Polarizing plate group and liquid crystal display device
By designing a rectangular polarizing plate group with a high phase difference value and orthogonal polarizing plate layers in the liquid crystal display device, combined with appropriate configuration of the protective film and adhesive layer, the problems of warpage and iridescence unevenness are solved, and the efficiency is improved. The heat resistance and display effect of the device.
Patent Information
- Application Number
- CN202410365910.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
In existing liquid crystal display devices, when a biaxially stretched polyester resin film is used as a protective film, it is easy to cause the laminated structure to warp in a heat-resistant environment, and it is difficult to simultaneously suppress iris unevenness, resulting in insufficient overall performance. .
Design a polarizing plate set, in which the viewing side and backlight side polarizing plates are both rectangular, with a protective film and polarizing plate layer with a high phase difference value. The absorption axes of the polarizing plate layer are orthogonal to each other, and by adjusting the rigidity ratio of the protective film and the configuration of the adhesive layer to balance the shrinkage difference of the polarizer layer to reduce the warpage of the laminated structure.
It effectively suppresses iridescent unevenness, reduces the warpage of the laminated structure in a heat-resistant environment, and improves the overall performance of the liquid crystal display device.
Smart Images

Figure CN118732128A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polarizing plate set and a liquid crystal display device. Background Art
[0002] Liquid crystal display devices are configured with polarizing plates on the viewing side and the backlight side of the liquid crystal unit based on the display principle. Each polarizing plate is a laminated body having at least a polarizer layer and a protective film for protecting the polarizer layer (for example, see Patent Document 1). As the protective film, a biaxially stretched polyester resin film having excellent mechanical properties (low moisture permeability, impact resistance) can be used.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2011-123402 Summary of the invention
[0006] Problems to be solved by the invention
[0007] When a protective film with a low phase difference value such as a biaxially stretched polyester resin film is used as a component of the viewing side polarizing plate, rainbow color unevenness (hereinafter referred to as "rainbow unevenness") is strongly generated due to its low phase difference. Here, if a protective film with a high phase difference value (such as a uniaxially stretched polyester resin film) is used to suppress the rainbow unevenness, the rainbow unevenness can be suppressed. However, if a laminated structure produced by bonding a polarizing plate having such a protective film to both sides of a glass is exposed to a heat-resistant environment of 80°C, the laminated structure as a whole will be greatly warped.
[0008] Therefore, an object of the present invention is to provide a polarizing plate set that can suppress rainbow unevenness and reduce warping of a laminated structure formed by bonding the polarizing plate set to a liquid crystal cell in a heat-resistant environment. Another object of the present invention is to provide a liquid crystal display device including the polarizing plate set.
[0009] Means for solving problems
[0010] Regarding the stacked structure having a stacked structure of "viewing side polarizing plate / liquid crystal unit / backlight side polarizing plate", according to the principle of a liquid crystal display device, the absorption axes of the polarizer layers possessed by each polarizing plate are usually orthogonal to each other. The polarizer layer has an absorption axis and therefore has anisotropy, and thus the degree of shrinkage when exposed to a heat-resistant environment is also anisotropic. Therefore, the above-mentioned stacked structure is warped as a whole due to the difference in the degree of shrinkage between the polarizer layer possessed by the viewing side polarizing plate and the polarizer layer possessed by the backlight side polarizing plate. In the case where the protective film possessed by each polarizing plate is a highly rigid protective film, the shrinkage of the polarizer layer can be suppressed and the warping of the stacked structure as a whole can be slightly eliminated, but it is difficult to achieve a balance. The inventors of the present invention have found that by making the rigidity of the protective film possessed by each rectangular polarizing plate a predetermined relationship, the warping of the stacked structure in a heat-resistant environment can be reduced, thereby completing the present invention.
[0011] The present invention provides a polarizing plate group, which is a pair of polarizing plate groups including a viewing side polarizing plate arranged on the viewing side of a liquid crystal unit and a backlight side polarizing plate arranged on the backlight side of the liquid crystal unit, the viewing side polarizing plate and the backlight side polarizing plate are both rectangular, both the viewing side polarizing plate and the backlight side polarizing plate have a polarizing layer and a protective film, the in-plane phase difference value of the protective film of the viewing side polarizing plate is greater than 6000nm, the absorption axis of the polarizing layer of the viewing side polarizing plate is oriented in the long side direction of the rectangle, the viewing side polarizing plate and the backlight side polarizing plate are arranged in a manner that the absorption axes of the polarizing layers they respectively have are orthogonal to each other, the ratio of the rigidity of the protective film of the viewing side polarizing plate in the short side direction of the rectangle to the rigidity of the protective film in the long side direction of the rectangle is greater than 2.0, and the absolute value of the difference between the rigidity of the protective film of the viewing side polarizing plate in the long side direction and the rigidity of the protective film of the backlight side polarizing plate in the long side direction is less than 90mmMPa.
[0012] The polarizing plate set of the present invention may have one or more of the following features.
[0013] The ratio of the contraction force in the longitudinal direction of the polarizer layer of the backlight-side polarizing plate to the contraction force in the longitudinal direction of the polarizer layer of the viewing-side polarizing plate may be 0.3 or more.
[0014] The ratio of the thickness of the polarizer layer of the backlight-side polarizing plate to the thickness of the polarizer layer of the viewing-side polarizing plate may be 0.6 or more.
[0015] The thickness of the polarizer layer of the backlight-side polarizing plate may be 0.015 mm or more.
[0016] The contraction force of the polarizer layer of the backlight-side polarizing plate in the longitudinal direction may be 0.8 N / 2 mm or more.
[0017] The thickness of the protective film of the viewing-side polarizing plate may be 0.06 mm or more, and the thickness of the protective film of the backlight-side polarizing plate may be 0.06 mm or less.
[0018] The polarizing layer of the viewing-side polarizing plate and the backlight-side polarizing plate may be a stretched film of polyvinyl alcohol.
[0019] Both the viewing-side polarizing plate and the backlight-side polarizing plate may have a (meth)acrylic resin film on the surface of the polarizer layer opposite to the protective film side.
[0020] Both the viewing-side polarizing plate and the backlight-side polarizing plate may be arranged so that the protective film side becomes the side away from the liquid crystal cell.
[0021] Both the viewing-side polarizing plate and the backlight-side polarizing plate may have a pressure-sensitive adhesive layer on the surface of the (meth)acrylic resin film opposite to the polarizer layer.
[0022] The present invention also provides a liquid crystal display device including a liquid crystal cell and the above polarizing plate set.
[0023] Effects of the Invention
[0024] According to the present invention, it is possible to provide a polarizing plate set that can suppress rainbow unevenness and reduce warping of a laminated structure formed by bonding the laminated structure to a liquid crystal cell in a heat-resistant environment.
[0025] Furthermore, a liquid crystal display device including the polarizing plate set can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a diagram showing a stacked structure according to one embodiment of the present invention.
[0027] Figure 2 It is a diagram showing a main part of one embodiment of the present invention.
[0028] Figure 3 It is a diagram showing measurement points of the warpage amount.
[0029] Description of Reference Numerals
[0030] 1…Liquid crystal display device, 2…Liquid crystal unit, 3…Polarizing plate group, 3A…Viewing side polarizing plate, 3B…Backlight side polarizing plate, 5A…First protective film, 5B…Third protective film, 6A…First polarizing plate layer, 6B…Second polarizing plate layer, 7A…Second protective film, 7B…Fourth protective film, 8…Adhesive layer, 9…Adhesive layer, 10…Laminated structure, 20…Glass substrate, 30…Measuring point, P1…Absorption axis of the first polarizing plate layer, P2…Absorption axis of the second polarizing plate layer, Q1…Stretching direction of the first protective film, Q2…Stretching direction of the third protective film. DETAILED DESCRIPTION
[0031] The present invention is a component of a liquid crystal display device, which is a pair of polarizing plate sets including a viewing side polarizing plate arranged on the viewing side of a liquid crystal cell and a backlight side polarizing plate arranged on the backlight side.
[0032] In addition, the present invention is a liquid crystal display device having a pair of polarizing plate groups. Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In addition, the same reference numerals are given to the same or corresponding parts in each figure, and repeated descriptions are omitted.
[0033] <Laminated structure>
[0034] like Figure 1 As shown, the liquid crystal display device 1 includes a liquid crystal cell 2 and a pair of polarizing plate groups 3 arranged in a manner of sandwiching the liquid crystal cell 2 from both sides of the liquid crystal cell 2. The pair of polarizing plate groups 3 is composed of a viewing side polarizing plate 3A arranged on one side of the liquid crystal cell 2 and a backlight side polarizing plate 3B arranged on the other side. Here, the terms "viewing side" and "backlight side" are names derived from the structure of the liquid crystal display device 1. It should be noted that Figure 1 This is a diagram showing a portion of the optical system for explaining the polarizing plate group 3 of this embodiment in the liquid crystal display device 1, and only a portion of a structure having a stacked structure such as "viewing side polarizing plate 3A / liquid crystal unit 2 / backlight side polarizing plate 3B" is shown. Hereinafter, the structure having this stacked structure is referred to as a "stacked structure" (symbol 10).
[0035] The viewing side polarizing plate 3A is laminated with a first protective film 5A, a first polarizer layer 6A, and a second protective film 7A in order from the side away from the liquid crystal cell 2. These layers are bonded to each other via an adhesive layer 8. The backlight side polarizing plate 3B is laminated with a third protective film 5B, a second polarizer layer 6B, and a fourth protective film 7B in order from the side away from the liquid crystal cell 2. These layers are bonded to each other via an adhesive layer 8.
[0036] The viewing side polarizing plate 3A and the backlight side polarizing plate 3B further have an adhesive layer 9 described later, and are respectively bonded to the liquid crystal cell 2 via the adhesive layer 9. The liquid crystal cell 2, the viewing side polarizing plate 3A, and the backlight side polarizing plate 3B are all rectangular, and are bonded so that the long side directions thereof are aligned with each other. Hereinafter, in this specification, the terms "long side direction" and "short side direction" are used based on the rectangle.
[0037] The aspect ratio of the rectangles of the viewing-side polarizing plate 3A and the backlight-side polarizing plate 3B may be such that the length in the long side direction is 1.2 to 3.0 times, 1.3 to 2.5 times, or 1.4 to 1.9 times the length in the short side direction.
[0038] Figure 2 This is a diagram in which the stacked structure 10 is decomposed and only the components related to the main part of this embodiment are extracted and drawn, and the left-right direction in the figure is drawn as the long side direction. Figure 2 As shown, the absorption axis P1 of the first polarizer layer 6A of the viewing side polarizing plate 3A is oriented in the long side direction. On the other hand, the absorption axis P2 of the second polarizer layer 6B of the backlight side polarizing plate 3B is oriented in the direction orthogonal to the absorption axis P1 of the first polarizer layer 6A, i.e., in the short side direction of the backlight side polarizing plate 3B.
[0039] <Protective film>
[0040] In the viewing side polarizing plate 3A and the backlight side polarizing plate 3B, the first protective film 5A and the third protective film 5B are respectively located at a position farther from the liquid crystal cell 2 than the first polarizing plate layer 6A and the second polarizing plate layer 6B. On the other hand, the second protective film 7A and the fourth protective film 7B are respectively located at a position closer to the liquid crystal cell 2 than the first polarizing plate layer 6A and the second polarizing plate layer 6B. Among them, the first protective film 5A and the third protective film 5B contribute to suppressing the shrinkage of the first polarizing plate layer 6A and the second polarizing plate layer 6B.
[0041] (First protective film and third protective film)
[0042] The first protective film 5A includes an optically transparent thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins such as chain polyolefin resins (polyethylene resins, polypropylene resins, etc.), cyclic polyolefin resins (norbornene resins, etc.); cellulose resins (cellulose ester resins, etc.); polyester resins (polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc.); polycarbonate resins; (meth) acrylic resins; polystyrene resins; polyetheretherketone resins; polysulfone resins, or mixtures and copolymers thereof. Among them, polyester resins are preferred.
[0043] Specific examples of the polyester-based resin include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polycyclohexane dimethyl terephthalate, and polycyclohexane dimethyl naphthalate.
[0044] The thickness of the first protective film 5A can be 10 μm to 200 μm, preferably 30 μm to 120 μm, more preferably 40 μm to 100 μm, further preferably 50 μm to 90 μm, and particularly preferably 60 μm to 85 μm. If the thickness of the first protective film 5A is 10 μm or more, there is a tendency that the web handleability of the film is high. On the other hand, if the thickness is 200 μm or less, it is preferred from the viewpoint of thin filming of the polarizing plate.
[0045] The first protective film 5A preferably has an elastic modulus within a specified range. The elastic modulus in the long side direction (also the direction parallel to the absorption axis P1 of the first polarizer layer 6A) can be 1400MPa to 2300MPa, preferably 1500MPa to 2200MPa, and more preferably 1600MPa to 1900MPa. The elastic modulus in the short side direction (also the direction orthogonal to the absorption axis P1 of the first polarizer layer 6A) can be 3600MPa to 4600MPa, preferably 3800MPa to 4400MPa, and more preferably 3950MPa to 4200MPa. Here, the elastic modulus refers to the tensile elastic modulus at 80°C. A rectangular test piece cut into a specified length is stretched along the long side direction using a tensile testing machine, and the tensile elastic modulus can be calculated based on the slope of the initial straight line in the obtained stress-strain curve.
[0046] The in-plane phase difference value of the first protective film 5A is 6000nm or more. The in-plane phase difference value is preferably 7000nm or more, more preferably 8000nm or more, and further preferably 10000nm or more. In this way, if the in-plane phase difference value is high, the number of peaks and valleys of the transmittance spectrum in the visible light wavelength region increases, so that almost all wavelengths of light in the wavelength region are transmitted. Therefore, the transmitted light is close to white light, so the rainbow unevenness is reduced.
[0047] The in-plane phase difference value of the first protective film 5A can be controlled to a specific range by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, a high phase difference value can be easily obtained by increasing the stretching ratio, lowering the stretching temperature, and increasing the thickness of the film. The in-plane phase difference value can be set by selecting the film forming conditions and thickness from the above conditions in consideration of the physical properties required for processing.
[0048] The first protective film 5A may be a single layer or may be composed of multiple layers. A film composed of multiple layers may be produced by coextrusion. In addition, from the viewpoint of increasing the elastic modulus to the above numerical range and from the viewpoint of increasing the phase difference to the above numerical value, the first protective film 5A is preferably a uniaxially stretched film. Figure 2 As shown, in the stacked structure 10, the stretching direction Q1 of the first protective film 5A is preferably the short-side direction.
[0049] The first protective film 5A may also have an anti-reflection layer on the surface opposite to the first polarizer layer 6A. The surface reflectivity of the anti-reflection layer is preferably 5.7% or less. If the surface reflectivity of the anti-reflection layer is 5.7% or less, there is a tendency that rainbow unevenness is not easily observed. The reason is not clear, but it is speculated that the interface reflectivity of the first protective film 5A containing the anti-reflection layer and the air is reduced. The surface reflectivity of the anti-reflection layer is more preferably 5.0% or less, further preferably 3.5% or less, and particularly preferably 2.0% or less. The lower limit of the surface reflectivity of the anti-reflection layer is not particularly limited, for example, 0.01%. The reflectivity can be measured by any method. For example, for the first protective film 5A that is bonded to a black acrylic plate via an adhesive on the opposite side of the anti-reflection layer side of the first protective film 5A monomer, a spectrophotometer (KonicaMinolta Japan Co., Ltd., CM-2600d) can be used to measure the light reflectivity at a wavelength of 550nm from the surface of the anti-reflection layer side.
[0050] The antireflection layer may be a single layer or a multilayer. Examples of the antireflection layer include a hard coat layer having fine irregularities on the surface and having an antiglare property for preventing glare from reflected light from the outside.
[0051] The anti-glare hard coating layer includes an anti-glare hard coating layer in which a filler is dispersed inside the hard coating layer to form a surface concavo-convex shape, and an anti-glare hard coating layer in which a surface concavo-convex shape is formed on the hard coating layer by an embossing method, etc. For example, when an ultraviolet curable resin is used to form the anti-glare hard coating layer, a resin composition in which a filler is dispersed in the ultraviolet curable resin may be applied to the first protective film 5A and irradiated with ultraviolet rays, or an ultraviolet curable resin may be applied to the first protective film 5A and irradiated with ultraviolet rays in a state where the coating film is closely attached to the concavo-convex surface of the mold.
[0052] As another form of the anti-reflection layer, when the anti-reflection layer is a single layer, if the thickness of the low refractive index layer composed of a material with a lower refractive index than the first protective film 5A is formed to be 1 / 4 wavelength or an odd multiple of the wavelength of light, an anti-reflection effect can be obtained. In addition, when the anti-reflection layer is a multilayer, if the low refractive index layer and the high refractive index layer are alternately made into two or more layers, and the thickness of each layer is appropriately controlled to be stacked, an anti-reflection effect can be obtained. In addition, a hard coating layer can also be stacked between the anti-reflection layer and the first protective film 5A as needed.
[0053] A known antireflection layer can be used as the antireflection layer. The antireflection layer is preferably formed by coating an organic thin film having a lower refractive index than the first protective film 5A or a hard coat layer laminated on the first protective film 5A.
[0054] The ratio of the rigidity in the short side direction of the first protective film 5A to the rigidity in the long side direction is 2.0 or more. The ratio is preferably 2.1 or more, more preferably 2.2 or more, and further preferably 2.3 or more. As the upper limit of the ratio, 5.0, 4.0, and 3.0 can be cited. Here, rigidity refers to the product of the elastic modulus and the thickness of the film.
[0055] For example, the rigidity of a film having an elastic modulus of 1705 MPa and a thickness of 0.08 mm (80 μm) is expressed as the product of these factors to be 136.4 (unit: “mm·MPa”).
[0056] The first protective film 5A may have a rigidity in the long-side direction of 60 mm·MPa to 200 mm·MPa, preferably 80 mm·MPa to 180 mm·MPa, and more preferably 100 mm·MPa to 160 mm·MPa. The rigidity in the short-side direction may be 100 mm·MPa to 400 mm·MPa, preferably 130 mm·MPa to 360 mm·MPa, and more preferably 160 mm·MPa to 340 mm·MPa.
[0057] The third protective film 5B plays an important role in reducing the warping of the laminated structure 10 together with the first protective film 5A. That is, the first protective film 5A and the third protective film 5B play a role in suppressing the shrinkage of the first polarizer layer 6A and the second polarizer layer 6B, respectively. From the viewpoint of suppressing the shrinkage of each polarizer layer from both sides of the liquid crystal cell 2, the third protective film 5B has the following properties.
[0058] The material constituting the third protective film 5B may be the same material as the thermoplastic resin constituting the first protective film 5A. The thermoplastic resin constituting the third protective film 5B may be the same type as the thermoplastic resin constituting the first protective film 5A, or may be different from the thermoplastic resin constituting the first protective film 5A.
[0059] Considering the balance with the rigidity of the first protective film 5A, the thickness of the third protective film 5B may be 10 μm to 100 μm, preferably 20 μm to 80 μm, more preferably 25 μm to 70 μm, further preferably 30 μm to 65 μm, and particularly preferably 35 μm to 60 μm.
[0060] The third protective film 5B preferably has an elastic modulus within a specified range. The elastic modulus in the long side direction (also the direction orthogonal to the absorption axis P2 of the second polarizer layer 6B) can be 2000MPa to 4500MPa, preferably 2200MPa to 4300MPa, and more preferably 2400MPa to 4100MPa. The elastic modulus in the short side direction (also the direction parallel to the absorption axis P2 of the second polarizer layer 6B) can be 1800MPa to 3200MPa, preferably 2000MPa to 3000MPa, and more preferably 2200MPa to 2800MPa.
[0061] The in-plane phase difference value of the third protective film 5B does not need to be as high as the in-plane phase difference of the first protective film 5A. Even if the third protective film 5B is in a shape that produces rainbow unevenness, the rainbow unevenness from the third protective film 5B is not easily observed in the liquid crystal display device 1. It is speculated that this is because the unpolarized light emitted by the backlight passes through the third protective film 5B, so the effect on the effect that the polarizing plate group 3 of this embodiment should exert is particularly small. The third protective film 5B can be a uniaxially stretched film or a biaxially stretched film.
[0062] The rigidity of the third protective film 5B in the long side direction can be 60 mm·MPa to 300 mm·MPa, preferably 80 mm·MPa to 250 mm·MPa, and more preferably 100 mm·MPa to 200 mm·MPa. The rigidity in the short side direction can be 60 mm·MPa to 200 mm·MPa, preferably 70 mm·MPa to 170 mm·MPa, and more preferably 80 mm·MPa to 135 mm·MPa.
[0063] The absolute value of the difference between the longitudinal rigidity of the first protective film 5A and the longitudinal rigidity of the third protective film 5B is 90 mm·MPa or less, preferably 70 mm·MPa or less, more preferably 50 mm·MPa or less, and further preferably 30 mm·MPa or less.
[0064] (Second protective film and fourth protective film)
[0065] The second protective film 7A and the fourth protective film 7B may be made of the same material as the thermoplastic resin constituting the first protective film 5A. Among them, (meth) acrylic resin or cellulose ester resin having excellent mechanical properties, transparency, cost, etc. is preferred. In this specification, "(meth) acrylic" refers to acrylic and / or methacrylic.
[0066] The (meth)acrylic resin may be a polymer having a structural unit derived from methacrylate as the main body (for example, containing 50% or more of the structural unit by mass), and is preferably a copolymer having other copolymer components copolymerized thereon. The (meth)acrylic resin may contain two or more structural units derived from methacrylate. Specifically, as (meth)acrylate, alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate may be cited, and the number of carbon atoms of the alkyl group is usually about 1 to 8. In addition, as polymerizable monomers that can be copolymerized with (meth)acrylate, styrene monomers such as styrene and alkylstyrene may be cited; monofunctional monomers such as unsaturated nitriles such as acrylonitrile and methacrylonitrile, and alkenyl esters of unsaturated carboxylic acids such as allyl (meth)acrylate and methallyl (meth)acrylate; dienyl esters of dibasic acids such as diallyl maleate; polyfunctional monomers such as unsaturated carboxylic acid diesters of diols such as alkylene glycol di(meth)acrylate. The (meth)acrylic resin film may contain two or more (meth)acrylic resins. The (meth)acrylic resin may be a resin composition mixed with additives added as needed.
[0067] As the (meth)acrylic resin, a (meth)acrylic resin having a ring structure can be used. As the (meth)acrylic resin having a ring structure, for example, a (meth)acrylic resin having a lactone ring structure, and a (meth)acrylic resin having a glutaric anhydride structure, a glutarimide structure, etc. can be cited. This is because the (meth)acrylic resin having a ring structure has high heat resistance, high moisture and heat resistance, high transparency, and has high mechanical strength by biaxial stretching.
[0068] Examples of the (meth)acrylic resin having a ring structure such as a lactone ring structure include resins described in JP-A-2000-230016, JP-A-2001-151814, JP-A-2002-120326, JP-A-2002-254544, and JP-A-2005-146084.
[0069] Examples of the (meth)acrylic resin having a glutaric anhydride structure, a glutarimide structure, and the like include resins described in JP-A-6-256537, JP-A-6-11615, and JP-A-2009-203348.
[0070] A film made of a (meth)acrylic resin does not easily generate phase difference in an unstretched state, but generates phase difference when stretched. Therefore, a substance functioning as a phase difference reducing agent may be added to the (meth)acrylic resin so that phase difference does not generate even when stretched.
[0071] Examples of the phase difference reducing agent include styrene-acrylonitrile copolymers, etc. The phase difference value can be controlled by the stretching ratio and the amount of the phase difference reducing agent added.
[0072] From the viewpoint of the impact resistance and film forming property of the film, the (meth) acrylic resin preferably contains acrylic rubber particles. Relative to the total amount of 100% by mass of the (meth) acrylic resin and the acrylic rubber particles, the amount of acrylic rubber particles that can be contained in the (meth) acrylic resin is preferably 5% by mass or more, and more preferably 10% by mass or more. The upper limit of the amount of acrylic rubber particles is not critical, but if the amount of acrylic rubber particles is too much, the surface hardness of the film is reduced, and in addition, when the film is subjected to surface treatment, the solvent resistance to the organic solvent in the surface treatment agent is reduced. Therefore, the amount of acrylic rubber particles that can be contained in the (meth) acrylic resin is preferably 80% by mass or less, and more preferably 60% by mass or less.
[0073] Specific examples of cellulose ester resins include cellulose acetate, propionate, butyrate, and mixed esters thereof, among which triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, and cellulose acetate butyrate are preferred.
[0074] The thermoplastic resin constituting the second protective film 7A and the fourth protective film 7B may be the same type as the thermoplastic resin constituting the first protective film 5A, or may be different from the thermoplastic resin.
[0075] The thickness of the second protective film 7A and the fourth protective film 7B can be 1 μm to 150 μm, preferably 5 μm to 100 μm, and more preferably 10 μm to 60 μm. The thickness is more preferably 50 μm or less, and more preferably 30 μm or less. Reducing the thickness of the second protective film 7A and the fourth protective film 7B is conducive to thinning the viewing side polarizing plate 3A and the backlight side polarizing plate 3B.
[0076] Both the second protective film 7A and the fourth protective film 7B may be uniaxially stretched films or biaxially stretched films.
[0077] <Polarizing Plate Layer>
[0078] The first polarizer layer 6A and the second polarizer layer 6B each include a polarizer. The first polarizer layer 6A and the second polarizer layer 6B may also be polarizers themselves.
[0079] A polarizer is a film having the property of absorbing linear polarized light having a vibration plane parallel to its absorption axis and transmitting linear polarized light having a vibration plane orthogonal to the absorption axis (parallel to the transmission axis). For example, the polarizer may be a film formed by adsorbing and aligning a dichroic pigment on a polyvinyl alcohol-based resin film, or may be a cured film formed by aligning a dichroic pigment in a polymerizable liquid crystal compound and polymerizing the polymerizable liquid crystal compound.
[0080] The polarizer may be any of an absorption polarizer (selectively transmitting linear polarized light in a certain direction from natural light as described above, and absorbing linear polarized light in another direction), a reflection polarizer (reflecting linear polarized light in another direction), and a scattering polarizer (scattering linear polarized light in another direction), but an absorption polarizer is preferred from the viewpoint of excellent visibility when the polarizing plate is applied to a liquid crystal display device, etc. Among them, the polarizer is more preferably a polyvinyl alcohol polarizer composed of a polyvinyl alcohol resin, further preferably a polyvinyl alcohol polarizer formed by adsorbing and aligning a dichroic pigment such as iodine and a dichroic dye on a polyvinyl alcohol resin film, and particularly preferably a polyvinyl alcohol polarizer formed by adsorbing and aligning iodine on a polyvinyl alcohol resin film.
[0081] Polyvinyl alcohol resin can be obtained by saponifying polyvinyl acetate resin. As polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of monomers copolymerizable with vinyl acetate and vinyl acetate can also be mentioned. As monomers copolymerizable with vinyl acetate, unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, (methyl) acrylamides having ammonium groups can be mentioned. As dichroic pigments, iodine and dichroic organic dyes can be used.
[0082] A polarizing plate as a film formed by adsorbing a dichroic dye on a polyvinyl alcohol resin film and orienting the film can be manufactured, for example, through the following steps: a dyeing step of dyeing the polyvinyl alcohol resin film with a dichroic dye; a crosslinking step of treating the film after the dyeing step with a crosslinking bath containing a crosslinking agent; and a stretching step of uniaxially stretching the film.
[0083] The method for manufacturing a polarizing plate may further include other steps other than those described above. Examples of other steps include a swelling step for swelling the film before the dyeing step; a water washing step for washing the film surface after the cross-linking step; a drying step for drying the polyvinyl alcohol-based resin film after the cross-linking step; an electromagnetic wave irradiation step for irradiating the film with electromagnetic waves after the cross-linking step; a color correction step for adjusting the color tone of the film after the cross-linking step; and a high temperature and high humidity step for subjecting the film after the cross-linking step to high temperature and high humidity treatment.
[0084] The stretching step, that is, uniaxial stretching of the polyvinyl alcohol-based resin film may be performed simultaneously with the other optional step treatments described above.
[0085] The various treatment processes included in the method for manufacturing a polarizer can be continuously implemented by continuously conveying a polyvinyl alcohol-based resin film as a raw material film along a film conveying path of a polarizer manufacturing device. The film conveying path is equipped with equipment (treatment bath, furnace, etc.) for implementing the above-mentioned various treatment processes in the order in which they are implemented. The treatment bath refers to a bath containing a treatment liquid for treating the polyvinyl alcohol-based resin film, such as a swelling bath, a dyeing bath, a cross-linking bath, and a cleaning bath.
[0086] The thickness of the first polarizer layer 6A can be 5 μm to 40 μm, preferably 10 μm to 35 μm, and more preferably 15 μm to 25 μm. The thickness of the second polarizer layer 6B can be 5 μm to 50 μm, preferably 10 μm to 40 μm, and more preferably 15 μm to 30 μm. The ratio of the thickness of the second polarizer layer 6B to the thickness of the first polarizer layer 6A (the thickness of the second polarizer layer 6B / the thickness of the first polarizer layer 6A) can be 0.6 or more, preferably 0.7 or more, and more preferably 0.9 or more.
[0087] The shrinkage force in the long side direction (also the direction parallel to the absorption axis P1) of the first polarizer layer 6A can be 2.0N / 2mm~6.0N / 2mm, preferably 3.0N / 2mm~5.0N / 2mm. The shrinkage force in the long side direction (also the direction orthogonal to the absorption axis P2) of the second polarizer layer 6B can be 0.8N / 2mm~3.0N / 2mm, preferably 1.5N / 2mm~2.5N / 2mm. Here, the shrinkage force refers to the shrinkage force in the long side direction generated when the test piece cut into a rectangular shape of a specified length is kept in the machine and kept at 80°C for 4 hours in a manner to maintain the size. It should be noted that the shrinkage force of the first polarizer layer 6A and the second polarizer layer 6B can be obtained by adjusting the thickness of the unstretched original film, the amount of boron contained in the cross-linking bath when manufacturing the polarizer, the immersion time in the cross-linking solution, the temperature of the cross-linking bath, and the total stretching ratio based on the original film.
[0088] The ratio of the contraction force in the long-side direction of the second polarizer layer 6B to the contraction force in the long-side direction of the first polarizer layer 6A (contraction force in the long-side direction of the second polarizer layer 6B / contraction force in the long-side direction of the first polarizer layer 6A) can be 0.3 or more, preferably 0.4 or more. The upper limit of the ratio can be 1.0 or less, preferably 0.8 or less, and more preferably 0.6.
[0089] <Adhesive Layer>
[0090] As the adhesive layer 8 for bonding the polarizer layers and the protective films to each other, a water-based adhesive or a curable adhesive that cures by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays can be used.
[0091] As the composition of the water-based adhesive, for example, a composition obtained by dissolving a polyvinyl alcohol resin or a carbamate resin in water as the main component, and a composition obtained by dispersing a polyvinyl alcohol resin or a carbamate resin in water as the main component can be cited. The composition of the water-based adhesive can further contain curing components such as polyaldehyde, melamine compounds, zirconium oxide compounds, zinc compounds, glyoxal compounds, water-soluble epoxy resins, and crosslinking agents. As the composition of the water-based adhesive, for example, an adhesive composition described in Japanese Patent Publication No. 2010-191389, an adhesive composition described in Japanese Patent Publication No. 2011-107686, a composition described in Japanese Patent Publication No. 2020-172088, and a composition described in Japanese Patent Publication No. 2005-208456 can be cited.
[0092] As the composition of the curable adhesive, it is preferred to be an active energy ray-curable adhesive composition containing a curable (polymerizable) compound as a main component and cured by irradiation with active energy rays. As the active energy ray-curable adhesive composition, there can be mentioned a cationic polymerizable adhesive composition containing a cationic polymerizable compound as a curable compound, a free radical polymerizable adhesive composition containing a free radical polymerizable compound as a curable compound, and a mixed adhesive composition containing both a cationic polymerizable compound and a free radical polymerizable compound as curable compounds.
[0093] Cationic polymerizable compounds are compounds or oligomers that are cured by cation polymerization reaction by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or by heating, and specifically include epoxy compounds, oxetane compounds, vinyl compounds, etc. Examples of epoxy compounds include alicyclic epoxy compounds (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule) such as 3,4-epoxycyclohexanecarboxylic acid 3,4-epoxycyclohexylmethyl ester; aromatic epoxy compounds (compounds having an aromatic ring and an epoxy group in the molecule) such as diglycidyl ether of bisphenol A; aliphatic epoxy compounds (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule) such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether, etc. Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.
[0094] Examples of the cationically polymerizable adhesive composition include cationically polymerizable compositions described in JP-A Nos. 2016-126345 and 2021-113969.
[0095] The free radical polymerizable compound is a compound or oligomer that is cured by free radical polymerization reaction by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or heating, and specifically, a compound having an ethylenically unsaturated bond can be mentioned. As the compound having an ethylenically unsaturated bond, a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, a vinyl compound having one or more vinyl groups in the molecule, etc. can be mentioned.
[0096] Examples of the radical polymerizable adhesive composition include radical polymerizable compositions described in JP-A-2016-126345, JP-A-2016-153474, and International Publication No. 2017 / 183335.
[0097] When the adhesive layer is formed of a water-based adhesive composition, its thickness may be, for example, 5 μm or less, preferably 1 μm or less, more preferably 0.5 μm or less, and may be 0.01 μm or more, preferably 0.05 μm or more. When the adhesive layer is formed of a curable adhesive composition (preferably an active energy ray-curable adhesive composition), its thickness may be, for example, 15 μm or less, preferably 10 μm or less, more preferably 5 μm or less, and may be 0.1 μm or more, preferably 0.3 μm or more, more preferably 0.5 μm or more.
[0098] <Adhesive Layer>
[0099] The viewing side polarizing plate 3A and the backlight side polarizing plate 3B are both bonded to the liquid crystal cell 2 via an adhesive layer 9. The adhesive layer 9 can be obtained by, for example, dissolving or dispersing an adhesive component in a solvent to prepare an adhesive composition, applying the adhesive composition on a release film, and drying the adhesive composition. The adhesive composition is bonded to the second protective film 7A side of the viewing side polarizing plate 3A and the fourth protective film 7B side of the backlight side polarizing plate 3B, respectively, and the release film is peeled off to bond to the liquid crystal cell 2.
[0100] Examples of the adhesive composition constituting the adhesive layer 9 include adhesive compositions containing (meth)acrylic resins, silicone resins, polyester resins, polyurethane resins, polyether resins, etc. as base polymers. Among them, (meth)acrylic adhesive compositions containing (meth)acrylic resins are preferred from the viewpoints of transparency, adhesive strength, reliability, heat resistance, reworkability, etc.
[0101] The thickness of the adhesive layer 9 is determined based on adhesive strength and the like, and is, for example, 1 μm to 50 μm, preferably 2 μm to 40 μm, and more preferably 3 μm to 30 μm.
[0102] <Liquid Crystal Unit>
[0103] A conventionally known liquid crystal cell can be used as the liquid crystal cell 2. The thickness of the liquid crystal cell 2 may be 0.2 mm to 20 mm, preferably 0.4 mm to 10 mm, more preferably 0.6 to 5 mm, and even more preferably 0.8 to 3 mm.
[0104] <Effect>
[0105] Usually, the stacked structure of "viewing side polarizing plate / liquid crystal unit / backlight side polarizing plate" constituted as a part of a liquid crystal display device is usually rectangular, and the viewing side polarizing plate and the backlight side polarizing plate are also rectangular. In addition, the stacked structure as a whole is often designed in such a way that the absorption axis of the polarizer layer of the viewing side polarizing plate is oriented in the long side direction. In this case, the stacked structure is warped in such a way that the viewing side polarizing plate side becomes a concave surface. Here, "warping" refers to the time-dependent change after the manufacture of the stacked structure, or the warping generated in the heat-resistant environment as a test of the stacked structure.
[0106] It is believed that the cause of the warping is caused by the difference in the degree of contraction between the polarizer layer of the viewing side polarizer and the polarizer layer of the backlight side polarizer. When the polarizer generally has a cross-linked structure in the molecular structure, it is further cross-linked as a time-dependent change after manufacturing. In addition, when the polarizer is stretched, a force that wants to return to the state before stretching acts. As a result, the two polarizer layers shrink, and the difference in the degree of contraction leads to warping as the entire laminated structure.
[0107] In this embodiment, the first protective film 5A and the third protective film 5B have the above-mentioned relationship with respect to rigidity, so that the degree of contraction of the first polarizer layer 6A and the second polarizer layer 6B is well balanced, and the contraction difference becomes small. Therefore, it is possible to reduce the warping of the entire stacked structure 10. In addition, since the in-plane phase difference value of the first protective film 5A is greater than 6000nm, the rainbow unevenness is suppressed.
[0108] The preferred embodiments of the present invention have been described above, but the present invention is not limited to the above embodiments. For example, in the above embodiments, the viewing side polarizing plate 3A and the backlight side polarizing plate 3B are provided with a polarizing layer and protective films attached to both sides thereof with an adhesive, but the viewing side polarizing plate 3A and the backlight side polarizing plate 3B may further include other functional layers such as a phase difference layer on the side close to the liquid crystal unit 2. Alternatively, the second protective film 7A and the fourth protective film 7B may also serve as a phase difference layer.
[0109] [Example]
[0110] The following examples and comparative examples are given to more specifically illustrate the present invention. It should be noted that the present invention is not limited to the following examples. It should be noted that "%" and "parts" in the description are mass % and mass parts unless otherwise specified.
[0111] <Manufacturing and Physical Property Measurement of Each Component>
[0112] (Manufacturing Example 1: Manufacture of Polarizing Plate 1)
[0113] A long polyvinyl alcohol film (average degree of polymerization: about 2400, degree of saponification: 99.9 mol % or more, thickness: 60 μm) is continuously conveyed and immersed in a swelling bath composed of pure water at 20°C for a residence time of 31 seconds (swelling process). Then, the film pulled out from the swelling bath is immersed in a dyeing bath containing iodine at 30°C with a potassium iodide / water ratio of 2 / 100 (mass ratio) for a residence time of 122 seconds (dyeing process). Next, the film pulled out from the dyeing bath is immersed in a cross-linking bath at 56°C with a potassium iodide / boric acid / water ratio of 12 / 4.1 / 100 (mass ratio) for a residence time of 70 seconds, and then immersed in a cross-linking bath at 40°C with a potassium iodide / boric acid / water ratio of 9 / 2.9 / 100 (mass ratio) for a residence time of 13 seconds (cross-linking process). In the dyeing process and the cross-linking process, longitudinal uniaxial stretching is performed by roller-to-roller stretching in the bath. The total stretching ratio based on the original film was set to 5.5 times. Next, the film pulled out from the crosslinking bath was immersed in a cleaning bath composed of pure water at 5°C for a residence time of 3 seconds (cleaning process), and then introduced into a drying furnace at 80°C for a residence time of 190 seconds for drying (drying process), thereby obtaining a polarizer. The thickness of the polarizer obtained as above (hereinafter referred to as "polarizer 1") was 24μm.
[0114] (Manufacturing Example 2: Manufacturing of Polarizing Plate 2)
[0115] A polarizing plate was produced in the same manner as in Production Example 1 except that the thickness of the long polyvinyl alcohol film was 45 μm. The thickness of the obtained polarizing plate (hereinafter referred to as “polarizing plate 2”) was 18 μm.
[0116] (Manufacturing Example 3: Manufacturing of Polarizing Plate 3)
[0117] A polarizing plate was produced in the same manner as in Production Example 1 except that the thickness of the long polyvinyl alcohol film was changed to 30 μm. The thickness of the obtained polarizing plate (hereinafter referred to as “polarizing plate 3”) was 12 μm.
[0118] (Production Example 4: Production of polyethylene terephthalate resin (1))
[0119] While the temperature of the esterification reaction tank was raised to 200°C, 86.4 parts of terephthalic acid and 64.6 parts of ethylene glycol were added to the esterification reaction tank to obtain a mixture. While the obtained mixture was stirred, 0.017 parts of antimony trioxide, 0.064 parts of magnesium acetate tetrahydrate, and 0.16 parts of triethylamine were added as catalysts to the obtained mixture. The gauge pressure in the esterification reaction tank was set to 0.34 MPa, and a pressurized esterification reaction was further performed at 240°C. Then, the esterification reaction tank was returned to normal pressure, and 0.014 parts of phosphoric acid were added.
[0120] Then, the temperature was raised to 260°C over 15 minutes, and 0.012 parts of trimethyl phosphate was added to obtain a mixture. After 15 minutes, the obtained mixture was dispersed using a high-pressure disperser, and after further 15 minutes, the obtained esterification reaction product was transferred to a polycondensation reaction tank and subjected to a polycondensation reaction under reduced pressure at 280°C.
[0121] After the polycondensation reaction is completed, the product is filtered using a NASLON filter with a 95% cutoff diameter of 5 μm, extruded from a nozzle into a bundle, cooled and solidified using cooling water that has been previously filtered (pore size: less than 1 μm), and cut into pellets to obtain polyethylene terephthalate resin (hereinafter referred to as "PET (1)").
[0122] (Production Example 5: Production of polyethylene terephthalate resin (2))
[0123] 10 parts of the dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) were mixed with 90 parts of PET (1) obtained in Production Example 4, and a polyethylene terephthalate resin (2) (hereinafter referred to as "PET (2)") containing an ultraviolet absorber was obtained using a kneading extruder.
[0124] (Production Example 6: Preparation of Coating Liquid for Forming Easy Adhesion Layer)
[0125] A water-dispersible sulfonic acid metal base-containing copolyester resin was prepared by subjecting a dicarboxylic acid component composed of 46 mol % of terephthalic acid, 46 mol % of isophthalic acid and 8 mol % of sodium 5-sulfoisophthalate to an ester exchange reaction and a polycondensation reaction with a diol component composed of 50 mol % of ethylene glycol and 50 mol % of neopentyl glycol.
[0126] Next, 51.4 parts of water, 38 parts of isopropyl alcohol, 5 parts of n-butyl cellosolve and 0.06 parts of nonionic surfactant were mixed to obtain a mixture. While the obtained mixture was heated and stirred to 77° C., 5 parts of the above-mentioned water-dispersible copolyester resin containing a sulfonic acid metal base was added, and stirring was continued until the lumps of the resin disappeared to obtain a resin aqueous dispersion. The obtained resin aqueous dispersion was cooled to 25° C. to obtain a uniform water-dispersible copolyester resin liquid with a solid content concentration of 5.0% by mass.
[0127] 3 parts of agglomerated silica particles were dispersed in 50 parts of water to obtain an aqueous dispersion of agglomerated silica particles. 0.54 parts of the aqueous dispersion of agglomerated silica particles was added to 99.46 parts of the water-dispersible copolyester resin solution, and 20 parts of water was further added while stirring to obtain a coating solution for forming an easily adhesive layer.
[0128] (Manufacturing Example 7: Manufacture of Protective Film 1)
[0129] In order to produce a film consisting of three layers, namely, layer A, layer B, and layer C, using two extruders, PET (1) was dried and supplied to extruder 1 (for outer layer A and outer layer C). In addition, PET (3) mixed with 90 parts of PET (1) produced in Production Example 4 and 10 parts of PET (2) produced in Production Example 5 was dried under reduced pressure at 135°C for 6 hours and then supplied to extruder 2 (for intermediate layer B). PET (1) supplied to extruder 1 and PET (3) supplied to extruder 2 were dissolved at 285°C. The two polymers were filtered using a filter material of a stainless steel sintered body (nominal filtration accuracy 10 μm, 95% particle interception), stacked using two types of three-layer confluence blocks, extruded from a tube head into a sheet, and then wound on a casting drum with a surface temperature of 30°C using an electrostatic casting method to cool and solidify to produce an unstretched PET film. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of the A layer, the B layer, and the C layer became 10:80:10.
[0130] Next, the unstretched PET film was coated on both sides by a reverse roll method in an amount of 0.08 g / m 2After applying the coating liquid for forming the easy-adhesive layer in a manner, it was dried at 80°C for 20 seconds. For the unstretched PET film formed with the coating layer, a tenter stretching machine was used to stretch the film to 4.0 times in the width direction in a hot air zone at a temperature of 125°C while holding the ends of the film with a clamp. Next, while maintaining the stretching amplitude in the width direction, it was treated at a temperature of 225°C for 10 seconds, and further relaxed by 3.0% in the width direction to obtain a uniaxially stretched PET film (hereinafter referred to as "protective film 1") having an easy-adhesive layer with a film thickness of about 80μm.
[0131] (Manufacturing Example 8: Manufacture of Protective Film 2)
[0132] A mixture of 90 parts of a (meth) acrylic resin having a lactone ring structure and 10 parts of an acrylonitrile-styrene (AS) resin (lactone ring content: 28.5%) was extruded to obtain an acrylic resin film (hereinafter referred to as "protective film 2") stretched to 2.0 times in length and 2.4 times in width with a thickness of 40 μm.
[0133] (Manufacturing Example 9: Manufacture of Polarizing Plate 1 with Pressure-Sensitive Adhesive Layer)
[0134] The protective film 1 obtained in Manufacturing Example 7 and the protective film 2 obtained in Manufacturing Example 8 were subjected to corona treatment on one side, and an epoxy-based ultraviolet curable adhesive was applied to the corona treated surface using an adhesive coating device. Next, the polarizer 1 with a thickness of 24 μm obtained in Manufacturing Example 1 was overlapped on the coating layer, and then pressed and laminated using a laminating roller, thereby obtaining a polarizing plate precursor. For the polarizing plate precursor, an ultraviolet irradiation device with a conveyor belt (the lamp is a metal halide lamp manufactured by EYEGRAPHICS) was used to achieve a cumulative light intensity of 200 mJ / cm 2 The polarizing plate is obtained by irradiating ultraviolet rays from the protective film 2 side in the manner of (UVB) to cure the above-mentioned adhesive. As described above, a polarizing plate 1 having a protective film 1 (polyester resin film) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) is obtained. The polarizing plate 1 is in a form in which the uniaxial stretching direction of the protective film 1 is orthogonal to the absorption axis direction of the polarizer (stretching direction of the polarizer).
[0135] Next, an adhesive layer with a release film having a (meth) acrylic adhesive layer (thickness 20 μm) on the release-treated surface of the release film was prepared. After the surface of the (meth) acrylic resin film was corona-treated, the adhesive layer with a release film was laminated on the (meth) acrylic resin film side of the above-mentioned polarizing plate, thereby obtaining a polarizing plate 1 with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film 1 (polyester resin film) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth) acrylic resin film) / adhesive layer / release film.
[0136] (Manufacturing Example 10: Manufacture of Polarizing Plate 2 with Pressure-Sensitive Adhesive Layer)
[0137] A polarizing plate was obtained in the same manner as in Production Example 9 except that a protective film of biaxially stretched polyethylene terephthalate (PET) containing a polyester resin having a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation) was used instead of the protective film 1 obtained in Production Example 7. Thus, a polarizing plate 2 having a protective film (biaxially stretched polyester resin film having a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) was obtained.
[0138] Then, the adhesive layer and the release film were laminated in the same manner as in Manufacturing Example 9, thereby obtaining a polarizing plate 2 with an adhesive layer. The polarizing plate with an adhesive layer had a structure of protective film (38 μm thick biaxially stretched polyester resin film, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.
[0139] (Manufacturing Example 11: Manufacture of Polarizing Plate 3 with Pressure-Sensitive Adhesive Layer)
[0140] For the polarizing plate 2 with an adhesive layer, a protective film of biaxially stretched polyethylene terephthalate (PET) containing a polyester resin with a thickness of 38 μm (manufactured by Toray Industries, Ltd., product name: Lumirror T60) was used instead of a protective film of biaxially stretched polyethylene terephthalate (PET) containing a polyester resin with a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation). A polarizing plate 3 with an adhesive layer was obtained in the same manner as in Production Example 10. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film with a thickness of 38 μm, manufactured by Toray Industries, Ltd., product name: Lumirror T60) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.
[0141] (Manufacturing Example 12: Manufacture of Polarizing Plate 4 with Pressure-Sensitive Adhesive Layer)
[0142] As for the polarizing plate 2 with an adhesive layer, the 18 μm polarizing plate 2 prepared in Preparation Example 2 was used instead of the 24 μm polarizing plate 1 prepared in Preparation Example 1. Except for this, the same operation as in Preparation Example 10 was performed to obtain a polarizing plate 4 with an adhesive layer. The polarizing plate with an adhesive layer had a structure of protective film (biaxially stretched polyester resin film with a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizing plate 2 / adhesive layer / protective film 2 ((meth) acrylic resin film) / adhesive layer / release film.
[0143] (Manufacturing Example 13: Manufacture of Polarizing Plate 5 with Pressure-Sensitive Adhesive Layer)
[0144] For the polarizing plate 2 with an adhesive layer, a protective film of biaxially stretched polyethylene terephthalate (PET) containing a polyester resin with a thickness of 50 μm (manufactured by Toray Industries, Ltd., product name: Lumirror T60) was used instead of a protective film of biaxially stretched polyethylene terephthalate (PET) containing a polyester resin with a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation). A polarizing plate 5 with an adhesive layer was obtained in the same manner as in Production Example 10. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film with a thickness of 50 μm, manufactured by Toray Industries, Ltd., product name: Lumirror T60) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.
[0145] (Manufacturing Example 14: Manufacture of Polarizing Plate 6 with Pressure-Sensitive Adhesive Layer)
[0146] For the polarizing plate 2 with an adhesive layer, the 12 μm polarizing plate 3 prepared in Preparation Example 3 was used instead of the 24 μm polarizing plate 1 prepared in Preparation Example 1. Except for this, the same operation as in Preparation Example 10 was performed to obtain a polarizing plate 6 with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film with a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizing plate 3 / adhesive layer / protective film 2 ((meth) acrylic resin film) / adhesive layer / release film.
[0147] (Measurement of In-Plane Phase Difference of Polyester Resin Film)
[0148] The in-plane retardation values of the protective film 1 obtained in Production Example 7 and a 38 μm thick biaxially stretched polyethylene terephthalate (PET) protective film (manufactured by Mitsubishi Chemical Corporation) were measured at a wavelength of 587 nm using a retardation measuring device (manufactured by Oji Scientific Instruments Co., Ltd., KOBRA-HB-RESPC).
[0149] (Measurement of elastic modulus of protective film at 80°C)
[0150] The protective film obtained above was cut into a rectangle of 100 mm in length and 10 mm in width. Next, the upper and lower clamps of a tensile tester (Autograph AG-1S tester, manufactured by Shimadzu Corporation) were used to clamp the two ends of the long side direction of the test piece in a manner that the interval between the clamps was 50 mm, and the test piece was stretched along the long side direction at a stretching speed of 50 mm / min under an environment of 80°C. The tensile elastic modulus (MPa) of the resin film at 80°C was calculated based on the slope of the initial straight line in the obtained stress-strain curve.
[0151] Regarding the test piece, a test piece (set as test piece 1) was prepared in which the direction parallel to the absorption axis of the polarizer (stretching direction of the polarizer, MD direction) when the protective film was attached to the polarizer was the long side direction, and the direction perpendicular to the absorption axis of the polarizer (TD direction) was the width direction, and a test piece (set as test piece 2) was prepared in which the direction perpendicular to the absorption axis of the polarizer (TD direction) when the protective film was attached to the polarizer was the long side direction, and the direction parallel to the absorption axis of the polarizer (stretching direction of the polarizer, MD direction) was the width direction.
[0152] The tensile elastic modulus in the direction parallel to the absorption axis of the polarizer (stretching direction of the polarizer, MD direction) when the protective film is attached to the polarizer is obtained from Test Piece 1, and the tensile elastic modulus in the direction orthogonal to the absorption axis of the polarizer (TD direction) when the protective film is attached to the polarizer is obtained from Test Piece 2.
[0153] (Polarizer shrinkage force)
[0154] A rectangular test piece (set as Test Piece 3) with a width of 2 mm and a length of 10 mm and a long side in the stretching direction (MD, absorption axis direction) was cut out from the polarizer 1 obtained in Manufacturing Example 1 to Manufacturing Example 3. A rectangular test piece (set as Test Piece 4) with a width of 2 mm and a length of 10 mm and a long side in the direction orthogonal to the stretching direction (TD, transmission axis direction) was cut out from the polarizer obtained in Manufacturing Examples 1 to 3. The sample was placed in a thermomechanical analyzer (TMA) "EXSTAR-6000" manufactured by SIINano Technology Co., Ltd., and the shrinkage force in the long side direction generated when it was kept at 80°C for 4 hours was measured while keeping the size constant. The shrinkage force in the absorption axis direction of the polarizer was obtained from Test Piece 3, and the shrinkage in the direction orthogonal to the absorption axis direction of the polarizer was obtained from Test Piece 4.
[0155] <Example 1>
[0156] A polarizing plate 1 with an adhesive layer is prepared as a viewing-side polarizing plate, and a polarizing plate 2 with an adhesive layer is prepared as a backlight-side polarizing plate. For the polarizing plate 1 with an adhesive layer as the viewing-side polarizing plate, it is cut in a manner that the long side direction becomes a direction parallel to the absorption axis of the polarizing plate. In addition, for the polarizing plate 2 with an adhesive layer as the backlight-side polarizing plate, it is cut in a manner that the long side direction becomes a direction orthogonal to the absorption axis of the polarizing plate. The size of the polarizing plate after cutting is 150 mm×90 mm. After peeling off the release film from the polarizing plate 1 with an adhesive layer, the adhesive layer is bonded to a single surface of an alkali-free glass substrate (thickness 0.2 mm, "Eagle XG" manufactured by Corning, 160 mm×102 mm). In addition, on the surface of the above-mentioned glass substrate different from the surface bonded with the polarizing plate, in order to reproduce the stacking state of the actual liquid crystal display device, the polarizing plate 2 with an adhesive layer is bonded, sandwiched between the glass substrate 20 ( Figure 3 ) makes the absorption axes of the two polarizing plates orthogonal to each other, thereby obtaining an optical laminate with glass bonded thereto.
[0157] (Warp Evaluation)
[0158] The optical laminate bonded with glass obtained by the above method is left to stand for 48 hours in an environment with a temperature of 80°C, taken out to an environment with a temperature of 23°C and a relative humidity of 55%, and then the warping state after 2 hours is evaluated. The polarizing plate 1 with an adhesive layer (the viewing side polarizing plate) is placed on the measuring table of a two-dimensional measuring instrument (manufactured by Nikon Corporation, NEXIV (trade name) MR-12072). Next, the focus is aligned with the surface of the measuring table, and based on this, the focus is aligned with 25 points on the sample surface, and the height from the focus serving as the reference is measured. The difference between the maximum and minimum heights at the 25 measuring points is taken as the amount of warping. Specifically, Figure 3 The indicated point (symbol 30) is used as a measurement point. Figure 3 The 25 points shown are points in a region 5 mm inside the end of the polarizing plate, and are arranged at intervals of about 20 mm in the short-side direction and about 35 mm in the long-side direction. The judgment criteria for warpage evaluation are as follows.
[0159] ◎: Very small (less than 0.4 mm)
[0160] ○: Small (more than 0.4 mm and less than 0.7 mm)
[0161] Δ: Large (more than 0.7 mm and less than 1.0 mm)
[0162] ×: Very large (over 1.0 mm)
[0163] (Rainbow unevenness evaluation)
[0164] The polarizing plate 1 with an adhesive layer as the viewing side polarizing plate and the polarizing plate 2 with an adhesive layer as the backlight side polarizing plate are cut in such a way that the long side direction is parallel to the absorption axis of the polarizing plate. The size of the cut polarizing plate is 150 mm × 90 mm. After peeling off the release film from the polarizing plate 1 with an adhesive layer, the adhesive layer is bonded to a single surface of an alkali-free glass substrate (thickness 0.2 mm, "Eagle XG" manufactured by Corning, 160 mm × 102 mm). In addition, on the surface of the above-mentioned glass substrate different from the bonding surface of the polarizing plate, in order to reproduce the display state of the actual liquid crystal display device, the polarizing plate 2 with an adhesive layer is bonded, sandwiched between the glass substrate 20 ( Figure 3 ) makes the absorption axes of the two polarizing plates parallel (the transmission axes are parallel), and an optical laminate bonded with glass is obtained.
[0165] On the backlight source, the above-mentioned optical laminate bonded with glass is arranged in a manner that the polarizing plate 2 with the adhesive layer becomes the light source side, and the polarizing plate is visually observed along the inclined direction from the polyester resin film side of the polarizing plate 1 with the adhesive layer to confirm the visibility of the rainbow-like unevenness. According to the degree of uneven coloring, etc., evaluation is performed according to the following criteria.
[0166] ○: Weak rainbow unevenness
[0167] ×: Strong rainbow unevenness
[0168] <Examples 2 to 5, Comparative Examples 1 to 2>
[0169] Polarizing plates with pressure-sensitive adhesive layers bonded to both surfaces of the alkali-free glass substrate were selected in the combination shown in Table 1, and glass-bonded optical laminates of Examples 2 to 5 and Comparative Examples 1 and 2 were obtained in the same manner as in Example 1. Each glass-bonded optical laminate was evaluated for warpage and rainbow unevenness.
[0170] <Results>
[0171] The polarizing plate groups of Examples 1 to 5 satisfy both of the following: [1] the ratio of the rigidity in the short-side direction of the outer protective film (first protective film) of the viewing-side polarizing plate to the rigidity in the long-side direction (b / a) is 2.0 or more; and [2] the absolute value of the difference between the rigidity in the long-side direction of the outer protective film (first protective film) of the viewing-side polarizing plate and the rigidity in the long-side direction of the outer protective film (third protective film) of the backlight-side polarizing plate is 90 mm·MPa or less. In this case, both the warping evaluation and the rainbow unevenness evaluation are good. In contrast, the polarizing plate groups of Comparative Examples 1 and 2 that do not satisfy either of [1] or [2] above are poorly evaluated for warping or rainbow unevenness.
[0172]
Table 1
[0173]
[0174] Industrial Applicability
[0175] The present invention can be used as a constituent member of a liquid crystal display device.
Claims
1. A polarizing plate set, comprising a viewing-side polarizing plate disposed on a viewing side of a liquid crystal cell and a backlight-side polarizing plate disposed on a backlight side of the liquid crystal cell, The viewing side polarizing plate and the backlight side polarizing plate are both rectangular. The viewing side polarizing plate and the backlight side polarizing plate both have a polarizing layer and a protective film. The in-plane phase difference value of the protective film of the viewing-side polarizing plate is 6000 nm or more, The absorption axis of the polarizer layer of the viewing-side polarizing plate is oriented toward the long side direction of the rectangle. The viewing-side polarizing plate and the backlight-side polarizing plate are arranged so that the absorption axes of the polarizing film layers of the respective polarizing plates are orthogonal to each other. The ratio of the rigidity of the protective film of the viewing-side polarizing plate in the short-side direction of the rectangle to the rigidity in the long-side direction of the rectangle is 2.0 or more. An absolute value of a difference between the rigidity of the protective film of the viewing-side polarizing plate in the longitudinal direction and the rigidity of the protective film of the backlight-side polarizing plate in the longitudinal direction is 90 mm·MPa or less.
2. The polarizing plate set according to claim 1, wherein: A ratio of the contraction force in the longitudinal direction of the polarizer layer of the backlight-side polarizing plate to the contraction force in the longitudinal direction of the polarizer layer of the viewing-side polarizing plate is 0.3 or more.
3. The polarizing plate set according to claim 1, wherein: A ratio of a thickness of the polarizer layer of the backlight-side polarizing plate to a thickness of the polarizer layer of the viewing-side polarizing plate is 0.6 or more.
4. The polarizing plate set according to claim 1, wherein: The polarizer layer of the backlight-side polarizing plate has a thickness of 0.015 mm or more.
5. The polarizing plate set according to claim 1, wherein: The contraction force of the polarizer layer of the backlight-side polarizing plate in the longitudinal direction is 0.8 N / 2 mm or more.
6. The polarizing plate set according to claim 1, wherein: The protective film of the viewing-side polarizing plate has a thickness of 0.06 mm or more. The protective film of the backlight-side polarizing plate has a thickness of 0.06 mm or less.
7. The polarizing plate set according to claim 1, wherein: The polarizing layer of the viewing-side polarizing plate and the backlight-side polarizing plate is a stretched film of polyvinyl alcohol.
8. The polarizing plate set according to claim 1, wherein: The viewing-side polarizing plate and the backlight-side polarizing plate each have a (meth)acrylic resin film on the surface of the polarizer layer opposite to the protective film side.
9. The polarizing plate set according to claim 8, wherein: The viewing-side polarizing plate and the backlight-side polarizing plate are both arranged so that the protective film side is located on a side away from the liquid crystal cell.
10. The polarizing plate set according to claim 8, wherein: The viewing-side polarizing plate and the backlight-side polarizing plate each have a pressure-sensitive adhesive layer on a surface of the (meth)acrylic resin film opposite to the polarizer layer. 11 . A liquid crystal display device comprising a liquid crystal cell and the polarizing plate set according to claim 1 .