silicon wafer was scanned by the ball method. Then, it was poured into a PFA sample bottle and detected by ICP-MS to obtain the Ti element content X2. X2 / X1 was calculated as the recovery rate of Ti element. The scanning solution was poured into a PFA sample bottle and silicon was added to drive out silicon. Then, 4 ml of scanning solution was used to extract the residual metal. The Ti element content X3 was obtained by ICP-MS detection. X3 / X1 was the recovery rate of Ti element after addition.

[0035] To verify the Ti recovery rate in the solution after etching the thick oxide layer, Ti standard solution was added to the extraction scanning solution at a mass ratio of 1:1, and ICP-MS was used to detect the Ti element content X1. 10 ml of the extraction scanning solution was added to the surface of the thick oxide layer of the silicon wafer. The entire surface of the silicon wafer was etched with a thick oxide layer of about 500 nm by the ball rolling method, and then poured into a PFA sample bottle. ICP-MS detection was used to obtain the Ti element content X2, and X2 / X1 was the Ti recovery rate; the scanning solution was poured into a PFA sample bottle and silicon was added to drive it out, and then 10 ml of extraction scanning was used to dissolve the residual metal, and the Ti element content X3 was obtained by ICP-MS detection; X3 / X1 was the Ti element recovery rate after addition.

[0036] Embodiment 2: A method for manually detecting the metal content in a thick oxide layer of a silicon wafer, comprising the following steps:

[0037] Step 1: The entire operation process needs to be carried out in a clean room environment of Class 100 or above. The pre-treatment work is completed in a fume hood. The fume hood requires a Class 10 dust-free environment with sufficient exhaust and a negative pressure state.

[0038] The fume hood has been cleaned and washed, and there is no pollution from materials such as metal and glass. The fume hood is clean, and the number of air particles with a particle size of ≥0.5μm and above is ≤1; the 400℃ ceramic or PTFE-coated heating plate is cleaned and placed in the fume hood, the PTFE film is cleaned and dried with nitrogen, and then laid on the ceramic plate or PTFE-coated plate of the heating plate.

[0039] Step 2: Place the box containing the thick oxide layer silicon wafers to be tested into the fume hood, open the box cover, use a vacuum pen to suck up the silicon wafers, and place them on the wafer rack with the thick oxide layer facing up.

[0040] Step 3: Use a pipette to transfer 3.5 ml of the prepared 35% HF solution to the surface of the silicon wafer. The thick oxide layer will react with HF quickly. Use a vacuum pen to slightly shake the silicon wafer to let the droplet roll over the entire surface of the silicon wafer and stay in the center of the silicon wafer. Do not touch the silicon wafer when pouring the hydrofluoric acid solution, and do not let the droplet fall when changing the ball.

[0041] Step 4: Pour the droplets on the silicon wafer into the prepared 100ml PFA sample bottle and record the sample bottle number; use a pipette to transfer an equal amount of HF-prepared solution into the prepared 100ml sample bottle and record the sample bottle number as a blank sample; place all PFA sample bottles containing thick oxide layer collection droplets and blank sample bottles on a ceramic or PTFE coated heating plate, adjust the temperature to 175°C, and heat for about 45 minutes until the liquid in the FPA sample bottle is dried; turn off the heating plate and cool to room temperature. Using evaporation, the water-soluble hexafluorodihydrogen silicon generated by the reaction of silicon dioxide and hydrofluoric acid, i.e. SiO2+6HF=H2SiF6+2H2O, continues to react under heating to generate silicon tetrafluoride gas and HF gas, i.e. H2SiF6=SiF4+2HF, which volatilizes and carries out silicon removal treatment.

[0042] Step 5: Use a pipette to transfer 7.5 ml of the prepared 6% HF + 6% H2O2 extraction scanning solution and add it to the evaporated and cooled PFA sample bottle and the blank sample PFA bottle. Gently shake the PFA bottle to allow the residual trace elements at the bottom of the bottle to be fully dissolved and extracted with the extraction scanning solution.

[0043] Step 6: The extract is subjected to ICP-MS analysis to obtain the Ti metal element content.

[0044] Verify the recovery rate of adding Ti standard solution to the extraction scanning liquid, add Ti standard solution to the extraction scanning liquid at a mass ratio of 1:1, and detect by ICP-MS to obtain the Ti element content X1; take 4 ml of the mixed solution of the extraction liquid and the standard solution into a PFA sample bottle, heat to evaporate and cool, then use 4 ml of 3-6% dilute nitric acid to extract the residual Ti element, and detect by ICP-MS to obtain the Ti element content X2; calculate X2 / X1 as the Ti element recovery rate.

[0045] To verify the recovery rate of Ti element added to the solution after extraction scanning of the thin oxide layer, Ti standard solution was added to the extraction scanning solution at a mass ratio of 1:1, and the Ti element content X1 was obtained by ICP-MS detection. 4 ml of extraction scanning solution was added to the surface of the silicon wafer, and the entire surface of the silicon wafer was scanned by the ball method. Then, it was poured into a PFA sample bottle and detected by ICP-MS to obtain the Ti element content X2. X2 / X1 was calculated as the recovery rate of Ti element. The scanning solution was poured into a PFA sample bottle and silicon was added to drive out silicon. Then, 4 ml of scanning solution was used to extract the residual metal. The Ti element content X3 was obtained by ICP-MS detection. X3 / X1 was the recovery rate of Ti element after addition.

[0046] To verify the Ti recovery rate in the solution after etching the thick oxide layer, Ti standard solution was added to the extraction scanning solution at a mass ratio of 1:1, and ICP-MS was used to detect the Ti element content X1. 10 ml of the extraction scanning solution was added to the surface of the thick oxide layer of the silicon wafer. The entire surface of the silicon wafer was etched with a thick oxide layer of about 500 nm by the ball rolling method, and then poured into a PFA sample bottle. ICP-MS detection was used to obtain the Ti element content X2, and X2 / X1 was the Ti recovery rate; the scanning solution was poured into a PFA sample bottle and silicon was added to drive it out, and then 10 ml of extraction scanning was used to dissolve the residual metal, and the Ti element content X3 was obtained by ICP-MS detection; X3 / X1 was the Ti element recovery rate after addition.

[0047] In summary, this manual method for detecting the metal content in the thick oxide layer of silicon wafers has the advantages of saving time and effort, convenient operation, low cost and good stability. By eliminating some test interference factors, the silicon-based content in the heating container is removed and the silicon content in the solution is removed, the accuracy of ICP-MS analysis is improved, and it can be applied to batch detection and analysis.

[0048] The above description is only a specific embodiment of the present invention, but the structural features of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are included in the patent scope of the present invention.

Claims

1. A method for manually detecting the metal content in a thick oxide layer of a silicon wafer, characterized in that The steps are as follows: Step 1: The entire operation process needs to be carried out in a Class 100 or above clean room environment. The pre-treatment work is completed in a fume hood. The fume hood requires a Class 10 dust-free micro environment with sufficient exhaust and a negative pressure state. Step 2: Put the box containing the silicon wafer with thick oxide layer to be tested into the fume hood, open the box cover, use a vacuum pen to suck the silicon wafer, and place it on the wafer rack with the thick oxide layer facing up; Step 3: Use a pipette to transfer 2ml~5ml of the prepared 20%~49% HF solution to the surface of the silicon wafer. The thick oxide layer will react with HF quickly. Use a vacuum pen to slightly shake the silicon wafer to let the droplet roll over the entire surface of the silicon wafer and stay in the center of the silicon wafer. Step 4: Place the silicon wafer on the PTFE film above the heating plate; adjust the temperature of the heating plate to 100-120°C, heat for 30-60 minutes until the droplets on the surface of the silicon wafer evaporate, turn off the heating plate, and cool to room temperature; Step 5: Use a pipette to transfer 1-5 ml of 2-10% HF + 2-10% H2O2 to the configured scanning solution and drop it onto the surface of the silicon wafer. Use the ball rolling method to extract and recover the metal on the surface of the silicon wafer and roll it twice more at the position where the hydrofluoric acid solution evaporates; Step 6: The extract is subjected to ICP-MS analysis to obtain the Ti metal element content.

2. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 1, characterized in that: The fume hood has been cleaned and washed, and there is no pollution from materials such as metal and glass. The fume hood is clean, and the number of air particles with a particle size of ≥0.5μm and above is ≤1; the 300-500℃ ceramic or PTFE-coated heating plate is cleaned and placed in the fume hood, the PTFE film is cleaned and dried with nitrogen, and then laid on the ceramic plate or PTFE-coated plate of the heating plate.

3. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 1, characterized in that: By evaporation, the water-soluble hexafluorodihydrogen silicon generated by the reaction of silicon dioxide and hydrofluoric acid, i.e. SiO2+6HF=H2SiF6+2H2O, continues to react under heating to generate silicon tetrafluoride gas and HF gas, i.e. H2SiF6=SiF4+2HF, which is volatilized to carry out silicon removal treatment.

4. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 1, characterized in that: Pour the droplets on the silicon wafer into the prepared 100ml PFA sample bottle and record the sample bottle number; use a pipette to transfer an equal amount of HF-prepared solution to the prepared 100ml sample bottle and record the sample bottle number as a blank sample; place all PFA sample bottles containing thick oxide layer collection droplets and blank sample bottles on a ceramic or PTFE coated heating plate, adjust the temperature to 150-200°C, and heat for about 30 to 60 minutes until the liquid in the FPA sample bottle is dry; turn off the heating plate and cool to room temperature.

5. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 4, characterized in that: Use a pipette to transfer 5-10 ml of the prepared extraction scanning solution of 2-10% HF + 2-10% H2O2 and add it to the evaporated and cooled PFA sample bottle and the blank sample PFA bottle. Gently shake the PFA bottle to allow the residual trace elements at the bottom of the bottle to be fully dissolved and extracted with the extraction scanning solution.

6. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 1 or 5, characterized in that: Verify the recovery rate of adding Ti standard solution to the extraction scanning liquid, add Ti standard solution to the extraction scanning liquid at a mass ratio of 1:1, and detect by ICP-MS to obtain the Ti element content X1; take 4 ml of the mixed solution of the extraction liquid and the standard solution into a PFA sample bottle, heat to evaporate and cool, then use 4 ml of 3-6% dilute nitric acid to extract the residual Ti element, and detect by ICP-MS to obtain the Ti element content X2; calculate X2 / X1 as the Ti element recovery rate.

7. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 1 or 5, characterized in that: To verify the recovery rate of Ti element added to the solution after extraction scanning of the thin oxide layer, Ti standard solution was added to the extraction scanning solution at a mass ratio of 1:1, and the Ti element content X1 was obtained by ICP-MS detection. 4 ml of extraction scanning solution was added to the surface of the silicon wafer, and the entire surface of the silicon wafer was scanned by the ball method. Then, it was poured into a PFA sample bottle and detected by ICP-MS to obtain the Ti element content X2. X2 / X1 was calculated as the recovery rate of Ti element. The scanning solution was poured into a PFA sample bottle and silicon was added to drive out silicon. Then, 4 ml of scanning solution was used to extract the residual metal. The Ti element content X3 was obtained by ICP-MS detection. X3 / X1 was the recovery rate of Ti element after addition.

8. The method for manually detecting the metal content in a thick oxide layer of a silicon wafer according to claim 1 or 5, characterized in that: To verify the Ti recovery rate in the solution after etching the thick oxide layer, Ti standard solution was added to the extraction scanning solution at a mass ratio of 1:1, and ICP-MS was used to detect the Ti element content X1. 10 ml of the extraction scanning solution was added to the surface of the thick oxide layer of the silicon wafer. The entire surface of the silicon wafer was etched with a thick oxide layer of about 500 nm by the ball rolling method, and then poured into a PFA sample bottle. ICP-MS detection was used to obtain the Ti element content X2, and X2 / X1 was the Ti recovery rate; the scanning solution was poured into a PFA sample bottle and silicon was added to drive it out, and then 10 ml of extraction scanning was used to dissolve the residual metal, and the Ti element content X3 was obtained by ICP-MS detection; X3 / X1 was the Ti element recovery rate after addition.

Citation Information

Cited By

  • Method for testing metal on surface of substrate

    CN120721469A