Optical laminate and image display device including the same
By using a liquid crystal alignment solidified layer and a specific adhesive layer in an optical laminate, combined with a specific laminate structure, the problems of thinning and insufficient bending resistance of polarizers with retardation layers in the prior art are solved, and high temperature performance is achieved. Excellent performance in high-humidity environments, suitable for image display devices in smart devices.
Patent Information
- Application Number
- CN202410372962.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polarizers with retardation layers have deficiencies in thinness and bending resistance. They are prone to deterioration and cracking in high-temperature and high-humidity environments, making it difficult to meet the diverse needs of smart devices.
An optical laminate composed of a polarizing plate, an orientation-cured layer of a liquid crystal compound, an adhesive layer with a Martens hardness of 150N/mm2 to 250N/mm2, and an adhesive layer with a VOC value of 100ppm or less is used, combined with a specific laminate structure and material properties to improve the thinness and bending resistance of the laminate.
The result is an optical laminate that is thin and has excellent bending resistance. It maintains good performance even in high-temperature and high-humidity environments and is suitable for use in a variety of image display devices.
Smart Images

Figure CN118732134A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical layered body and an image display device including the optical layered body. Background Art
[0002] In recent years, image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (such as organic EL display devices and inorganic EL display devices) are rapidly becoming popular. Image display devices typically use polarizers and phase difference plates. In actual use, polarizers with phase difference layers that integrate polarizers and phase difference plates are widely used (for example, Patent Document 1). As the desire for thinning of image display devices becomes stronger, the desire for thinning of polarizers with phase difference layers also becomes stronger. For the purpose of thinning polarizers with phase difference layers, the thinning of phase difference layers is underway, using phase difference layers made of liquid crystal materials. In addition, as the use of image display devices expands, the expectations for image display devices are diversified. For example, smart phones are required to be foldable. Therefore, it is strongly desired to be able to realize such a polarizer with a phase difference layer for an image display device.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 3325560 Summary of the invention
[0006] Problems to be solved by the invention
[0007] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide an optical layered body which is thin and excellent in bending resistance.
[0008] Means used to solve problems
[0009] 1. The optical laminate according to the embodiment of the present invention comprises: a polarizing plate including a polarizer; a first phase difference layer which is an alignment solidified layer of a liquid crystal compound; and an adhesive layer having a Martens hardness of 150 N / mm 2 ~250N / mm 2 ; a second phase difference layer, which is an oriented solidified layer of a liquid crystal compound; and an adhesive layer, whose VOC value is less than 100 ppm.
[0010] 2. An optical laminate according to another embodiment of the present invention comprises, in order: a polarizing plate including a polarizer; a first phase difference layer which is an alignment solidified layer of a liquid crystal compound; and an adhesive layer having a Martens hardness of 150 N / mm 2 ~250N / mm 2; a second phase difference layer, which is an orientation solidified layer of a liquid crystal compound; and an adhesive layer, whose polymerization rate is greater than 98.5%.
[0011] 3. In the optical layered body according to 1 or 2 above, the adhesive layer may have a thickness of 0.3 μm to 3 μm.
[0012] 4. In the optical layered body according to any one of 1 to 3 above, the pressure-sensitive adhesive layer may have a thickness of 10 μm to 100 μm.
[0013] 5. The total thickness of the optical layered body according to any one of 1 to 4 above may be 180 μm or less.
[0014] 6. In any one of 1 to 5 above, the optical layer stack may be: the in-plane phase difference Re(550) of the first phase difference layer is 100nm to 190nm, and satisfies Re(450) / Re(550)<1, and the angle between the slow axis of the first phase difference layer and the absorption axis of the polarizer is 40° to 50°.
[0015] 7. In any one of 1 to 5 above, the Re (550) of the first phase difference layer is 200nm to 300nm, the Re (550) of the second phase difference layer is 100nm to 200nm, the angle formed by the slow axis of the first phase difference layer and the absorption axis of the polarizer is 10° to 20°, and the angle formed by the slow axis of the second phase difference layer and the absorption axis of the polarizer is 70° to 80°.
[0016] 8. Another aspect of the present invention provides an image display device. The image display device according to an embodiment of the present invention includes the optical layered body according to any one of 1 to 6 above.
[0017] Effects of the Invention
[0018] According to the embodiment of the present invention, a thin optical layered body having excellent bending resistance can be provided. The optical layered body according to the embodiment of the present invention has excellent bending resistance even in a high-temperature and high-humidity environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention.
[0020] Explanation of symbols
[0021] 10 Polarizer
[0022] 11 Polarizer
[0023] 12. Protective layer
[0024] 13. Protective layer
[0025] 21. First phase difference layer
[0026] 22. Second phase difference layer
[0027] 30 Adhesive layer
[0028] 40 Adhesive layer
[0029] 100 Optical laminate DETAILED DESCRIPTION
[0030] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0031] (Definition of terms and symbols)
[0032] The definitions of terms and symbols in this specification are as follows.
[0033] (1) Refractive index (nx, ny, nz)
[0034] “nx” is the refractive index in the direction where the refractive index in the plane is maximum (ie, the slow axis direction), “ny” is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and “nz” is the refractive index in the thickness direction.
[0035] (2) In-plane phase difference (Re)
[0036] "Re(λ)" is the in-plane phase difference measured at 23°C with light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C with light of wavelength 550nm. Re(λ) is obtained by the formula: Re(λ) = (nx-ny) × d when the thickness of the layer (film) is set to d (nm).
[0037] (3) Retardation in the thickness direction (Rth)
[0038] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C with light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C with light of wavelength 550nm. Rth(λ) is obtained by the formula: Rth(λ) = (nx-nz) × d when the thickness of the layer (film) is set to d (nm).
[0039] (4) Nz coefficient
[0040] The Nz coefficient is obtained by Nz=Rth / Re.
[0041] (5) Angle
[0042] When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles relative to a reference direction. Therefore, for example, "45°" means ±45°.
[0043] A. Overall structure of optical laminate
[0044] Figure 1 It is a schematic cross-sectional view of an optical laminate of one embodiment of the present invention. The optical laminate 100 shown in the figure comprises, in order: a polarizer 10, a first phase difference layer 21 as an orientation solidification layer of a liquid crystal compound (hereinafter, also referred to as a liquid crystal orientation solidification layer), an adhesive layer 30, a second phase difference layer 22 as a liquid crystal orientation solidification layer, and an adhesive layer 40. Representatively, the polarizer 10 includes a polarizer 11, and protective layers 12 and 13 arranged on both sides of the polarizer 11. In the example shown in the figure, the stacking of the protective layers 12 and 13 with the polarizer 11, and the stacking of the polarizer 10 with the first phase difference layer 21 can be carried out via an adhesive layer (not shown), respectively. The adhesive layer can be an adhesive layer formed by any appropriate adhesive, or an adhesive layer formed by any appropriate adhesive. Their stacking can also be carried out directly without an adhesive layer depending on the purpose.
[0045] In the example shown in the figure, protective layers are stacked on both sides of the polarizer 11, and one protective layer (for example, the protective layer 13 disposed on the inner side) may be omitted, and the protective layer is stacked only on one side of the polarizer. The first phase difference layer 21 and the second phase difference layer 22 are liquid crystal orientation solidification layers, which are stacked via the adhesive layer 30. For the adhesive layer 30, the Martens hardness of the adhesive composition forming the adhesive layer is 150N / mm 2 ~250N / mm 2 . The optical laminate 100 is provided with an adhesive layer 40 as the outermost layer, and can be attached to an image display device (substantially an image display unit). In one embodiment of the present invention, the VOC value of the adhesive layer 40 is 100 ppm or less. In another embodiment of the present invention, the polymerization rate of the adhesive layer 40 is 98.5% or more. In actual use, it is preferred to temporarily attach a release liner to the surface of the adhesive layer 40 until the optical laminate 100 is provided for use. By temporarily attaching a release liner, the adhesive layer can be protected until actual use, and the optical laminate can be rolled up. In this specification, a "liquid crystal orientation solidified layer" refers to a layer in which a liquid crystal compound is oriented in a prescribed direction within the layer and its orientation state is fixed. In addition, an "orientation solidified layer" is a concept that includes an orientation solidified layer obtained by solidifying a liquid crystal monomer as described later.
[0046] The phase difference layer as the liquid crystal orientation solidification layer can achieve the same in-plane phase difference as the resin film with a significantly thinner thickness than the resin film. Therefore, it can contribute to the thinning of the optical laminate. On the other hand, the liquid crystal orientation solidification layer is a brittle layer, so a hard adhesive layer that can support the liquid crystal orientation solidification layer is used. If a Martens hardness of 150N / mm 2 The above adhesive layer is used as the adhesive layer of the liquid crystal orientation solidification layer, i.e., the first phase difference layer and the second phase difference layer, and the durability of the phase difference layer can be improved. On the other hand, the hard adhesive layer has a tendency to crack easily due to the bending stress during bending. The optical laminate of the embodiment of the present invention also has an adhesive layer. By having an adhesive layer, the bending resistance can be improved. In addition, in a high temperature and high humidity environment (for example, a temperature of 60°C and a humidity of 90%RH), the adhesive layer is easily deteriorated, and there is also a problem of easy cracking. The inventors found that one reason for the deterioration of the adhesive layer is the volatile components from the adhesive layer. In addition, it was found that the thickness of the liquid crystal orientation solidification layer was thin, and therefore, it was difficult to fully block the contact between the adhesive layer and the volatile components. The optical laminate of the embodiment of the present invention uses an adhesive layer with a VOC value of less than 100ppm or an adhesive layer with a polymerization rate of more than 98.5%. These adhesive layers can not only improve the bending resistance of the adhesive layer, but also suppress the generation of volatile components from the adhesive layer even when the optical laminate is placed in a high temperature and high humidity environment. The Martens hardness is 150N / mm 2 ~250N / mm 2 The optical laminate according to an embodiment of the present invention which uses a pressure-sensitive adhesive layer having a VOC value of 100 ppm or less and a pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more is not only thin and has excellent bending resistance, but also has excellent bending resistance in a high-temperature and high-humidity environment.
[0047] The total thickness of the optical laminate is 180 μm or less, preferably 50 μm to 170 μm, more preferably 70 μm to 160 μm, and further preferably 90 μm to 155 μm. In addition, in this specification, the total thickness of the optical laminate refers to the total thickness of the polarizer, the first phase difference layer and the second phase difference layer, the adhesive layer, and the adhesive layer for laminating them (that is, the total thickness of the optical laminate does not include the thickness of the release liner that can be temporarily attached to the adhesive layer 40 provided as the outermost layer and its surface).
[0048] Hereinafter, the components of the optical layered body will be described in more detail.
[0049] B. Polarizer
[0050] B-1. Polarizer
[0051] Typically, the polarizer is composed of a resin film containing a dichroic substance (typically iodine). As the resin film, any appropriate resin film that can be used as a polarizer can be used. The resin film is typically a polyvinyl alcohol resin (hereinafter referred to as "PVA resin") film. The resin film can be a single-layer resin film or a laminate of two or more layers.
[0052] As a specific example of a polarizer composed of a single-layer resin film, a polarizer obtained by subjecting a PVA-based resin film to a dyeing treatment and a stretching treatment (representatively uniaxial stretching) using iodine can be cited. The dyeing using iodine can be performed, for example, by immersing the PVA-based resin film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. Stretching can be performed after the dyeing treatment, or it can be performed while dyeing. In addition, dyeing can also be performed after stretching. As needed, the PVA-based resin film is subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. For example, by immersing the PVA-based resin film in water and washing it with water before dyeing, not only can the dirt and anti-blocking agent on the surface of the PVA-based resin film be cleaned, but the PVA-based resin film can also be swelled to prevent uneven dyeing.
[0053] As a specific example of a polarizer obtained using a laminate, there can be cited a laminate using a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate using a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. The polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be made, for example, by the following method: a PVA-based resin solution is applied to a resin substrate and dried to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; the laminate is stretched and dyed to make the PVA-based resin layer into a polarizer. In this embodiment, it is preferred to form a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution for stretching. In addition, stretching may further include stretching the laminate in the air at a high temperature (for example, above 95°C) before stretching in a boric acid aqueous solution as required. In addition, in the present embodiment, it is preferred that the laminate is subjected to a drying shrinkage treatment in which the laminate is shrunk by more than 2% in the width direction by conveying along the length direction and heating at the same time. Representatively, the manufacturing method of the present embodiment includes: sequentially performing an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, even when PVA is coated on a thermoplastic resin, the crystallinity of PVA can be improved, and high optical properties can be achieved. In addition, by simultaneously improving the orientation of PVA in advance, when immersed in water in the subsequent dyeing process and stretching process, problems such as reduction and dissolution of the orientation of PVA can be prevented, and high optical properties can be achieved. In addition, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and reduction of the orientation of the polyvinyl alcohol molecules are suppressed compared to the case where the PVA-based resin layer does not contain a halide. As a result, the optical properties of the polarizer obtained by the treatment process of immersing the laminate in a liquid such as a dyeing treatment and an underwater stretching treatment can be improved. In addition, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment. The obtained laminate of resin substrate / polarizer can be used directly (that is, the resin substrate can be made into a protective layer of polarizer), or the resin substrate can be peeled off from the laminate of resin substrate / polarizer, and any appropriate protective layer corresponding to the purpose can be stacked on the peeling surface for use. The details of the manufacturing method of such a polarizer are recorded in, for example, Japanese Patent Publication No. 2012-73580 (Japanese Patent No. 5414738) and Japanese Patent No. 6470455. The entire contents of these publications can be cited as references in this specification.
[0054] The thickness of the polarizer is preferably 1 μm to 25 μm, more preferably 1 μm to 15 μm, further preferably 1 μm to 10 μm, further preferably 1 μm to 8 μm, and particularly preferably 2 μm to 5 μm. In one embodiment, the thickness of the polarizer is 8 μm or less. In an embodiment of the present invention, even when a polarizer of the above thickness is used, a thin optical laminate with excellent bending resistance can be provided.
[0055] The polarizer preferably shows absorption dichroism at any wavelength of 380nm to 780nm. The single transmittance Ts of the polarizer is preferably 40% to 48%, more preferably 41% to 46%. The polarization degree P of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more. Representatively, the single transmittance is a Y value obtained by measuring with an ultraviolet visible spectrophotometer and correcting for visibility. The polarization degree is typically calculated by the following formula based on the parallel transmittance Tp and the orthogonal transmittance Tc obtained by measuring with an ultraviolet visible spectrophotometer and correcting for visibility.
[0056] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0057] B-2. Protective layer
[0058] The protective layer is formed by any appropriate film that can be used as the protective layer of the polarizer. As the specific example of the material that becomes the main component of the film, cellulose resins such as triacetyl cellulose (TAC), polyester, polyvinyl alcohol, polycarbonate, polyamide, polyimide, polyether sulfone, polysulfone, polystyrene, polynorbornene, polyolefin, (methyl) acrylic acid, acetate and other transparent resins can be enumerated. In addition, thermosetting resins or ultraviolet curing resins such as (methyl) acrylic acid, polyurethane, (methyl) acrylic polyurethane, epoxy, silicone can also be enumerated. In addition, glassy polymers such as siloxane polymers can also be enumerated. In addition, the polymer film recorded in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl and nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be mentioned. The polymer film can be, for example, an extrusion molding of the above resin composition.
[0059] The optical laminate is typically disposed on the visible side of the image display device, and the protective layer 12 is typically disposed on the visible side thereof. Therefore, the protective layer (outer protective layer) may be subjected to surface treatments such as hard coating, antireflection, anti-blocking, and anti-glare treatments as required.
[0060] The thickness of the protective layer is preferably 40 μm or less, more preferably 10 μm to 40 μm, and further preferably 10 μm to 30 μm. When surface treatment is performed, the thickness of the outer protective layer (protective layer 12 ) includes the thickness of the surface treatment layer.
[0061] C. Phase difference layer
[0062] As described above, the first phase difference layer and the second phase difference layer are oriented and solidified layers of liquid crystal compounds. If a liquid crystal compound is used, an in-plane phase difference equivalent to that of a resin film can be achieved with a thickness significantly thinner than that of a resin film. The phase difference layer oriented by the liquid crystal compound is thin and brittle, so there will be problems with bending resistance. In addition, the volatile components from the adhesive layer easily reach the adhesive layer, and cracking of the adhesive layer in a high temperature and high humidity environment will become a problem. As described above, in the optical laminate of the embodiment of the present invention, an adhesive layer with a VOC of less than 100 ppm, or an adhesive layer with a polymerization rate of more than 98.5% is used as the adhesive layer. If it has a Martens hardness of 150N / mm 2 ~250N / mm 2 An optical laminate having an adhesive layer with a VOC value of 100 ppm or less, an adhesive layer with a polymerization rate of 98.5% or more is not only thin and has excellent bending resistance, but also has excellent bending resistance in a high temperature and high humidity environment.
[0063] The phase difference layer typically has a circular polarization function or an elliptically polarized light function. In one embodiment, the first phase difference layer preferably has Re(550) of 100nm to 190nm, and satisfies the relationship of Re(450) / Re(550)<1, and the angle between the slow axis of the phase difference layer and the absorption axis of the polarizer is 40° to 50°. In this embodiment, the refractive index characteristics of the second phase difference layer preferably show the relationship of nz>nx=ny (hereinafter, also referred to as embodiment 1). In another embodiment of the present invention, Re(550) of the first phase difference layer is 200nm to 300nm, and Re(550) of the second phase difference layer is 100nm to 200nm. In addition, the angle between the slow axis of the first phase difference layer and the absorption axis of the polarizer is 10° to 20°, and the angle between the slow axis of the second phase difference layer and the absorption axis of the polarizer is 70° to 80° (hereinafter, also referred to as embodiment 2).
[0064] C-1. Implementation Method 1
[0065] As described above, in Embodiment 1, the first phase difference layer preferably has Re(550) of 100nm to 190nm, and satisfies Re(450) / Re(550)<1 of the phase difference layer, and the angle between the slow axis of the phase difference layer and the absorption axis of the polarizer is 40° to 50°. In this embodiment, the refractive index characteristics of the second phase difference layer preferably show the relationship of nz>nx=ny.
[0066] C-1-1. First phase difference layer
[0067] In this embodiment, the first retardation layer can function as a λ / 4 plate. The in-plane retardation Re(550) of the first retardation layer is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and further preferably 130 nm to 160 nm.
[0068] The Nz coefficient of the first retardation layer is preferably 0.9 to 1.5, and more preferably 0.9 to 1.3. When such a relationship is satisfied, when the obtained optical layered body is used in an image display device, a very excellent reflection hue can be achieved.
[0069] The thickness of the first retardation layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 7 μm, and further preferably 1 μm to 5 μm.
[0070] The first phase difference layer can show a reverse dispersion wavelength characteristic in which the phase difference value increases correspondingly with the wavelength of the measurement light, the phase difference value can show a forward wavelength dispersion characteristic in which the phase difference value decreases correspondingly with the wavelength of the measurement light, and the phase difference value can also show a flat wavelength dispersion characteristic that hardly changes with the wavelength of the measurement light. In one embodiment, the first phase difference layer preferably shows a reverse dispersion wavelength characteristic. In this case, Re(550) / Re(650) is preferably greater than 1, more preferably greater than 1 and less than 1.2, and further preferably 1.01 to 1.15. In addition, Re(450) / Re(550) of the first phase difference layer is preferably less than 1, more preferably greater than 0.8 and less than 1, and further preferably greater than 0.8 and less than 0.95. If it is such a structure, very excellent anti-reflection characteristics can be achieved. If it is such a structure, very excellent anti-reflection characteristics can be achieved.
[0071] In this embodiment, the angle between the slow axis of the first phase difference layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, and further preferably about 45°. If the angle is within such a range, as described above, as long as the first phase difference layer is a λ / 4 plate, an optical laminate having very excellent circularly polarized light properties (resulting in very excellent anti-reflection properties) can be obtained.
[0072] As described above, the first phase difference layer is preferably an oriented solidified layer of a liquid crystal compound. If a liquid crystal compound is used, the difference between nx and ny of the phase difference layer can be significantly increased compared to non-liquid crystal materials, so the thickness of the phase difference layer for obtaining the desired in-plane phase difference can be significantly reduced. As a result, the optical laminate can be further thinned.
[0073] C-1-2. Second phase difference layer
[0074] As described above, the second phase difference layer can be a so-called positive C plate whose refractive index characteristics preferably show the relationship of nz>nx=ny. If a positive C plate is used as the second phase difference layer, it is possible to prevent reflection in the oblique direction well, and the wide viewing angle of the anti-reflection function can be achieved. In this case, the phase difference Rth(550) in the thickness direction of the second phase difference layer is preferably -50nm~-300nm, more preferably -70nm~-250nm, further preferably -90nm~-200nm, and particularly preferably -100nm~-180nm. Here, "nx=ny" not only includes the case where nx and ny are strictly equal, but also includes the case where nx and ny are substantially equal. That is, the in-plane phase difference Re(550) of another phase difference layer can be less than 10nm.
[0075] The second phase difference layer having a refractive index characteristic of nz>nx=ny can be formed by any appropriate material. The second phase difference layer is preferably formed by a film containing a liquid crystal material fixed to a vertical orientation. The liquid crystal material (liquid crystal compound) capable of vertical orientation can be a liquid crystal monomer or a liquid crystal polymer. As a specific example of the liquid crystal compound and the method for forming the phase difference layer, the liquid crystal compound and the method for forming the phase difference layer described in
[0020] to
[0028] of Japanese Patent Gazette No. 2002-333642 can be cited. In this case, the thickness of the second phase difference layer is preferably 0.5μm to 10μm, more preferably 0.5μm to 8μm, and further preferably 0.5μm to 5μm.
[0076] C-2. Second Embodiment
[0077] In the second embodiment, the first phase difference layer preferably has Re (550) of 200nm to 300nm, and the angle between the slow axis of the first phase difference layer and the absorption axis of the polarizer is 10° to 20°. The second phase difference layer preferably has Re (550) of 100nm to 200nm, and the angle between the slow axis of the second phase difference layer and the absorption axis of the polarizer is 70° to 80°. In this embodiment, either the first phase difference layer or the second phase difference layer can function as a λ / 4 plate, and the other can function as a λ / 2 plate. For example, when the first phase difference layer functions as a λ / 2 plate and the second phase difference layer functions as a λ / 4 plate, the Re (550) of the first phase difference layer is preferably 200nm to 300nm, more preferably 200nm to 270nm, further preferably 210nm to 260nm, and particularly preferably 230nm to 260nm. The Re(550) of the second retardation layer is preferably 100 nm to 200 nm, more preferably 100 nm to 170 nm, further preferably 110 nm to 150 nm, particularly preferably 110 nm to 130 nm.
[0078] The thickness of the first phase difference layer can be adjusted, for example, to obtain the desired in-plane phase difference of the λ / 2 plate. The thickness of the first phase difference layer is, for example, 2.0 μm to 4.0 μm. The thickness of the second phase difference layer can be adjusted, for example, to obtain the desired in-plane phase difference of the λ / 4 plate. The thickness of the second phase difference layer is, for example, 0.5 μm to 2.5 μm.
[0079] In this embodiment, the angle formed by the slow axis of the first phase difference layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and further preferably 12° to 16°. In addition, the angle formed by the slow axis of the second phase difference layer and the absorption axis of the polarizer is preferably 70° to 80°, more preferably 72° to 78°, and further preferably 72° to 76°. In this embodiment, the first phase difference layer and the second phase difference layer can show a reverse dispersion wavelength characteristic in which the phase difference value increases accordingly with the wavelength of the measuring light, can also show a forward wavelength dispersion characteristic in which the phase difference value decreases accordingly with the wavelength of the measuring light, and can also show a flat wavelength dispersion characteristic in which the phase difference value hardly changes with the wavelength of the measuring light.
[0080] For at least one of the first phase difference layer and the second phase difference layer, the refractive index characteristic typically shows a relationship of nx>ny=nz. In addition, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within the range that does not impair the effect of the present invention, sometimes ny>nz or ny<nz can be obtained. The Nz coefficient of the phase difference layer is preferably 0.9 to 1.5, and more preferably 0.9 to 1.3.
[0081] The case where the first phase difference layer functions as a λ / 2 plate and the second phase difference layer functions as a λ / 4 plate is described, but the first phase difference layer may function as a λ / 4 plate and the second phase difference layer may function as a λ / 2 plate. In addition, the angle between the slow axis of the first phase difference layer and the absorption axis of the polarizer may be set to about 75°, and the angle between the slow axis of the second phase difference layer and the absorption axis of the polarizer may be set to about 15°.
[0082] D. Adhesive layer
[0083] As mentioned above, the Martens hardness of the adhesive layer is 150 N / mm 2 ~250N / mm 2 That is, the adhesive layer used in the embodiment of the present invention can use a Martens hardness of 150N / mm 2 ~250N / mm 2 As described above, an adhesive layer formed using an adhesive composition having high hardness tends to crack easily due to bending stress. The optical laminate of an embodiment of the present invention has an adhesive layer having a VOC value of 100 ppm or less or an adhesive layer having a polymerization rate of 98.5% or more as an adhesive layer. If such an adhesive layer is provided, the generation of volatile components from the adhesive layer can be suppressed, and an optical laminate having excellent bending resistance even in a high temperature and high humidity environment can be obtained.
[0084] The Martens hardness of the adhesive layer (more specifically, the adhesive composition forming the adhesive layer) is 150 N / mm 2 ~250N / mm 2 , more preferably 155N / mm 2 ~240N / mm 2, More preferably, it is 160N / mm 2 ~230N / mm 2 , particularly preferably 160N / mm 2 ~220N / mm 2 . If the Martens hardness of the adhesive layer is within the above range, the impact resistance is excellent. On the other hand, the generation of cracks due to bending stress during bending may become significant. If it is an optical laminate according to an embodiment of the present invention, an optical laminate having excellent bending resistance, even in a high temperature and high humidity environment, can be provided. In this specification, the Martens hardness can be measured by the following method.
[0085] <Martens hardness>
[0086] The adhesive forming the adhesive layer was applied to the glass by a rod coater and sandwiched with the glass via a spacer with a thickness of 1 μm. Next, UV light was irradiated by a UV light irradiator to cure the adhesive, and a single film of an adhesive layer with a thickness of 1 μm was formed between the glasses as an analysis sample. The obtained analysis sample was fixed to a support, and one side of the glass was removed, and nanoindentation measurement was performed under the following conditions.
[0087] Measuring device: Nanoindenter (manufactured by ELIONIX, product name "ENT-NEXUS")
[0088] Use indenter: Berkovich (triangular cone)
[0089] Measurement method: Single indentation measurement
[0090] Measurement temperature: room temperature (25°C)
[0091] Press load: 500μN
[0092] Pressing / pulling time: 10 seconds
[0093] Maximum load holding time: 1 second
[0094] The thickness of the adhesive layer is preferably 0.3 μm to 3 μm, more preferably 0.5 μm to 2.5 μm, and further preferably 0.7 μm to 2 μm. If the thickness of the adhesive layer is within the above range, the first phase difference layer and the second phase difference layer can be appropriately bonded. According to an embodiment of the present invention, an optical laminate having excellent bending resistance can be provided even if the thickness of the adhesive layer is within the above range.
[0095] As long as the adhesive layer has the above-mentioned Martens hardness, any appropriate adhesive can be used. For example, an active energy ray-curable adhesive can be used. As the active energy ray-curable adhesive, any appropriate active energy ray-curable adhesive can be used, for example, an ultraviolet curable adhesive and an electron beam curable adhesive can be mentioned.
[0096] Active energy ray-curable adhesives typically contain monofunctional components, multifunctional components (curing components) and photopolymerization initiators. The monofunctional components and multifunctional components are typically free radical polymerizable compounds, respectively. As preferred monofunctional components, for example, higher alkyl esters of (meth) acrylic acid and modified bodies thereof can be mentioned. Specifically, isostearyl acrylate, lauryl acrylate, acryloylmorpholine, unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone, etc. can be mentioned. As preferred multifunctional components, for example, monomers and / or oligomers having two or more functional groups such as (meth) acrylate groups and (meth) acrylamide groups can be mentioned. Specifically, polyethylene glycol diacrylate, trimethylolpropane triacrylate, glycerol triacrylate can be mentioned. As specific examples of monofunctional components or multifunctional components other than the above, tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, phenoxydiethylene glycol acrylate, cyclic trimethylolpropane formal acrylate, dioxanediol diacrylate, EO modified diglycerol tetraacrylate, γ-butyrolactone acrylate, N-methylpyrrolidone, hydroxyethyl acrylamide, N-hydroxymethyl acrylamide, N-methoxymethyl acrylamide, N-ethoxymethyl acrylamide, 9-vinyl carbazole can be cited. In one embodiment, the monofunctional component or the multifunctional component has a ring structure. Specifically, acryloyl morpholine, γ-butyrolactone acrylate, unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone, N-methylpyrrolidone, 9-vinyl carbazole can be cited. The monofunctional component or the multifunctional component can be used only one, or two or more can be used in combination.
[0097] As required, the active energy ray-curable adhesive may further include a cationic polymerizable compound. The cationic polymerizable compound may be monofunctional or polyfunctional. As a monofunctional cationic polymerizable compound, for example, p-tert-butylphenyl glycidyl ether and 3-ethyl-3-[(2-ethylhexyl)oxy]oxetane may be mentioned. As a polyfunctional cationic polymerizable compound, for example, 3-ethyl-3-{[(3-ethyloxetane-3-yl)methoxy]methyl}oxetane may be mentioned. As a cationic polymerizable compound, a silane coupling agent may be used. As a silane coupling agent, for example, 3-glycidoxypropyltrimethoxysilane may be mentioned.
[0098] The active energy ray-curable adhesive may further contain any appropriate additives, such as a plasticizer (for example, an oligomer component), a crosslinking agent, a diluent, etc. These additives may be used in any appropriate content according to the purpose.
[0099] The details of the active energy ray-curable adhesive are described in, for example, Japanese Patent Application Laid-Open No. 2018-017996. The description of this publication is incorporated herein by reference.
[0100] E. Adhesive layer
[0101] In one embodiment of the present invention, the VOC value of the adhesive layer is less than 100ppm. In addition, in another embodiment of the present invention, the polymerization rate of the adhesive layer is 98.5% or more. Even when these adhesive layers are placed in a high temperature and high humidity environment (e.g., a temperature of 60°C and a humidity of 90%RH), it is possible to suppress the volatilization of components that deteriorate the adhesive layer from the adhesive layer. The deterioration of the adhesive layer caused by the volatile components from the adhesive layer can be suppressed, and as a result, an optical laminate having excellent bending resistance even in a high temperature and high humidity environment can be provided.
[0102] The VOC value of the adhesive layer is 100 ppm or less, preferably 95 ppm or less, more preferably 90 ppm or less, further preferably 85 ppm or less, and particularly preferably 80 ppm or less. The VOC value of the adhesive layer can be 0 ppm. If the VOC value of the adhesive layer is within the above range, the generation of volatile components from the adhesive layer can be suppressed even in a high temperature and high humidity environment. In this specification, the VOC value is measured by the following method.
[0103] <Measurement of VOC value>
[0104] Cut the optical laminate into a size of 100 mm × 50 mm as a test body. Place the release liner of the adhesive layer attached to the test body on the table with the release liner facing upward, and arrange the sensor part of the VOC monitor (e.g., manufactured by TOYO MEDIC, product name "ppbRAE3000") at a height of 40 mm from the adhesive layer side surface of the test body (the surface after the release liner is peeled off). Next, peel the release liner from the adhesive layer and measure for 60 seconds. The maximum value in the 60-second measurement is taken as the VOC value.
[0105] The polymerization rate of the adhesive layer is 98.5% or more, more preferably 98.6% or more, and further preferably 99% or more. The polymerization rate of the adhesive layer may also be 100%. If the polymerization rate of the adhesive layer is within the above range, the generation of volatile components from the adhesive layer can be suppressed even in a high temperature and high humidity environment. The polymerization rate of the adhesive layer can be calculated by drying the adhesive layer at 130° C. for 3 hours and using the following formula based on the weight of the adhesive layer before and after drying.
[0106] Polymerization rate (%) = weight of adhesive layer after drying / weight of adhesive layer before drying × 100
[0107] The thickness of the adhesive layer is preferably 10 μm to 100 μm, more preferably 15 μm to 80 μm, and even more preferably 20 μm to 60 μm.
[0108] As long as the VOC value or weight ratio of the adhesive layer is within the above range, any appropriate adhesive composition can be used to form it. As the specific example of the adhesive constituting the adhesive layer, acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, polyurethane adhesives, epoxy adhesives, and polyether adhesives can be cited. By adjusting the type, quantity, combination and proportion of the monomers of the base resin forming the adhesive, as well as the amount of cross-linking agent, reaction temperature, reaction time, etc., it is possible to prepare an adhesive with the desired characteristics corresponding to the purpose. The base resin of the adhesive can be used only one, or two or more can be used in combination. From the viewpoints of transparency, processability and durability, acrylic adhesives (acrylic adhesive compositions) are preferred.
[0109] The acrylic adhesive typically contains a (meth)acrylic polymer as a main component. The (meth)acrylic polymer is contained in the adhesive composition in a proportion of, for example, 50 wt % or more, preferably 70 wt % or more, and more preferably 90 wt % or more of the solid content of the adhesive composition.
[0110] The (meth)acrylic polymer contains an alkyl (meth)acrylate as a monomer unit as a main component. In addition, (meth)acrylate refers to acrylate and / or methacrylate. The alkyl (meth)acrylate may be contained in the monomer component forming the (meth)acrylic polymer in a ratio of preferably 80% by weight or more, more preferably 90% by weight or more. As the alkyl group of the alkyl (meth)acrylate, for example, a linear or branched alkyl group having 1 to 18 carbon atoms can be cited. The average carbon number of the alkyl group is preferably 3 to 9, more preferably 3 to 6.
[0111] The acrylic adhesive may preferably contain a silane coupling agent and / or a crosslinking agent. As the silane coupling agent, for example, an epoxy-containing silane coupling agent may be mentioned. As the crosslinking agent, for example, an isocyanate crosslinking agent and a peroxide crosslinking agent may be mentioned. In addition, the acrylic adhesive composition may contain an antioxidant and / or a conductive agent. The details of the adhesive layer or the acrylic adhesive composition are, for example, recorded in Japanese Patent Publication No. 2006-183022, Japanese Patent Publication No. 2015-199942, Japanese Patent Publication No. 2018-053114, Japanese Patent Publication No. 2016-190996, and International Publication No. 2018 / 008712, and the contents of these publications may be cited as references in this specification.
[0112] In one embodiment, the adhesive layer is provided for annealing. If it is an adhesive layer provided after annealing, the proportion of volatile components contained in the adhesive layer can be reduced. Therefore, even if the adhesive composition itself contains volatile components, it can be suitably used as the adhesive layer of the optical laminate of the embodiment of the present invention. The annealing process can be carried out under any appropriate conditions in a manner such that the adhesive layer has the above-mentioned VOC value and / or weight ratio. For example, it can be carried out by putting the material of the adhesive layer sandwiched by a release liner into an oven. The heating temperature and the heating time can be set to any appropriate range according to the composition and thickness of the adhesive composition forming the adhesive layer. The processing temperature of the annealing process is, for example, 100°C to 140°C, preferably 105°C to 135°C, more preferably 110°C to 130°C, and further preferably 115°C to 125°C. In addition, the processing time of the annealing process is, for example, 1 minute to 5 minutes, preferably 1.5 minutes to 4.5 minutes, more preferably 2 minutes to 4 minutes, and further preferably 2.5 minutes to 3.5 minutes.
[0113] The storage modulus of the adhesive layer at 23°C is preferably 0.1×10 5 Pa~1.5×10 5 Pa, more preferably 0.2×10 5 Pa~1.0×10 5 Pa, more preferably 0.3×10 5 Pa~0.8×10 5 Pa. When the storage modulus of the pressure-sensitive adhesive layer at 23° C. is within the above range, a thin optical laminate having excellent bending resistance can be provided. The storage modulus at 23° C. can be measured using a dynamic viscoelasticity measuring apparatus.
[0114] F. Image display device
[0115] The optical laminate of the embodiment of the present invention described above can be applied to an image display device. Therefore, the embodiment of the present invention includes an image display device using such an optical laminate. As representative examples of image display devices, liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices, inorganic EL display devices) can be cited. The image display device of the embodiment of the present invention has the above-mentioned optical laminate on its visible side. The optical laminate can be stacked in a manner that the polarizer becomes the visible side and the adhesive layer becomes the side of the image display unit (e.g., liquid crystal unit, organic EL unit, inorganic EL unit) (in a manner that the polarizer becomes the visible side).
[0116] Example
[0117] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. The measuring methods of each characteristic are as follows. In addition, unless otherwise specified, the "parts" and "%" in the examples and comparative examples are weight references.
[0118] <Production Example 1: Preparation of Adhesive Composition 1>
[0119] Acryloylmorpholine (ACMO) (manufactured by KJ Chemicals, trade name "ACMO") 20 parts by weight, FA1DDM (unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone; manufactured by Daicel Corporation, trade name "PLACCEL FA1DDM") 10 parts by weight, EAF5710 (a mixture of fluorene acrylate and reactive acrylate; manufactured by Osaka Gas Chemical Co., Ltd., trade name "OGSOL EA-F5710") 60 parts by weight, UP1190 (acrylic acid polymer; manufactured by Toagosei Co., Ltd., trade name "ARUFON UP-1190") 5 parts by weight, Omnirad907 (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one; manufactured by IGM Resins, trade name "Omnirad907") 3 parts by weight, DETX-S (2,4-diethylthioxanthone; manufactured by Nippon Kayaku Co., Ltd., trade name "KAYACURE DETX-S") were mixed at 25°C for 1 hour to obtain an adhesive composition 1.
[0120] <Production Example 2: Preparation of Adhesive Composition 2>
[0121] Adhesive composition 2 was obtained in the same manner as in Production Example 1 except that the composition was changed as follows.
[0122] “Adhesive composition 2”: 27.5 parts by weight of ACMO, 17.5 parts by weight of FA1DDM, 45 parts by weight of EAF5710, 5 parts by weight of UP1190, 3 parts by weight of Omnirad907, and 2 parts by weight of DETX-S
[0123] <Production Example 3: Preparation of Adhesive Composition 3>
[0124] Adhesive composition 3 was obtained in the same manner as in Production Example 1 except that the composition was changed as follows.
[0125] “Adhesive composition 3”: 20 parts by weight of HEAA (N-(2-hydroxyethyl)acrylamide; manufactured by KJ Chemicals, trade name “HEAA”), 25 parts by weight of ACMO, 35 parts by weight of 1,9-NDA (1,9-nonanediol diacrylate; manufactured by Kyoeisha Chemical Co., Ltd., trade name “Light Acrylate 1,9ND-A”), 15 parts by weight of UG4010 (acrylate polymer; manufactured by Toagosei Co., Ltd., trade name “ARUFON UG-4010”), 4 parts by weight of Omnirad 907, and 1 part by weight of Omnirad 184 (1-hydroxycyclohexyl phenyl ketone; manufactured by IGM Resins, trade name “Omnirad 184”)
[0126] <Production Example 4: Preparation of Adhesive Composition 4>
[0127] Adhesive composition 4 was obtained in the same manner as in Production Example 1 except that the composition was changed as follows.
[0128] “Adhesive composition 4”: 35 parts by weight of ACMO, 25 parts by weight of FA1DDM, 30 parts by weight of EAF5710, 5 parts by weight of UP1190, 3 parts by weight of Omnirad907, and 2 parts by weight of DETX-S
[0129] <Production Example 5: Preparation of Adhesive Composition 5>
[0130] Adhesive composition 5 was obtained in the same manner as in Production Example 1 except that the composition was changed as follows.
[0131] “Adhesive composition 5”: 15 parts by weight of HEAA, 2 parts by weight of M5300 (acrylate of ω-carboxy polycaprolactone; manufactured by Toagosei Co., Ltd., trade name “ARONIX M-5300”), 30 parts by weight of ACMO, 40 parts by weight of 1,9-NDA, 10 parts by weight of UP1190, 3 parts by weight of Omnirad907, and 2 parts by weight of DETX-S
[0132] <Production Example 6: Preparation of Adhesive Layer 1>
[0133] 1. Preparation of prepolymer composition
[0134] In a flask, 0.05 parts by weight of 2,2-dimethoxy-1,2-diphenyl-1-one (manufactured by IGM Resins, trade name "Omnirad651") and 0.05 parts by weight of 1-hydroxycyclohexyl phenyl ketone (manufactured by IGM Resins, trade name "Omnirad184") as photopolymerization initiators were added to a monomer mixture containing 60 parts by weight of n-octyl acrylate (NOAA), 30 parts by weight of butyl acrylate (BA), 8 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 2 parts by weight of N-vinyl-2-pyrrolidone (NVP) to obtain a mixture. The obtained mixture was irradiated with ultraviolet rays in a nitrogen atmosphere to polymerize a part of the monomer components in the mixture, thereby obtaining a prepolymer composition (containing monomer components that have not undergone polymerization reaction) with a polymerization rate of about 10%.
[0135] 2. Preparation of Adhesive Composition
[0136] 100 parts by weight of the obtained prepolymer composition, 0.08 parts by weight of a crosslinking agent (dipentaerythritol hexaacrylate (DPHA)), 0.05 parts by weight of a photopolymerization initiator (2,2-dimethoxy-1,2-diphenyl-1-one; manufactured by IGM Resins, trade name "Omnirad651"), and 0.3 parts by weight of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-403") were mixed to obtain an adhesive composition.
[0137] 3. Formation of adhesive layer
[0138] The obtained adhesive composition was applied to the release-treated surface of a release liner (manufactured by Mitsubishi Chemical Corporation, trade name "DIAFOIL MRF#38", thickness 38 μm) having a release-treated surface on one side to form a coating film. Next, the release-treated surface of a release liner (manufactured by Mitsubishi Chemical Corporation, trade name "DIAFOIL MRN#38", thickness 38 μm) having a release-treated surface on one side was attached to the side of the coating film not laminated with the release liner. Next, the coating film between the release liners was irradiated with ultraviolet rays (irradiation light source: black light, irradiation intensity: 5 mW / cm 2 ) and the coating film was photocured to form an adhesive layer (thickness 25 μm). Next, the adhesive layer sandwiched between release liners was placed in an oven and annealed at 120° C. for 3 minutes to obtain an adhesive layer 1.
[0139] <Production Example 7: Preparation of Adhesive Layer 2>
[0140] A pressure-sensitive adhesive layer 2 (thickness: 25 μm) was obtained in the same manner as in Production Example 6 except that the annealing treatment was not performed.
[0141] <Production Example 8: Preparation of Adhesive Layer 3>
[0142] 1. Preparation of acrylic acid base polymer
[0143] A mixture containing 44 parts by weight of 2-ethylhexyl acrylate (2EHA), 43 parts by weight of lauryl acrylate (LA), 6 parts by weight of 4-hydroxybutyl acrylate (4HBA), 7 parts by weight of N-vinyl-2-pyrrolidone (NVP), and 0.015 parts by weight of a photopolymerization initiator (manufactured by IGM Resins, trade name "Omnirad 184") was irradiated with ultraviolet rays and polymerized to obtain a prepolymer composition (polymerization rate: about 10%). In addition, the prepolymer composition contains monomer components that have not undergone a polymerization reaction.
[0144] 2. Preparation of Adhesive Composition
[0145] Next, 100 parts by weight of the prepolymer composition, 0.08 parts by weight of 1,6-hexanediol diacrylate (HDDA), 1 part by weight of an acrylic oligomer, and 0.3 parts by weight of a silane coupling agent (trade name "KBM403", manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed to prepare a photocurable adhesive composition.
[0146] 3. Formation of adhesive layer
[0147] The obtained adhesive composition was applied to the release-treated surface of a polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Corporation, trade name "DIAFOIL MRF#75", thickness 75 μm) with silicone release treatment on one side to form a coating film. Next, the release-treated surface of a PET film (manufactured by Mitsubishi Chemical Corporation, trade name "DIAFOIL MRF#75", thickness 75 μm) with silicone release treatment on one side was attached to the coating film on the PET film. Next, the coating film was irradiated with ultraviolet rays (irradiation light source: black light, irradiation intensity: 5 mW / cm 2 ) and the coating film was cured by ultraviolet light. The thickness of the obtained adhesive layer 3 was 50 μm.
[0148] <Production Example 9: Preparation of Adhesive Layer 4>
[0149] An adhesive layer 4 (thickness: 50 μm) was obtained in the same manner as in Production Example 6 except that the annealing treatment was not performed and the thickness was set to 50 μm.
[0150] [Example 1]
[0151] 1. Preparation of polarizer
[0152] An amorphous isophthalic acid copolymer polyethylene terephthalate (IPA copolymer PET) film (thickness: 100 μm) having a water absorption rate of 0.75% and a Tg of 75° C. in a strip shape was used as a substrate. A corona treatment was applied to one side of the substrate, and an aqueous solution containing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (polymerization degree 1200, acetoacetyl modification degree 4.6%, saponification degree 99.0 mol% or more, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name: GOHSEFIMER Z200) in a ratio of 9:1 was applied to the corona-treated surface at 25° C. and dried to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate.
[0153] The free end of the obtained laminate was uniaxially stretched (in-air auxiliary stretching) to 2.4 times in the longitudinal direction (length direction) between rolls having different peripheral speeds in an oven at 130°C.
[0154] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).
[0155] Next, the laminate was immersed in a dyeing solution (an aqueous solution obtained by adding 7.0 parts by weight of potassium iodide and 1.0 parts by weight of solid iodine to 100 parts by weight of water) at 30° C. and dyed (dyeing treatment) so that the transmittance of the obtained polarizer would be 42% or more.
[0156] Next, the film was immersed in a crosslinking bath (boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 35 seconds (crosslinking treatment).
[0157] Then, while immersing the laminate in a boric acid aqueous solution (boric acid concentration: 4.0 wt %) at a liquid temperature of 70°C, the laminate was uniaxially stretched (underwater stretching) between rollers having different peripheral speeds in the longitudinal direction (length direction) at a total stretching ratio of 5.5 times.
[0158] Then, the laminated body was immersed in a cleaning bath (an aqueous solution prepared by mixing 4 parts by weight of potassium iodide with respect to 100 parts by weight of water) at a liquid temperature of 20° C. for 3 seconds (cleaning treatment).
[0159] Then, the resulting product was dried in an oven at 60° C. for 60 seconds to obtain a laminate having a PVA-based resin layer (polarizer) having a thickness of 5 μm.
[0160] 2. Preparation of polarizer
[0161] An acrylic resin film (20 μm thick) having a lactone ring structure was bonded to the surface of the polarizer obtained above (the side opposite to the resin substrate) via an ultraviolet curing adhesive as a protective layer. Specifically, the curing adhesive was applied so that the total thickness reached 1.0 μm, and bonded using a roller. Then, UV rays were irradiated from the protective layer side to cure the adhesive.
[0162] 3. Preparation of the first phase difference layer
[0163] After adding 55 parts by weight of the compound represented by formula (I), 25 parts by weight of the compound represented by formula (II), and 20 parts by weight of the compound represented by formula (III) to 400 parts by weight of cyclopentanone (CPN), the mixture was heated to 60°C and stirred to dissolve. Then, the solution of the above-mentioned compound was returned to room temperature, 3 parts by weight of Irgacure 907 (manufactured by BASF Japan), 0.2 parts by weight of Megafac F-554 (manufactured by DIC), and 0.1 parts by weight of p-methoxyphenol (MEHQ) were added to the solution of the above-mentioned compound, and the mixture was further stirred. The stirred solution was transparent and uniform. The obtained solution was filtered with a 0.20 μm membrane filter to obtain a polymerizable composition.
[0164] Separately, a polyimide solution for an alignment film was applied to a glass substrate having a thickness of 0.7 mm by spin coating, dried at 100° C. for 10 minutes, and then fired at 200° C. for 60 minutes to obtain a coating film. The obtained coating film was rubbed with a commercially available rubbing device to form an alignment film.
[0165] Next, the polymerizable composition obtained above was applied on a substrate (substantially an alignment film) by spin coating and dried at 100° C. for 2 minutes. After the obtained coating film was cooled to room temperature, a high pressure mercury lamp was used to illuminate the film at 30 mW / cm 2 The phase difference layer (thickness 3 μm) as the orientation solidification layer of the liquid crystal compound was obtained by irradiating ultraviolet rays with an intensity of 1000 nm for 30 seconds. The in-plane phase difference Re(550) of the phase difference layer was 130 nm. In addition, the Re(450) / Re(550) of the phase difference layer was 0.851, and it showed reverse dispersion wavelength characteristics. The phase difference layer can function as a λ / 4 plate.
[0166] [Chemical formula 1]
[0167]
[0168] [Chemical formula 2]
[0169]
[0170] 4. Fabrication of the Second Phase Difference Layer
[0171] A liquid crystal coating liquid was prepared by dissolving 20 parts by weight of a side chain liquid crystal polymer represented by the following chemical formula (the numbers 65 and 35 in the formula represent the molar % of the monomer unit, and for convenience, it is expressed as a block polymer: weight average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. Then, the coating liquid was applied to a PET substrate subjected to a vertical alignment treatment by a bar coater, and then heated and dried at 80°C for 4 minutes, thereby aligning the liquid crystal. The liquid crystal layer was cured by irradiating the liquid crystal layer with ultraviolet rays, and a phase difference layer (thickness 4 μm) exhibiting a refractive index characteristic of nz>nx=ny was formed on the substrate.
[0172] [Chemical formula 3]
[0173]
[0174] 5. Fabrication of optical laminates
[0175] The polarizing plate obtained from the resin substrate in 2 is peeled off. Next, the first phase difference layer is bonded to the surface after the resin substrate of the polarizer is peeled off via an ultraviolet curing adhesive. At this time, the bonding is performed in a manner that the absorption axis of the polarizer forms an angle of 45° with the slow axis of the first phase difference layer. Next, the first phase difference layer and the second phase difference layer are stacked via an adhesive layer (thickness of 1 μm) formed using the adhesive composition obtained in Manufacturing Example 1 to obtain a polarizing plate with a phase difference layer having a structure of a protective layer (acrylic resin film having a lactone ring structure) / ultraviolet curing adhesive layer / polarizer / ultraviolet curing adhesive layer / first phase difference layer / adhesive layer (adhesive layer formed by adhesive composition 1) / second phase difference layer.
[0176] Next, one release liner was peeled off from the pressure-sensitive adhesive layer 1 obtained in Production Example 7, and the surface from which the release liner of the pressure-sensitive adhesive layer 1 was peeled was laminated on the surface of the polarizing plate with a retardation layer on the second retardation layer side to obtain an optical laminate.
[0177] [Examples 2 to 4]
[0178] Except having changed the adhesive composition and the pressure-sensitive adhesive layer which form the adhesive layer as described in Table 1, it carried out similarly to Example 1, and obtained the optical laminated body.
[0179] (Comparative Examples 1 to 4 and Reference Examples 1 to 6)
[0180] Except having changed the adhesive composition and the pressure-sensitive adhesive layer which form the adhesive layer as described in Table 1, it carried out similarly to Example 1, and obtained the optical laminated body.
[0181] [evaluate]
[0182] The following evaluations were performed using the optical layered bodies obtained in Examples, Comparative Examples, and Reference Examples, and the adhesive compositions and pressure-sensitive adhesives used therein.
[0183] 1. Thickness
[0184] The thickness of 10 μm or less was measured using an interferometer film thickness meter (manufactured by Otsuka Electronics Co., Ltd., product name "MCPD-3000"), and the thickness exceeding 10 μm was measured using a digital micrometer (manufactured by Anritsu Co., Ltd., product name "KC-351C").
[0185] 2. VOC value
[0186] The optical laminate obtained in the examples, comparative examples and reference examples was cut into a size of 100 mm × 50 mm as a test body. The test body was placed on a table with the protective layer side facing downward and the release liner attached to the adhesive layer facing upward, and the sensor part of the portable VOC monitor (manufactured by TOYO MEDIC, product name "ppbRAE3000") was arranged at a height of 40 mm from the adhesive layer side surface of the test body (the surface of the adhesive layer after the release liner was peeled off). Next, the release liner was peeled off from the adhesive layer and the measurement was performed for 60 seconds. The maximum value in the 60-second measurement was taken as the VOC value.
[0187] 3. Polymerization rate
[0188] Samples were collected from the adhesive layers of the examples, comparative examples, and reference examples, and their weights were measured. Next, the samples were dried at 130° C. for 3 hours, and the weights of the dried samples were measured. The polymerization rate was calculated from the weights of the samples before and after drying using the following formula.
[0189] Polymerization rate (%) = weight of sample after drying / weight of sample before drying × 100
[0190] 4. Martens hardness
[0191] Adhesive compositions 1 to 5 were applied to glass by a bar coater and sandwiched with glass via a spacer having a thickness of 1 μm. Next, UV light (visible light (enclosed gallium metal halide lamp) was irradiated by a UV light irradiator. Irradiation device: Fusion UV Systems, Inc., product name "Light HAMMER10", valve: V valve, peak illuminance: 1600 mW / cm2 , cumulative exposure 1000 / mJ / cm 2 (wavelength 380-440nm)), the adhesive was cured to form a single film of an adhesive layer with a thickness of 1 μm between the glasses, and an analysis sample was obtained. The obtained analysis sample was fixed, one side of the glass was removed, and nanoindentation measurement was performed under the following conditions.
[0192] Measuring device: Nanoindenter (manufactured by ELIONIX, product name "ENT-NEXUS")
[0193] Use indenter: Berkovich (triangular cone)
[0194] Measurement method: Single indentation measurement
[0195] Measurement temperature: room temperature (25°C)
[0196] Press load: 500μN
[0197] Pressing / pulling time: 10 seconds
[0198] Maximum load holding time: 1 second
[0199] 5. Bending test
[0200] The optical laminates obtained in the examples, comparative examples and reference examples were cut into 100 mm in length and 30 mm in width so that the angle between the transverse direction of the cut optical laminate and the absorption axis of the polarizer was about 135°. The release liner was peeled off from the adhesive layer of the cut optical laminate, and an acrylic resin film (thickness of 20 μm) having a lactone ring structure was bonded to the adhesive layer to prepare a test piece.
[0201] On two double-jointed clamshell plates of a desktop durability tester (manufactured by YUASA SYSTEM Machine Co., Ltd., product name "DR11MR4-CS"), align the longitudinal center of the prepared test piece with the center (bending line) of the bending part of the tester, and fix it with a double-sided tape in such a way that the acrylic resin film with a lactone ring structure laminated on the adhesive layer of the test piece becomes the plate side. The durability tester is placed in an environment with a room temperature of 60°C and a humidity of 90% RH. The radius of curvature during the bending test is set to 1.5mm, the folding speed is set to 30rpm (folding and opening operations are performed 30 times in 1 minute), and the folding operation is repeated 200,000 times. After the test, the test piece is observed through an optical microscope (magnification: 10 times) to observe whether there are cracks in the adhesive layer between the first phase difference layer and the second phase difference layer. If there is no crack or the crack length is less than 100μm, it is evaluated as no crack, and if the crack length is more than 100μm, it is evaluated as cracked.
[0202] Table 1
[0203]
[0204] As is clear from Table 1, the optical layered bodies of Examples of the present invention are excellent in bending resistance even under a high-temperature and high-humidity environment.
[0205] Industrial Applicability
[0206] The optical layered body according to the embodiment of the present invention can be suitably used in image display devices such as liquid crystal display devices, organic EL display devices, and inorganic EL display devices.
Claims
1. An optical laminate, comprising: A polarizing plate comprising a polarizer; A first phase difference layer, which is an alignment solidified layer of a liquid crystal compound; The adhesive layer has a Martens hardness of 150N / mm 2 ~250N / mm 2 ; A second phase difference layer, which is an alignment solidified layer of a liquid crystal compound; and The adhesive layer has a VOC value of 100 ppm or less.
2. An optical laminate, comprising: A polarizing plate comprising a polarizer; A first phase difference layer, which is an alignment solidified layer of a liquid crystal compound; The adhesive layer has a Martens hardness of 150N / mm 2 ~250N / mm 2 ; A second phase difference layer, which is an alignment solidified layer of a liquid crystal compound; as well as The polymerization rate of the adhesive layer is 98.5% or more.
3. The optical layered body according to claim 1 or 2, in, The thickness of the adhesive layer is 0.3 μm to 3 μm.
4. The optical layered body according to claim 1 or 2, in, The thickness of the adhesive layer is 10 μm to 100 μm. The optical layered body according to claim 1 or 2, which has a total thickness of 180 μm or less.
6. The optical layered body according to claim 1 or 2, in, The in-plane phase difference Re(550) of the first phase difference layer is 100nm to 190nm, and satisfies Re(450) / Re(550)<1, The angle formed by the slow axis of the first phase difference layer and the absorption axis of the polarizer is 40° to 50°.
7. The optical layered body according to claim 1 or 2, in, The Re(550) of the first phase difference layer is 200nm to 300nm, and the Re(550) of the second phase difference layer is 100nm to 200nm. The angle between the slow axis of the first phase difference layer and the absorption axis of the polarizer is 10° to 20°. The angle formed by the slow axis of the second phase difference layer and the absorption axis of the polarizer is 70° to 80°. 8 . An image display device comprising the optical layered body according to claim 1 .