Glass wafer, light guide plate, and image display device
By optimizing the materials and processes of the glass wafer, the warping problem of the glass wafer when forming diffractive optical elements is solved, the optical performance of the light guide plate and the image display quality are improved, and high-precision optical element positions are achieved.
Patent Information
- Application Number
- CN202410359030.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-18
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, when forming diffractive optical elements of glass wafers, heating causes warping, resulting in a decrease in position accuracy, affecting the optical performance of the light guide plate and the quality of image display.
A thin plate-shaped glass wafer with a Young's modulus of over 100GPa and a refractive index of over 1.9 is used. Both sides have periodic concave and convex structures. By optimizing the composition and process of the glass, warpage is reduced and positional accuracy is improved.
It effectively reduces the warpage of the glass wafer when forming diffractive optical elements, improves the optical performance of the light guide plate and the quality of image display, and ensures high-precision positioning of optical elements.
Smart Images

Figure BDA0004762257610000171 
Figure BDA0004762257610000181 
Figure BDA0004762257610000231
Abstract
Description
Technical Field
[0001] The present invention relates to a glass wafer, a light guide plate and an image display device, and in particular to a highly elastic glass substrate for a light guide plate with diffraction optical elements on both sides of a transparent display screen. Background Art
[0002] In recent years, with the development of AR (augmented reality), MR (mixed reality) and VR (virtual reality) technologies, display devices such as head-mounted displays have been developed as AR devices, MR devices and VR devices. Among them, eyeglass-type wearable terminals called smart glasses disclosed in Patent Document 1 have attracted attention.
[0003] In smart glasses, light emitted from an image light source is guided to the wearer's eyes by a light guide plate, which is equivalent to a lens, and displayed as an image.
[0004] Specifically, the light emitted from the image light source enters the light guide plate through the diffractive optical element formed on the surface of the light guide plate. Then, the light entering the light guide plate travels while being repeatedly totally reflected inside the light guide plate, and is emitted toward the wearer's eyes by the diffractive optical element set in front of the wearer's eyes.
[0005] The light guide plate for smart glasses is manufactured using semiconductor circuit manufacturing equipment. In the mass production process of semiconductor circuits, multiple integrated circuits are formed on the surface of a silicon wafer using photolithography technology. Then, the silicon wafer with multiple integrated circuits is cut and separated by dicing to manufacture multiple semiconductor circuit elements.
[0006] The light guide plate can be manufactured by the same process as the mass production process of semiconductor circuits. That is, a plurality of diffractive optical elements are formed on the surface of a thin plate of glass such as a glass wafer, and the glass wafer is cut and separated by dicing to manufacture a plurality of light guide plates.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: (Japanese) Patent Publication No. 2016-139174 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] When forming a diffractive optical element, sub-micron precision is required. However, when forming a diffractive optical element on the surface of a glass wafer, for example, the glass wafer is heated to above 100° C. The inventors have found that in the existing glass wafer, the heating causes the glass wafer to warp, resulting in a problem that the diffractive optical element cannot be formed with high precision. Specifically, it is described as follows.
[0012] As the material of the diffractive optical raw material, inorganic materials such as titanium oxide, silicon nitride, silicon carbide, or organic materials such as transparent resins are used. In the case of using inorganic materials, a film of inorganic materials is formed on the surface of a glass wafer, and the film is finely processed by photolithography to form a diffractive optical element. In photolithography, a photoresist is coated on the film-forming surface of the glass wafer, and the entire wafer is heated on a hot plate to perform pre-baking for evaporating the solvent of the photoresist. Then, the pattern of the photomask is transferred to the photoresist by ultraviolet exposure. After exposure, in order to thermally crosslink the photoresist, the wafer is placed on a hot plate and heated (post-baked) to about 120 to 150°C. Then, after the photoresist is developed, fine concave and convex are formed on the film by etching to form a diffractive optical element. In the case of using organic materials, a transparent ultraviolet curing resin or other resin is coated on the main surface of the glass wafer to form a coating film, and the pattern is transferred to the coating film by a mold of a shape after the fine concave and convex pattern of the diffractive optical element is reversed. After that, the wafer is placed on a hot plate and heated to about 125°C for firing to form a diffractive optical element.
[0013] Whether it is an inorganic material or an organic material, when a glass wafer is heated on a hot plate, warping occurs in the glass wafer. When the thermal conductivity of the glass is low and it is heated on a hot plate, a large temperature difference is generated between the main surface facing the hot plate, that is, the main surface facing downward, and the main surface on the opposite side, that is, the main surface facing upward. The amount of expansion of the main surface facing downward at high temperature is greater than the amount of expansion of the main surface facing upward at low temperature, so the glass wafer is warped in a convex shape downward. The peripheral portion of the warped glass wafer is separated from the hot plate, so that in the main surface, the central portion becomes a higher temperature than its peripheral portion. In this state, due to the thermal crosslinking of the photoresist and the firing of the organic material, positional deviation is also generated in the fine pattern of the diffractive optical element after the heating is completed.
[0014] A light guide plate having diffractive optical elements on both sides is manufactured by forming a diffractive optical element on one side of a glass wafer and then further forming a diffractive optical element on the back side thereof. As described above, in the past, when a diffractive optical element was formed on one side, the position of the diffractive optical element on the wafer was offset, and the positional accuracy was reduced. In order to obtain a light guide plate having diffractive optical elements on both sides, a diffractive optical element is further formed on the back side of a glass wafer having a low positional accuracy of the diffractive optical element. When the diffractive optical element is formed on the back side, it is difficult to form the diffractive optical element with high accuracy because the glass wafer is warped when it is heated on a hot plate. Therefore, the position of the diffractive optical element is further offset on both the front and back sides of the glass wafer.
[0015] As described above, after forming the diffractive optical element, the glass wafer is cut and separated by dicing to manufacture a plurality of light guide plates. However, due to the positional deviation of the diffractive optical element on the wafer, the positional accuracy of the diffractive optical element in each light guide plate decreases. As a result, a deviation occurs in the diffraction direction of light. When assembling the image display device, it is necessary to correct the deviation. When the deviation is large, there is a problem that the quality of the displayed image is reduced.
[0016] Therefore, a glass wafer capable of forming a diffractive optical element with high precision is required.
[0017] The present invention has been made in view of such circumstances, and an object of the present invention is to provide a glass wafer having reduced warping when a diffractive optical element is formed, a light guide plate obtained from the glass wafer, and an image display device including the light guide plate.
[0018] Technical solutions for solving technical problems
[0019] The gist of the present invention is as follows.
[0020] (1) A glass wafer for manufacturing a light guide plate, comprising a thin plate-shaped glass portion, having diffractive optical element portions on both main surfaces thereof, and an area of one main surface of the glass portion of 1950 mm 2 In the above, the thickness of the glass portion is 3.0 mm or less, and the Young's modulus of the glass portion is 100 GPa or more.
[0021] (2) The glass wafer according to (1), wherein the diffractive optical element portion has a periodic concavo-convex structure, and the period of the concavo-convex structure is 500 nm or less.
[0022] (3) In the glass wafer according to (1), the refractive index nd of the glass portion is 1.9 or more.
[0023] (4) The glass wafer according to (1), wherein the average linear expansion coefficient of the glass portion at -30°C to 70°C is 80×10 -6 K -1 the following.
[0024] (5) A light guide plate comprising a glass portion and diffractive optical element portions on both main surfaces of the glass portion, wherein the thickness of the glass portion is 3.0 mm or less and the Young's modulus of the glass portion is 100 GPa or more.
[0025] (6) In the light guide plate described in (5), the diffractive optical element portion has a periodic concavo-convex structure, and the period of the concavo-convex structure is 500 nm or less.
[0026] (7) In the light guide plate described in (5), the refractive index nd of the glass portion is 1.9 or more.
[0027] (8) An image display device comprising the light guide plate described in (5) above.
[0028] (9) The image display device according to (8), wherein the image display device is a glasses type.
[0029] Effects of the Invention
[0030] According to the present invention, it is possible to provide a glass wafer having reduced warpage when a diffractive optical element is formed, a light guide plate obtained from the glass wafer, and an image display device including the light guide plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 (a) and (b) are diagrams schematically showing the structure of a head-mounted display using a light guide plate according to one embodiment of the present invention.
[0032] Figure 2 It is a side view schematically showing the structure of a head mounted display using a light guide plate according to one embodiment of the present invention.
[0033] Figure 3 It is a diagram schematically showing a method for measuring BOW.
[0034] Figure 4 It is a figure which shows typically the glass part in a plan view, and is used for demonstrating the method of evaluating the warpage of a glass part.
[0035] FIG5(1) is a diagram schematically showing a cross section of a glass portion, and is used to explain a method of evaluating the warpage of the glass portion.
[0036] FIG5(2) is a diagram for explaining a method for evaluating the warpage of a glass portion. DETAILED DESCRIPTION
[0037] In this specification, the refractive index refers to the refractive index nd at the d-line (wavelength 587.56 nm) of helium unless otherwise specified.
[0038] The Abbe number νd is used as a value indicating a property related to dispersion and is represented by the following equation: nF is the refractive index of blue hydrogen at the F line (wavelength 486.13 nm), and nC is the refractive index of red hydrogen at the C line (656.27 nm).
[0039] νd=(nd-1) / (nF-nC)
[0040] In the present invention, the glass composition is expressed on an oxide basis unless otherwise specified. Here, the "glass composition on an oxide basis" refers to the glass composition obtained by converting the glass raw materials into oxides in the glass after they are completely decomposed during melting. All glass components expressed on an oxide basis (excluding Sb (Sb) added as a clarifier)2 O 3 ) and Ce(CeO 2 The total content of )) is 100 mass %. The description of each glass component is recorded as SiO according to custom. 2 、TiO 2 The content and total content of the glass component are by mass unless otherwise specified, and “%” means “mass %”.
[0041] The content of the glass component can be quantified by a known method, such as inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In addition, in the present invention, the content of a constituent component of 0% means that the constituent component is substantially not contained, and the constituent component is allowed to be contained at an unavoidable impurity level.
[0042] Hereinafter, one embodiment of the present invention will be described.
[0043] Glass wafer
[0044] The glass wafer of the present embodiment has a thin plate-shaped glass portion and has diffractive optical element portions on both main surfaces thereof.
[0045] <Glass Department>
[0046] (shape)
[0047] In the glass wafer of the present embodiment, the glass portion is in the shape of a thin plate. Preferably, the glass portion is in the shape of a circular plate. In addition, the glass portion may also have a thin plate shape whose main surface is in the shape of a polygon, a square or a rectangle. Since the glass portion has such a thin plate shape, a light guide plate can be manufactured from the glass wafer using a conventional semiconductor circuit manufacturing device.
[0048] (area)
[0049] In the glass wafer of this embodiment, the area of one main surface of the glass portion is 1950 mm 2 Above, preferably 4400mm 2 Above, more preferably 7850mm 2 Above, more preferably 17670mm 2 Above, preferably 70690mm 2 By increasing the area of the main surface of the glass portion, the number of light guide plates that can be obtained per unit area can be increased. The upper limit of the area of the main surface of the glass portion is not particularly limited, but from the perspective of using conventional semiconductor circuit manufacturing equipment, it is usually 159050mm 2 .
[0050] (Diameter of the inscribed circle)
[0051] In the glass wafer of the present embodiment, the size of the glass portion can also be evaluated by the size of a circle that is virtually inscribed in the shape of the main surface of the glass portion. That is, the diameter of the circle that is virtually inscribed in the shape of the main surface of the glass portion is preferably 50 mm or more, more preferably 75 mm or more, further preferably 100 mm or more, and most preferably 150 mm or more. By increasing the diameter of the inscribed circle, the number of light guide plates that can be obtained per unit area can be increased. The upper limit of the diameter of the inscribed circle is not particularly limited, but from the perspective of using conventional semiconductor circuit manufacturing equipment, it is usually 450 mm.
[0052] (diameter)
[0053] In the glass wafer of the present embodiment, when the glass portion is in the shape of a circular plate, the diameter of the glass portion is preferably 50 mm or more, more preferably 75 mm or more, further preferably 100 mm or more, and most preferably 150 mm or more. By increasing the diameter of the glass portion, the number of light guide plates available per unit area can be increased. The upper limit of the diameter of the glass portion is not particularly limited, but from the perspective of using conventional semiconductor circuit manufacturing equipment, it is usually 450 mm.
[0054] (thickness)
[0055] In the glass wafer of the present embodiment, the thickness of the glass portion is 3.0 mm or less, preferably 1.0 mm or less, more preferably 0.8 mm or less, and further preferably 0.5 mm or less. The lower limit of the thickness of the glass portion is not particularly limited, but is generally 0.2 mm, preferably 0.25 mm. By setting the thickness of the glass portion to the above range, a light guide plate that can be used as a lens of smart glasses can be manufactured, and the light guide plate can be manufactured from the glass wafer using a conventional semiconductor circuit manufacturing device.
[0056] (Young's modulus)
[0057] In the glass wafer of the present embodiment, the Young's modulus of the glass portion is more than 100GPa, preferably more than 110GPa, and more preferably more than 120GPa. The upper limit of the Young's modulus of the glass portion is usually 150GPa, preferably 140GPa, as long as it is not particularly limited. By setting the Young's modulus of the glass portion to the above range, when the glass portion is heated and a diffractive optical element portion is formed on its main surface, the warping of the glass portion can be reduced, and the diffractive optical element portion can be formed with high precision. In addition, by setting the Young's modulus of the glass portion to the above range, the breakage during the transportation of the glass wafer can be reduced. In addition, the breakage during the removal and processing of the glass wafer or the glass portion from the wafer box can also be reduced.
[0058] Young's modulus was measured and calculated based on JIS R 1602-1995. Specifically, a glass sample with a length of 20 mm, a width of 20 mm, and a height of 100 mm, which was made of the same material as the glass part, was fully annealed and placed in a constant temperature chamber, and the longitudinal wave velocity (Vl) and transverse wave velocity (Vs) of 5 MHz ultrasonic waves were measured, and Young's modulus (E) and rigidity (G) were calculated according to the following formulas.
[0059] E=(4G 2 -3G×Vl 2 ×ρ) / (G-Vl 2 ×ρ)
[0060] G=Vs 2 ×ρ
[0061] Here, ρ is the density of the glass sample, and the value of specific gravity can be used. The density (specific gravity) of the glass sample at room temperature is consistent with the density (specific gravity) of the glass portion at room temperature. That is, the density at room temperature is the specific gravity plus the unit g / cm 3 To express.
[0062] (Average linear expansion coefficient α at -30℃ to 70℃ n )
[0063] In the glass wafer of the present embodiment, the average linear expansion coefficient α of the glass portion at -30°C to 70°C is n Preferably 80×10 -6 K -1 Below, more preferably 75×10 -6 K -1 Average linear expansion coefficient α of the glass part at -30℃ to 70℃ n The lower limit is not particularly limited, but is usually 60×10 -6 K -1 When heating from one side on a hot plate when forming the diffractive optical element portion, it is preferred to reduce the average linear expansion coefficient α of the glass portion at -30°C to 70°C from the viewpoint of reducing the expansion difference between the two main surfaces of the glass portion and reducing the warping of the glass portion. n Set to the above range.
[0064] Average linear expansion coefficient α at -30℃~70℃ n The dilatometer was used for measurement and the dilatometer was used for calculation.
[0065] α n =dL n / (L×dT n )
[0066] Here, dT nis the temperature difference between -30 and 70°C (K), L is the initial length of the glass sample (mm), dL n It is the change in sample length (mm) within the temperature range of -30 to 70°C.
[0067] (Refractive index nd)
[0068] In the glass wafer of the present embodiment, the refractive index nd of the glass portion is preferably 1.9 or more, more preferably 1.95 or more, and further preferably 2.00 or more. The upper limit of the refractive index nd of the glass portion is not particularly limited, but is generally 2.2. The light incident on the glass portion travels inside the glass portion while repeatedly undergoing total reflection, and from the viewpoint of emitting with a sufficient viewing angle, the refractive index of the glass portion is preferably set to the above range.
[0069] (Abbe number νd)
[0070] In the glass wafer of this embodiment, the upper limit of the Abbe number νd of the glass portion may be 40, 35, or 30. The lower limit of the Abbe number νd of the glass portion is not particularly limited, but is usually 15.
[0071] (Glass transition temperature Tg)
[0072] In the glass wafer of the present embodiment, the glass transition temperature Tg of the glass portion is preferably 600° C. or higher, more preferably 630° C. or higher, and further preferably 650° C. or higher. The upper limit of the glass transition temperature Tg of the glass portion is not particularly limited, but is generally 780° C., preferably 760° C. When the glass portion is heated to form a diffractive optical element portion on its main surface, the glass transition temperature Tg of the glass portion is preferably set to the above range from the viewpoint of reducing the warpage of the glass portion and maintaining the desired refractive index and good thermal stability of the glass portion.
[0073] (Internal transmittance)
[0074] In the glass wafer of the present embodiment, the glass portion has light transmittance with respect to visible light. Light transmittance is evaluated by the internal transmittance of a glass sample with a thickness of 10.0 mm ± 0.1 mm at a wavelength of 420 nm to 800 nm. Internal transmittance refers to the transmittance of the glass sample excluding the surface reflection loss on the incident side and the exit side. The transmittance (external transmittance) T1 and T2 including the surface reflection loss of two glass samples composed of the same glass and having different thicknesses d1 and d2 can be measured respectively, and the internal transmittance τ with a thickness of 10.0 ± 0.1 mm at a specific wavelength is calculated using the following formula.
[0075] logτ=-[(logT1-logT2)×10] / Δd
[0076] Among them, d2>d1, Δd=d2-d1, and log is the common logarithm.
[0077] The internal transmittance of a glass sample with a thickness of 10.0 mm ± 0.1 mm and made of the same material as the glass portion, i.e., the internal transmittance of the glass portion converted to a thickness of 10.0 mm ± 0.1 mm, is preferably 78% or more, more preferably 83% or more, and even more preferably 90% or more in the wavelength range of 420 nm to 800 nm.
[0078] In addition, the minimum value of the internal transmittance at a wavelength of 420 nm to 800 nm is preferably the internal transmittance at the short wavelength end of the wavelength range, i.e., at a wavelength of 420 nm. That is, the internal transmittance of a glass sample having a thickness of 10.0 mm ± 0.1 mm and made of the same material as the glass portion at a wavelength of 420 nm (converted to the internal transmittance of the glass portion having a thickness of 10.0 mm ± 0.1 mm) is preferably 78% or more, more preferably 83% or more, and even more preferably 90% or more.
[0079] (proportion)
[0080] In the glass wafer of this embodiment, the specific gravity of the glass portion is preferably 5.5 or less, more preferably 5.4 or less, and further preferably 5.3 or less. Although the lower limit of the specific gravity of the glass portion is not particularly limited, it is usually 4.3. When used as a spectacle lens of smart glasses, from the viewpoint of reducing the discomfort caused by the weight of the lens when wearing, the specific gravity of the glass portion is preferably set to the above range.
[0081] (Specific elastic modulus)
[0082] In the glass wafer of the present embodiment, the specific elastic modulus of the glass portion is preferably 24.0MN / Kg or more, more preferably 24.5MN / Kg or more, and further preferably 25.0MN / Kg or more. The upper limit of the specific elastic modulus of the glass portion is not particularly limited, but is preferably about 30MN / Kg. When the glass portion is heated to form a diffractive optical element portion on its main surface, from the viewpoint of reducing the warping of the glass portion, the specific elastic modulus of the glass portion is preferably set to the above range.
[0083] (Material)
[0084] In the glass wafer of this embodiment, the material of the glass portion only needs to satisfy the above Young's modulus and the average linear expansion coefficient α at -30°C to 70°C. n , there is no particular limitation. As a material of the glass portion, for example, optical glass can be cited. The glass portion is preferably composed of optical glass.
[0085] Specifically, as the material of the glass portion, a glass having a B-La composition can be exemplified. Therefore, the glass composition of the B-La system shown below is a non-limiting example. It should be noted that the material of the glass portion is not limited to the glass having a B-La composition as shown below, as long as it is a material that can obtain a glass wafer that can reduce the warpage when forming a diffractive optical element.
[0086] The glass portion preferably has a glass composition shown below (indicated by mass %).
[0087] B 2 O 3 and SiO 2 The total content of 2 O 3 +SiO 2 ] is preferably 5 to 25%.
[0088] La 2 O 3 , Gd 2 O 3 , Y 2 O 3 and Yb 2 O 3 The total content [La 2 O 3 +Gd 2 O 3 +Y 2 O 3 +Yb 2 O 3 ] is preferably 25 to 68%.
[0089] TiO 2 , Nb 2 O 5 、 2 O 5 and WO 3 The total content [TiO 2 +Nb 2 O 5 +Ta 2 O 5 +WO 3 ] is preferably 5 to 40%.
[0090] The total content of MgO, CaO, SrO and BaO [MgO+CaO+SrO+BaO] is preferably 0 to 20%.
[0091] Li 2 O、Na 2 O and K 2 The total content of O [Li 2 O+Na2 O+K 2 O] is preferably 0 to 5%.
[0092] ZrO 2 The content of is preferably 0 to 12%.
[0093] The content of ZnO is preferably 0 to 10%.
[0094] B 2 O 3 The content of is preferably 3 to 20%.
[0095] SiO 2 The content of is preferably 0 to 15%.
[0096] La 2 O 3 The content of is preferably 25 to 60%.
[0097] G 2 O 3 The content of is preferably 0 to 30%.
[0098] Y 2 O 3 The content of is preferably 0 to 16%.
[0099] Yb 2 O 3 The content of is preferably 0 to 5%.
[0100] The TiO content is preferably 0 to 28%.
[0101] Nb 2 O 5 The content of is preferably 0 to 15%.
[0102] Ta 2 O 5 The content of is preferably 0 to 10%.
[0103] WO 3 The content of is preferably 0 to 6%.
[0104] The content of MgO is preferably 0 to 5%.
[0105] The content of CaO is preferably 0 to 5%.
[0106] The content of SrO is preferably 0 to 5%.
[0107] The content of BaO is preferably 0 to 20%.
[0108] Li 2 The content of O is preferably 0 to 5%.
[0109] Na 2The content of O is preferably 0 to 5%.
[0110] K 2 The content of O is preferably 0 to 5%.
[0111] Sb 2 O 3 The content of is preferably 0 to 1%.
[0112] Lu 2 O 3 The content of is preferably 0 to 1%.
[0113] Sc 2 O 3 The content of is preferably 0 to 1%.
[0114] Ga 2 O 3 The content of is preferably 0 to 1%.
[0115] GeO 2 The content of is preferably 0 to 1%.
[0116] In the glass portion, from the viewpoint of increasing Young's modulus, it is preferred that the total content [La 2 O 3 +Gd 2 O 3 +Y 2 O 3 +Yb 2 O 3 ]、ZrO 2 The content of MgO+CaO+SrO+BaO and the content of TiO are set to the above ranges. In addition, from the viewpoint of suppressing the increase of the average linear expansion coefficient, it is preferred to set the total content [MgO+CaO+SrO+BaO] and the total content [Li 2 O+Na 2 O+K 2 O] is set to the above range.
[0117] In addition, the glass portion preferably does not contain Pb, Te, Cd, Th, Tl, V, Cr, Ni, Fe, U, Nd, Cu, Er, Eu, etc.
[0118] <Diffractive Optical Element Department>
[0119] The glass wafer of the present embodiment has a diffraction optical element portion on the two main surfaces of the glass portion. The diffraction optical element portion is not particularly limited as long as it includes a component having the function of a diffraction grating. For example, the diffraction optical element portion includes a diffraction grating having the function of diffracting the light (image) incident from the image light source in the glass portion, that is, a diffraction optical element for light incidence, or a diffraction grating having the function of diffracting the light traveling in the glass portion by total reflection and emitting to the outside, that is, a diffraction optical element for light emission. In this case, in the glass wafer, each region that becomes a light guide plate after being cut and separated by cutting forms a diffraction optical element for incident and a diffraction optical element for emission. Since the light beam before entering the light guide plate is thin, the area of the diffraction optical element for incident is small. On the other hand, since the diffraction optical element for emission enlarges the displayed image in front of the eyes of the person wearing the image display device, its area is large. The larger the viewing angle, the larger the area of the diffraction optical element for emission.
[0120] In the glass wafer of the present embodiment, the shape of the diffraction grating of the diffraction optical element portion is not particularly limited. Therefore, the diffraction grating can be a diffraction grating having a groove shape, or a so-called holographic diffraction grating using holography. For example, the diffraction optical element portion can have a periodic concave-convex structure as a diffraction grating. In this case, from the viewpoint that the light (image) incident from the image light source travels while repeatedly undergoing total reflection inside the glass portion, and from the viewpoint that the light is emitted at a sufficient viewing angle, the period of the concave-convex structure is preferably less than 500nm, more preferably less than 400nm, and can also be less than 280nm.
[0121] The material of the diffractive optical element portion is not particularly limited, and may be either an inorganic material or an organic material. From the viewpoint of maintaining the light transmittance of the eyeglass lens as smart glasses, a transparent material is preferably used. As an inorganic material, for example, titanium oxide, silicon nitride, and silicon carbide can be cited, but it is not limited thereto. In addition, in the films of titanium oxide, silicon nitride, silicon carbide, etc., the molar ratio of elements such as Ti, Si, O, N, and C is not necessarily an integer ratio (non-stoichiometric). Therefore, in this specification, the inorganic material of the diffractive optical element portion also includes materials that form a stoichiometric ratio and materials that do not form a stoichiometric ratio, which are recorded as titanium oxide, silicon nitride, silicon carbide, etc. As an organic material, a transparent resin can be cited, for example, it can also be a UV-curable resin.
[0122] The glass wafer of this embodiment can be cut and separated by dicing to manufacture a plurality of light guide plates.
[0123] Light guide plate
[0124] The light guide plate of the present embodiment includes a glass portion and has diffractive optical element portions on both main surfaces of the glass portion.
[0125] The light guide plate of this embodiment inherits the characteristics of the glass wafer as it is, and the characteristics of the glass portion and the diffractive optical element portion in the glass wafer can be used as the characteristics of the glass portion and the diffractive optical element portion in the light guide plate as it is.
[0126] In particular, in the light guide plate of this embodiment, the thickness of the glass portion is 3.0 mm or less, preferably 1.0 mm or less, more preferably 0.8 mm or less, and further preferably 0.5 mm or less. The lower limit of the thickness of the glass portion is not particularly limited, but is usually 0.2 mm, preferably 0.25 mm.
[0127] In the light guide plate of the present embodiment, the Young's modulus of the glass portion is 100 GPa or more, preferably 110 GPa or more, and more preferably 120 GPa or more. The upper limit of the Young's modulus of the glass portion is not particularly limited, but is usually 150 GPa, preferably 140 GPa.
[0128] In the glass portion and the diffractive optical element portion of the light guide plate of the present embodiment, the properties other than those described above, namely, the average linear expansion coefficient α of the glass portion at -30°C to 70°C n , refractive index nd, Abbe number νd, glass transition temperature Tg, internal transmittance, specific gravity, specific elastic modulus, material, and the type, shape, period and material of the diffraction optical element part can be the same as the glass part and the diffraction optical element part of the glass chip.
[0129] Image display device
[0130] The image display device of this embodiment includes the above-mentioned light guide plate.
[0131] Hereinafter, a light guide plate according to one embodiment of the present invention and an image display device using the light guide plate will be described in detail with reference to the accompanying drawings. It should be noted that the same or corresponding parts in the drawings are denoted by the same reference numerals and will not be described repeatedly.
[0132] Figure 1 1 is a diagram showing a configuration example of a head mounted display 1 (hereinafter referred to as “HMD 1 ”) using a light guide plate 10 according to one embodiment of the present invention. Figure 1 (a) is a front side stereoscopic view of HMD 1. Figure 1 (b) is a back side stereoscopic view of HMD1. Figure 1 (a) and Figure 1As shown in (b), a spectacle lens 3 is mounted on the front portion of a spectacle frame 2 worn on the user's head. A backlight 4 for illuminating an image is mounted on the mounting portion 2a of the spectacle frame 2. A signal processing device 5 for playing images and a speaker 6 for playing sounds are provided on the temple portion of the spectacle frame 2. The FPC (Flexible Printed Circuits) 7 constituting the wiring extending from the circuit of the signal processing device 5 is wired along the spectacle frame 2. The display element unit (e.g., a liquid crystal display element) 20 is wired to the center position of the user's eyes through the FPC 7, and the approximate center portion of the display element unit 20 is arranged on the optical axis of the backlight 4 and is held. The display element unit 20 is relatively fixed relative to the light guide plate 10 in a manner of being located in the approximate center portion of the light guide plate 10. In addition, HOE (Holographic Optical Element) 32R, 32L (first diffractive optical element) are respectively formed on the first surface 10a of the light guide plate 10 in a portion located in front of the user's eyes. The HOEs 52R and 52L are formed on the second surface 10 b of the light guide plate 10 at positions facing the display element unit 20 with the light guide plate 10 interposed therebetween.
[0133] Figure 2 FIG. 1 is a side view schematically showing the structure of an HMD 1 according to one embodiment of the present invention. Figure 2 In order to make the drawings clearer, only the main parts of the image display device are shown, and the illustration of the eyeglass-type frame 2 and the like is omitted. Figure 2 As shown in FIG. 1 , the HMD 1 has a structure that is bilaterally symmetrical about a center line X connecting the image display element 24 and the center of the light guide plate 10. Furthermore, the light of each wavelength incident on the light guide plate 10 from the image display element 24 is split into two as described later and guided to the right eye and the left eye of the user, respectively. The optical paths of the light of each wavelength guided to each eye are also approximately bilaterally symmetrical about the center line X.
[0134] like Figure 2 As shown, the backlight 4 has a laser light source 21, a diffusion optical system 22, and a microlens array 23. The display element unit 20 is an image generating unit having an image display element 24, and is driven, for example, in a field sequential manner. The laser light source 21 has laser light sources corresponding to wavelengths of R (wavelength 633nm), G (wavelength 546nm), and B (wavelength 436nm), and irradiates light of each wavelength in sequence at high speed. Light of each wavelength is incident on the diffusion optical system 22 and the microlens array 23, and is converted into a uniform, highly directional parallel light beam without uneven light quantity, and is vertically incident on the display panel surface of the image display element 24.
[0135] The image display element 24 is, for example, a transmissive liquid crystal (LCDT-LCOS) panel driven in a field sequential manner. The image display element 24 applies modulation corresponding to the image signal generated by the image engine (not shown) of the signal processing device 5 to each wavelength of light. The light of each wavelength modulated by the pixels of the effective area of the image display element 24 is incident on the light guide plate 10 with a prescribed beam cross section (a shape roughly the same as that of the effective area). It should be noted that the image display element 24 can also be replaced by other display elements such as DMD (Digital Mirror Device) or reflective liquid crystal (LCOS) panel, MEMS (Micro Electro Mechanical Systems), organic EL (Electro-Luminescence), inorganic EL, etc.
[0136] The display element unit 20 is not limited to a field sequential display element, but may be an image generating unit of a simultaneous display element (a display element having RGB color filters arranged in a predetermined manner on the emission surface). In this case, a white light source is used as the light source, for example.
[0137] like Figure 2 As shown, the light of each wavelength modulated by the image display element 24 is incident into the light guide plate 10 from the first surface 10a in sequence. HOE 52R, 52L (second diffractive optical element) is formed on the second surface 10b of the light guide plate 10. HOE 52R, 52L is, for example, a volume phase type HOE of a rectangular reflective type, and has a structure in which three sheets of photopolymers are stacked on which interference fringes corresponding to the light of each wavelength of R, G, and B are recorded respectively. That is, HOE 52R, 52L is configured to have a wavelength selection function of diffracting the light of each wavelength of R, G, and B and allowing the light of other wavelengths to pass.
[0138] HOEs 32R and 32L are also reflective volume phase HOEs, and have the same layer structure as HOEs 52R and 52L. HOEs 32R, 32L, 52R, and 52L may have substantially the same pitch of interference fringe patterns, for example.
[0139] The centers of the HOEs 52R and 52L coincide with each other, and the interference fringe patterns are stacked in a state where they are flipped by 180 degrees. Moreover, the centers of the HOEs 52R and 52L coincide with the center line X in the stacked state. Lights of various wavelengths modulated by the image display element 24 are sequentially incident on the HOEs 52R and 52L via the light guide plate 10.
[0140] HOE 52R, 52L diffracts light of each wavelength incident sequentially to the right eye and the left eye respectively at a predetermined angle. Light of each wavelength diffracted by HOE 52R, 52L is repeatedly totally reflected at the interface between the light guide plate 10 and the air, and is transmitted inside the light guide plate 10 and incident on HOE 32R, 32L. Here, HOE 52R, 52L assigns the same diffraction angle to light of each wavelength. Therefore, light of all wavelengths having approximately the same incident position relative to the light guide plate 10 (or according to other expressions, emitted from approximately the same coordinates within the effective area of the image display element 24) propagates on approximately the same optical path within the light guide plate 10 and is incident on approximately the same position on HOE 32R, 32L. From another point of view, HOE 52R, 52L diffracts light of each wavelength of RGB in order to faithfully reproduce the pixel position relationship within the effective area of the image displayed on the effective area of the image display element 24 on HOE 32R, 32L.
[0141] Thus, in one embodiment of the present invention, HOEs 52R and 52L diffract the light of all wavelengths emitted from substantially the same coordinates in the effective region of the image display element 24 into substantially the same position on HOEs 32R and 32L, respectively. Alternatively, HOEs 52R and 52L may be configured to diffract the light of all wavelengths that are relatively staggered and originally the same pixel in the effective region of the image display element 24 into substantially the same position on HOEs 32R and 32L.
[0142] Light of each wavelength incident on HOE 32R, 32L is diffracted by HOE 32R, 32L and emitted in sequence approximately vertically from the second surface 10b of the light guide plate 10 to the outside. In this way, the light of each wavelength emitted as approximately parallel light is imaged on the right eye retina and the left eye retina of the user as a virtual image I of the image generated by the image display element 24. In addition, the HOE 32R, 32L may be given a capacitive effect in such a way that the user can observe the virtual image I of the enlarged image. That is, the light incident on the peripheral area of HOE 32R, 32L may be emitted at an angle closer to the center of the eye and imaged on the user's retina. Alternatively, in order to enable the user to observe the virtual image I of the enlarged image, HOE 52R, 52L may diffract the light of each wavelength of RGB in such a way that the pixel position relationship on HOE 32R, 32L becomes an enlarged similar shape relative to the pixel position relationship in the effective area of the image displayed on the effective area of the image display element 24.
[0143] The higher the refractive index, the shorter the air-converted optical path length of the light traveling in the light guide plate 10, so by using the light guide plate of this embodiment having a glass portion with a high refractive index, it is possible to expand the viewing angle relative to the width of the image display element 24. In addition, in this embodiment, although the refractive index of the glass portion is high, the specific gravity is suppressed to a low level, so that a light guide plate that is lightweight and can achieve the above-mentioned effect can be provided.
[0144] In the above, a head-mounted display screen is used as an example to explain the image display device, but the image display device of this embodiment may also be a glasses-type smart glasses. In addition, it may be another image display device. In addition, the diffraction optical element may also be a diffraction grating having a fine concave-convex periodic structure by changing to a holographic diffraction grating. In the above example, a light guide plate for both eyes is described, but a light guide plate for displaying images in the left eye and the right eye may be provided separately.
[0145] <Manufacturing of glass wafers>
[0146] The glass wafer of the present embodiment can be manufactured by manufacturing a glass portion and forming the diffractive optical element portion on both main surfaces thereof.
[0147] The glass portion can be manufactured using, for example, a glass molded body. Hereinafter, the manufacture of a glass molded body made of optical glass will be described exemplarily.
[0148] Optical glass can be manufactured by mixing glass raw materials in a manner to obtain a specified composition and using the mixed glass raw materials according to a known glass manufacturing method. For example, a plurality of compounds are mixed and fully mixed to form a batch of raw materials, and the batch of raw materials is placed in a quartz crucible or a platinum crucible for rough melting (rough melting). The molten material obtained by the rough melting is rapidly cooled and crushed to produce cullet. The cullet is then placed in a platinum crucible for heating and remelting (remelting) to form molten glass, and then the molten glass is formed and gradually cooled after clarification and homogenization to obtain a glass formed body composed of optical glass. The forming and gradual cooling of the molten glass can be performed by applying known methods.
[0149] Furthermore, as long as the desired glass components can be introduced into the glass in a desired content, the compounds used when preparing the batch raw materials are not particularly limited, but examples of such compounds include oxides, carbonates, nitrates, hydroxides, fluorides, and the like.
[0150] The glass part can be produced by a method including a step of processing a glass molded body. Examples of the processing include cutting, cutting, rough grinding, fine grinding, and polishing.
[0151] In addition, the glass portion can also be produced by, for example, the following method.
[0152] By a known method, glass raw materials are melted to form molten glass in a manner of a prescribed composition, and the molten glass is poured into a casting mold and formed into a plate-like shape to produce a glass material composed of optical glass. The obtained glass material is appropriately cut, ground, and polished to produce a cut piece of a size and shape suitable for pressure forming. The cut piece is heated and softened, and pressure-formed (reheating press) is performed by a known method to produce a glass blank with a shape similar to that of the glass portion. The glass blank is annealed, and ground and polished by a known method to produce a glass portion.
[0153] The glass wafer can be manufactured by forming a diffractive optical element portion on the two main surfaces of the glass portion. The method for forming the diffractive optical element portion is not particularly limited. For example, the following examples illustrate the case where the diffractive optical element portion is formed by an organic material and the case where the diffractive optical element portion is formed by an inorganic material. In addition, when the diffractive optical element portion is set as a holographic diffraction grating, it can be formed by a known method.
[0154] In the case of being formed by an organic material, an organic material is applied to one main surface of the glass portion to form a coating film, and a mold of the shape of the diffraction grating pattern of the diffractive optical element portion after being reversed is transferred to the coating film. Thereafter, it is heated to about 125° C. and fired to manufacture a glass wafer having a diffractive optical element portion formed at a predetermined position on one main surface (surface) of the glass portion. Thereafter, a diffractive optical element portion is further formed on the other main surface (back) in the same manner. A glass wafer having a diffractive optical element portion formed at predetermined positions on two main surfaces of the glass portion can be manufactured. The organic material is not particularly limited, but a transparent resin can be cited, for example, an ultraviolet curable resin.
[0155] In the case of being formed by an inorganic material, an inorganic material film is formed on one main surface of the glass portion in a vacuum chamber by sputtering, evaporation or chemical vapor deposition (CVD). After the film is formed, it is taken out from the vacuum chamber, coated with a photoresist, and subjected to pre-baking, exposure, post-baking (about 120 to 150°C), development, and a diffraction grating pattern is formed by etching. In this way, a glass wafer having a diffraction optical element portion formed at a specified position on one main surface (surface) of the glass portion can be manufactured. Then, a diffraction optical element portion is further formed on the other main surface (back) by the same method. A glass wafer having a diffraction optical element portion formed at specified positions on the two main surfaces of the glass portion can be manufactured. Examples of inorganic materials include titanium oxide, silicon nitride or silicon carbide, but are not limited thereto.
[0156] <Manufacturing of light guide plates>
[0157] The manufacturing method of the light guide plate is not particularly limited, and the light guide plate can be manufactured by a known method. For example, a glass wafer having a diffractive optical element portion formed thereon is cut and separated by dicing, thereby manufacturing a plurality of light guide plates. In addition, when the glass wafer is cut and separated, an anti-reflection film may be formed on the main surface of the wafer, and a protective sheet may be attached thereto with an ultraviolet peeling adhesive to protect the main surface of the wafer, and the protective sheet may be peeled off by irradiating ultraviolet rays after cutting and separating.
[0158] <Manufacturing of image display device>
[0159] The manufacturing method of the image display device is not particularly limited, and the image display device can be manufactured by a known method. For example, if it is a glasses-type image display device, the light guide plate can be assembled to Figure 2 In the head mounted display 1 shown, the light guide plate is mounted on a frame together with a light source and an optical system and manufactured.
[0160] [Example]
[0161] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the embodiments shown in the examples.
[0162] (Example 1)
[0163] A glass wafer including a glass portion composed of glass A, B, or C shown in Table 1 was produced in the following procedure and various evaluations were performed.
[0164] [Preparation of glass samples]
[0165] The compound raw materials corresponding to the constituent components of the glass part, i.e., oxides, carbonates, etc., are weighed and fully mixed as the raw materials for preparation. The prepared raw materials are placed in a platinum crucible, heated to 1000-1350°C in an atmospheric environment or a water vapor environment and melted, and homogenized and clarified by stirring to obtain molten glass. The molten glass is cast into a forming mold and formed, and gradually cooled to obtain a glass sample. In addition, the molten glass is heat-treated in the atmosphere for a long time in a water vapor environment to increase the transmittance in the visible area.
[0166] [Measurement of optical properties]
[0167] The refractive index nd, Abbe number νd, glass transition temperature Tg, Young's modulus, and average linear expansion coefficient α of the obtained glass sample were measured by the following method. n The specific gravity, specific elastic modulus, and internal transmittance at wavelengths of 420 nm and 800 nm (values calculated based on a thickness of 10.0 mm) were measured. The results are shown in Table 1.
[0168] 〔Refractive index nd and Abbe number νd〕
[0169] The refractive indices nd, ng, nF, and nC were measured by the refractive index measurement method of JIS standard JIS B 7071-1, and the Abbe number νd was calculated based on the following formula.
[0170] νd=(nd-1) / (nF-nC)
[0171] 〔Glass transition temperature Tg〕
[0172] The glass transition temperature Tg was measured at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH JAPAN.
[0173] 〔Young's modulus〕
[0174] Young's modulus was measured and calculated based on JIS R 1602-1995. Specifically, a glass sample was processed into a size of 20 mm in length, 20 mm in width, and 100 mm in height, and after being fully annealed, it was placed in a constant temperature chamber, and the longitudinal wave velocity (Vl) and transverse wave velocity (Vs) of 5 MHz ultrasonic waves were measured, and Young's modulus (E) and rigidity (G) were calculated by the following formulas, respectively.
[0175] E=(4G 2 -3G×Vl 2 ×ρ) / (G-Vl 2 ×ρ)
[0176] G=Vs 2 ×ρ
[0177] Here, ρ is the density of the glass sample, and the value of specific gravity is used.
[0178] 〔Average linear expansion coefficient α at -30℃~70℃ n 〕
[0179] Average linear expansion coefficient α at -30℃~70℃ n The dilatometer was used for measurement and the dilatometer was used for calculation.
[0180] α n =dL n / (L×dT n )
[0181] Here, dT n is the temperature difference between -30 and 70°C (K), L is the initial length of the glass sample (mm), dL n It is the change in sample length (mm) within the temperature range of -30 to 70°C.
[0182] 〔proportion〕
[0183] The specific gravity was measured by the Archimedean method.
[0184] 〔Specific elastic modulus〕
[0185] The specific elastic modulus is calculated by dividing the Young's modulus by the density at room temperature. The density at room temperature is calculated by adding the unit (g / cm 3 ) to indicate.
[0186] 〔Internal transmittance〕
[0187] The glass sample was processed to have a thickness of 10 mm ± 0.1 mm and parallel and optically polished planes, and the internal transmittance at wavelengths of 420 nm and 800 nm was measured. The transmittance (external transmittance) T1 and T2 including surface reflection loss of two glass samples composed of the same glass sample and having different thicknesses d1 and d2 were measured respectively, and the internal transmittance τ was calculated using the following formula.
[0188] logτ=-[(logT1-logT2)×10] / Δd
[0189] Among them, d2>d1, Δd=d2-d1, and log is the common logarithm.
[0190] surface 1
[0191]
[0192]
[0193] [Production of glass wafers]
[0194] The above-mentioned glass sample was cut, ground, and polished to produce a glass portion in the shape of a disk. The area, diameter, and thickness of one main surface of the glass portion are shown in Table 2. In addition, the flatness of the glass portion before forming the diffractive optical element portion was evaluated by BOW. In addition, it was confirmed that the warping of the glass portion was reduced when the diffractive optical element portion was formed.
[0195] [Flatness before forming the diffractive optical element (BOW)]
[0196] Flatness is evaluated by BOW. BOW was measured using the flatness measuring instrument FlatMaster MSP300 manufactured by Tropel. It should be noted that BOW can be measured using a known method, such as a non-contact BOW measuring instrument, and the standard for the measurement of BOW of the American Society for Testing Materials standard ASTMF534 can be applied. Specifically, the glass portion is supported at three points arranged at equal intervals (120° intervals) on the circumference of an imaginary circle with a diameter slightly smaller than the diameter of the glass portion. At this time, the center of the glass portion and the center of the imaginary circle are arranged in the vertical direction, and the glass portion is not fixed (clamped). The deviation of the center point of the central surface of the glass portion from the imaginary plane (called the central surface reference plane) containing the three points supporting the glass portion is set as BOW.
[0197] Here, if Figure 3 As shown in FIG. 1 , the central surface refers to an imaginary surface that is equidistant from the two main surfaces of the glass portion and is located inside the glass portion. When the center point of the central surface of the glass portion is located above the central surface reference plane, BOW is a positive value. On the other hand, when the center point of the central surface of the glass portion is located below the central surface reference plane, BOW is a negative value. The larger the absolute value of BOW, the greater the curvature of the glass portion.
[0198] [Evaluation of warpage of glass portion during formation of diffractive optical element portion]
[0199] When a plurality of diffractive optical element parts are formed together on the main surface of the glass part, it is desired to make the dimensional accuracy and positional accuracy of all the diffractive optical element parts converge within the allowable range. The warping of the glass part becomes the main reason for the reduction of the above-mentioned dimensional accuracy and positional accuracy. The following is an explanation of the influence of the warping of the glass part on the dimensional accuracy and positional accuracy of the diffractive optical element part. The warping (flatness) of the glass part uses the value of BOW for quantitative representation.
[0200] The glass portion having a disk shape and a diameter of Φ (mm) will be described.
[0201] The area on the main surface of the glass portion where the diffractive optical element portion is formed is referred to as an effective area. Figure 4 As shown, the effective range is the range surrounded by a circle A with a radius of [(Φ / 2)-5 mm] from the center.
[0202] As shown in Fig. 5 (1) and Fig. 5 (2), if a central surface reference plane relative to circle A is assumed, [(Φ / 2)-5 mm] becomes the effective range length c. That is, the effective range length c is expressed by the following formula.
[0203] c=(Φ / 2)-5mm
[0204] When the glass portion is viewed from above in the direction of the central axis, the distance from the center of the glass portion to the circumference of the circle A is referred to as the actual length b.
[0205] The following equation holds true between the BOW value a, the implementation length b, and the effective range length c.
[0206] a 2 +b 2 =c 2
[0207] The above, the following equation holds.
[0208] b=[c 2 -a 2 ] 1 / 2 =[{(Φ / 2)-5mm} 2 -a 2 ] 1 / 2
[0209] That is, the difference (offset) between the effective range length c and the implementation length b is expressed as follows.
[0210] c-b=[(Φ / 2)-5mm]-[{(Φ / 2)-5mm} 2 -a 2 ] 1 / 2
[0211] When a plurality of diffractive optical element portions are formed by photolithography on the main surface of the glass portion, the value of BOW is maximum near the circumference of circle A representing the effective range, resulting in maximum positional deviation. Due to this positional deviation, errors occur in the period (pitch) of the concave-convex structure of the diffraction grating included in the diffractive optical element portion.
[0212] In order to maintain the performance of the diffractive optical element, it is desirable to suppress the error of the periodicity of the concavo-convex structure of the diffraction grating to within ±5%. In addition, the smaller the period of the concavo-convex structure of the diffraction grating, the more difficult it is to suppress the error to be small.
[0213] For example, when the period of the concave-convex structure of the diffraction grating is 150nm, 5% thereof is 7.5nm. That is, "7.5nm" becomes the maximum allowable value of the error in the period of the concave-convex structure of the diffraction grating. In the case where the glass portion is warped, if the above-mentioned offset "c-b" is within "7.5nm", the error of the periodicity of the concave-convex structure of the diffraction grating can be suppressed within ±5%. On the other hand, in the case where the above-mentioned offset "c-b" exceeds "7.5nm", the error of the periodicity of the concave-convex structure of the diffraction grating exceeds ±5%. In such a glass portion with large warping, the diffraction optical element portion cannot be formed with high precision.
[0214] Specifically, it shows the offset when the period of the concavo-convex structure of the diffraction grating is 150nm. When the diameter of the glass part is 200mm and the BOW value is 44μm, the offset "c-b" exceeds 7.5nm, so the periodic error of the concavo-convex structure of the diffraction grating contained in the diffraction optical element part near the circumference of circle A exceeds the maximum allowable value. In such a glass part, the diffraction optical element part cannot be formed with high precision.
[0215] Similarly, when the diameter of the glass portion is 250 mm and the BOW value is 55 μm, and when the diameter of the glass portion is 300 mm and the BOW value is 66 μm, the offset "c-b" exceeds 7.5 nm, so the periodic error of the concave-convex structure of the diffraction grating included in the diffraction optical element portion near the circumference of circle A exceeds the maximum allowable value. In such a glass portion, the diffraction optical element portion cannot be formed with high precision.
[0216] As shown in Table 2 (1) to (3), before the diffractive optical element portion is formed, the value of BOW is 10 to 30 μm, and the error in the period of the concavo-convex structure of the diffraction grating can be suppressed to within ±5%.
[0217] A diffraction optical element portion is formed on the produced glass portion by the following method to obtain a glass wafer. At this time, the warping of the glass portion during heating is sufficiently small. In addition, the value of the BOW of the glass wafer after the diffraction optical element portion is formed is also sufficiently small to suppress the error in the period of the concave-convex structure of the diffraction grating to within ±5%. In other words, it was confirmed that the diffraction optical element portion is formed with high precision over the entire effective range of the glass portion. For the glass wafer obtained by forming the diffraction optical element portion, the period of the concave-convex structure of the diffraction grating and the height difference between the convex and concave parts of the diffraction grating were measured. The results are shown in Table 2.
[0218] [Formed from organic materials]
[0219] On one main surface of the glass portion, a siloxane polymer is coated as an organic material to form a coating film, and a mold of the shape of the inverted diffraction grating pattern of the diffraction optical element portion is transferred onto the coating film. Thereafter, the glass portion is heated to about 125°C and fired, and a diffraction optical element portion of the size shown in Table 2 is formed at a specified position on the main surface of the glass portion. Next, a siloxane polymer is coated as an organic material on the other main surface to form a coating film, and a mold of the shape of the inverted diffraction grating pattern of the diffraction optical element portion is transferred onto the coating film. Thereafter, the glass portion is heated to about 125°C and fired, and a diffraction optical element portion of the size shown in Table 2 is formed at a specified position on the other main surface of the glass portion. A glass wafer having diffraction optical element portions formed on both main surfaces is obtained.
[0220] [Made from inorganic materials]
[0221] A titanium oxide film, a silicon nitride film, or a silicon carbide film is formed on one main surface of the glass portion in a vacuum chamber by sputtering. After the film is formed, it is taken out of the vacuum chamber, and a photoresist liquid is uniformly coated on the main surface of the glass portion where the film is formed. The glass portion is then heated to evaporate the solvent of the photoresist (pre-baking), and a photomask having a pattern corresponding to the periodic fine structure pattern of the diffractive optical element is used to transfer the pattern of the photomask to the photoresist on the surface of the glass portion by irradiating ultraviolet rays (exposure). After exposure, the photoresist is selectively removed using a developer (development), and each glass portion is heated to about 120 to 150°C to thermally crosslink the photoresist (post-baking). Next, the film on the main surface of the glass portion is selectively etched to form a diffractive optical element portion. Thereafter, a diffractive optical element portion is formed at a specified position on the other main surface by the same method. In this way, a glass wafer having a diffractive optical element portion of a size shown in Table 2 is obtained.
[0222] [Period (pitch) of the concave-convex structure of the diffraction grating]
[0223] Determined by scanning electron microscopy (SEM).
[0224] [Difference in height between the convex and concave parts of the diffraction grating]
[0225] Measured by atomic force microscopy (AFM).
[0226] (Example 2)
[0227] The glass wafer produced in Example 1 was cut and separated by dicing to produce a plurality of light guide plates. Table 2 shows the size and number of light guide plates obtained from one glass wafer.
[0228] (Example 3)
[0229] The light guide plate produced in Example 2 is assembled into Figure 2 In the head mounted display 1 shown. That is, the light guide plate produced in Example 2 is mounted on the frame together with the light source and the optical system, and a glasses-type image display device is produced. When the image display device is worn to display images, images with a high FOV can be displayed with high image quality, and a sufficient sense of immersion can be obtained.
[0230] Table 2(1)
[0231]
[0232] Table 2(2)
[0233]
[0234]
[0235] Table 2(3)
[0236]
[0237]
[0238] The embodiments disclosed this time should be considered as illustrative in all aspects and not restrictive. The scope of the present invention is indicated by the claims rather than the above description, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0239] For example, by adjusting the composition of the glass composition exemplified above as described in the specification, the optical glass of one embodiment of the present invention can be produced.
[0240] In addition, it is apparent that two or more items described as examples or preferred ranges in the specification can be arbitrarily combined.
Claims
1. A glass wafer for manufacturing a light guide plate, characterized in that: A glass portion having a thin plate shape and having diffractive optical element portions on both main surfaces thereof, The area of one main surface of the glass portion is 1950 mm 2 above, The thickness of the glass part is less than 3.0 mm. The Young's modulus of the glass portion is 100 GPa or more.
2. The glass wafer according to claim 1, The diffractive optical element portion has a periodic concavo-convex structure, and the period of the concavo-convex structure is 500 nm or less.
3. The glass wafer according to claim 1, The refractive index nd of the glass portion is 1.9 or more.
4. The glass wafer according to claim 1, The average linear expansion coefficient of the glass part at -30℃ to 70℃ is 80×10 -6 K -1 the following.
5. A light guide plate, characterized in that: A glass portion having diffractive optical element portions on two main surfaces thereof, The thickness of the glass part is less than 3.0 mm. The Young's modulus of the glass portion is 100 GPa or more.
6. The light guide plate according to claim 5, The diffractive optical element portion has a periodic concavo-convex structure, and the period of the concavo-convex structure is 500 nm or less.
7. The light guide plate according to claim 5, wherein: The refractive index nd of the glass portion is 1.9 or more.
8. An image display device, The light guide plate comprising the light guide plate according to claim 5.
9. The image display device according to claim 8, The image display device is of a glasses type.