Photoresist composition and preparation method thereof
By using a quaternary resin containing a tannic acid structure in the photoresist to combine with natural colloids to form a hydrogen bond structure, the problem of edge erosion by photoacid generators is solved, edge roughness and surface defects are significantly reduced, and the improve film quality.
Patent Information
- Application Number
- CN202410850272.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
During the pattern preparation process of existing photoresists, the edge of the pattern is eroded by the photoacid generator, resulting in high edge roughness, and surface particles are easily introduced, affecting the film forming quality.
Quaternary resin containing a tannic acid structure is combined with natural colloids to form a hydrogen bond structure to resist the erosion of photoacid generators and improve the film-forming quality of the photoresist.
It effectively reduces the edge roughness and surface defects of the photoresist, significantly improves the film-forming quality, and significantly reduces the number of surface defects.
Smart Images

Figure CN118732392A_ABST
Abstract
Description
Technical field:
[0001] The invention belongs to the technical field of integrated circuits, and in particular relates to a photoresist composition and a preparation method thereof. Background technology:
[0002] Photoresist, also known as photoresist, is the most critical material in the photolithography process. The pattern on the mask is projected onto the photoresist, stimulating a photochemical reaction, and forming a photoresist pattern after baking and development. Since the first chemically amplified photoresist came out in 1982, scientists have been continuously upgrading and improving the various properties of photoresists. In addition to intrinsic properties such as viscosity, specific gravity, and refractive index, the performance of photoresists also includes processing properties such as energy, feature size, focal length, process window, and edge roughness (LWR). Among them, the improvement of edge roughness and surface defects has always been a hot topic in the field of photoresists. After exposure and development, part of the photoresist is dissolved in the developer, and the other part of the photoresist remains on the surface of the wafer to form the required pattern. The edges of these photoresist patterns are rough and uneven, and this phenomenon is quantified and called edge roughness. Surface defects are surface particles or blank spots carried by the photoresist itself or introduced during the spin coating process. Edge roughness and surface defects will be transferred to the semiconductor substrate during etching or ion implantation, resulting in unstable electrical properties during the period. In the process of preparing patterns, the photoacid generator corrodes the pattern edges, resulting in rough edges. In addition, the existing photoresists are prone to introducing surface particles, resulting in problems such as low film quality. Summary of the invention:
[0003] To solve the above problems, the present application provides a photoresist composition and a preparation method thereof. A quaternary resin is prepared and a natural colloid is introduced into the formula, which can effectively resist the erosion of the photoacid generator on the edge of the photoresist and improve the surface film quality, thereby reducing the edge roughness and surface defects.
[0004] To achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0005] A photoresist composition comprises the following components in mass fractions:
[0006] 5-50% of copolymer containing tannic acid structure, preferably 10-25%;
[0007] Colloid 0.01-2%, preferably 0.1-1%;
[0008] Photoacid generator 0.1-10%, preferably 0.5-3%;
[0009] Acid diffusion inhibitor 0.1-10%, preferably 0.5-3%;
[0010] Organic solvent 30-92%, preferably 65-90%;
[0011] Preferably, the copolymer containing tannic acid structure comprises structural unit Q, structural unit X, structural unit Y and structural unit Z:
[0012] Among them, the structure of the structural unit Q is:
[0013]
[0014] R1 is hydrogen, C1-C12 branched or straight chain alkyl, preferably hydrogen, C1-C5 branched or straight chain alkyl;
[0015] The structure of the structural unit X is: Wherein R2 is hydrogen, C1-C30 branched or straight chain alkyl, trifluoromethyl, halogen, halogen substituted alkyl, preferably hydrogen, C1-C10 branched or straight chain alkyl;
[0016] The structure of the structural unit Y is: Wherein R3 is hydrogen, C1-C30 branched or straight chain alkyl, trifluoromethyl, halogen, halogen substituted alkyl, preferably hydrogen, C1-C10 branched or straight chain alkyl, R4 has 0-5, R4 is selected from hydrogen, C3-C30 alkyl, preferably hydrogen, C3-C8 alkyl.
[0017] The structural unit Z is selected from one or more of the following structures:
[0018]
[0019] R5, R7, R10, and R11 are each independently selected from hydrogen, C1-C30 branched or straight-chain alkyl, trifluoromethyl, halogen, and halogen-substituted alkyl, preferably hydrogen, C1-C10 branched or straight-chain alkyl; R8 is selected from hydrogen, C1-C12 alkyl, and C4-C12 cycloalkyl, preferably hydrogen and C1-C7 alkyl; R6, R9, and R12 are each independently selected from C4-C30 substituted or unsubstituted branched alkyl, and C4-C30 substituted or unsubstituted cycloalkyl, preferably C4-C10 substituted or unsubstituted branched alkyl, and C4-C10 substituted or unsubstituted cycloalkyl.
[0020] Preferably, the molar ratio of the structural unit Q, the structural unit X, the structural unit Y and the structural unit Z is 0-30:0-70:0-30:10-40, wherein the molar numbers of the structural unit Q, the structural unit X and the structural unit Y are not equal to zero.
[0021] More preferably, the molar ratio of the structural unit Q, the structural unit X, the structural unit Y and the structural unit Z is 3-20:20-60:5-20:10-30.
[0022] Preferably, the tetrapolymer containing tannic acid structure is prepared by copolymerization of double-bond modified tannic acid, p-hydroxystyrene compound, styrene compound and compound containing acid labile group protection structure.
[0023] Preferably, the structural formula of the double bond modified tannic acid is: wherein R1 is defined the same as above.
[0024] Preferably, the structure of the p-hydroxystyrene compound is: wherein R2 is defined the same as above.
[0025] Preferably, the structure of the styrene compound is: The definitions of R3 and R4 are the same as above.
[0026] Preferably, the compound containing an acid-labile group protection structure is selected from one or more of the following structures:
[0027] The definitions of substituents R5 to R12 are the same as those above.
[0028] Preferably, the double bond modified tannic acid is selected from one or more of acrylic acid modified tannic acid, methacrylic acid modified tannic acid, ethacrylic acid modified tannic acid, and propylacrylic acid modified tannic acid.
[0029] Preferably, the double bond modified tannic acid is prepared by reacting tannic acid with olefinic acid chloride;
[0030] Preferably, the preparation method of the double-bond modified tannic acid is as follows: dissolving tannic acid in a solvent and stirring to dissolve; adding an inorganic base to the solution and stirring; and adding olefinic acid chloride to react to prepare the double-bond modified tannic acid.
[0031] Preferably, the solvent is an amine solvent selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and N-ethylpyrrolidone.
[0032] Preferably, the inorganic base is selected from alkali metal carbonates and alkali metal bicarbonates, and is used to activate the hydrogen on the hydroxyl group of tannic acid, preferably one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate;
[0033] Preferably, the molar ratio of the inorganic base to tannic acid is 5 to 20:1.
[0034] Preferably, the olefinic acid chloride is selected from one or more of acryloyl chloride, methacryloyl chloride, ethylacryloyl chloride, and propylacryloyl chloride;
[0035] Preferably, the molar ratio of olefinic acid chloride to tannic acid is 1 to 5:1.
[0036] Preferably, in the reaction for preparing double-bond modified tannic acid, the reaction is carried out at room temperature and the reaction time is 12 to 72 hours.
[0037] After the reaction is completed, the obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove the solvent, and then the product after rotary evaporation is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then the extraction liquid is used for extraction three times, and the obtained organic phase is rotary evaporated, and finally the oily product after rotary evaporation is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product double-bond modified tannic acid;
[0038] Preferably, the extracting liquid is a saturated sodium chloride solution and tetrahydrofuran.
[0039] Preferably, the p-hydroxystyrene compound is selected from p-hydroxystyrene, 2-alkyl p-hydroxystyrene, 3-alkyl p-hydroxystyrene, 2,6-alkyl p-hydroxystyrene, 2,5-alkyl p-hydroxystyrene, 3,5-alkyl p-hydroxystyrene, 3,6-alkyl p-hydroxystyrene, more preferably p-hydroxystyrene, 2-alkyl p-hydroxystyrene, 3-alkyl p-hydroxystyrene;
[0040] Preferably, the styrene compound is selected from styrene, 2-alkylstyrene, 3-alkylstyrene, 2,6-alkylstyrene, 2,5-alkylstyrene, 3,5-alkylstyrene, 3,6-alkylstyrene, more preferably styrene, 2-alkylstyrene, 3-alkylstyrene;
[0041] Preferably, the compound containing an acid-labile group protecting structure is selected from at least three of tert-butyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, tert-butoxystyrene, tert-butoxycarbonylstyrene, ethoxyethoxystyrene, cyclohexaneoxystyrene, propoxypropoxystyrene, cyclopentaneoxystyrene, cyclopentaneoxyethoxystyrene, propoxyethoxystyrene, tert-butoxypropoxystyrene, tetrahydropyranylstyrene and tert-butoxycarbonyl, and more preferably tert-butyl acrylate, cyclopentyl acrylate, cyclohexane acrylate, tert-butoxystyrene, tert-butoxycarbonylstyrene, ethoxyethoxystyrene, cyclohexaneoxystyrene and tetrahydropyranylstyrene.
[0042] The copolymerization process is a prior art in the art, and the present invention does not make specific requirements. For example, free radical polymerization can be used for copolymerization, and reference can be made to the methods disclosed in patents such as US2005 / 0186507A1, EP1343048A2, EP1020768A1, and US2008 / 0193878 A1.
[0043] In the present invention, the weight average molecular weight of the copolymer containing tannic acid structure is 1,000 to 100,000, preferably 5,000 to 30,000, for example, 10,000.
[0044] In the present invention, the copolymer containing tannic acid structure comprises 0-30 mol%, preferably 3-20 mol% of double bond modified tannic acid structural units; 0-70 mol%, preferably 20-60 mol% of p-hydroxystyrene compound structural units; 0-30 mol%, preferably 5-20 mol% of styrene compound structural units; and 10-40 mol%, preferably 10-30 mol% of compound structural units containing acid-labile group protection structures. The molar numbers of the above structural units are not 0.
[0045] The introduction of natural colloids into the formulation can form a large number of hydrogen bond structures with tannic acid to improve the film quality of the photoresist. Preferably, the colloid is a polysaccharide or protein, which can be extracted from plants or animals, preferably one or more of gelatin, xanthan gum, gellan gum, agar, and carrageenan.
[0046] Preferably, the photoacid generator is selected from one or more of onium salts, triazines, sulfonyldiazomethanes, oxime esters, and nitrobenzyl sulfonates, preferably perfluorobutyltriphenylsulfonium salt, trifluoromethyltriphenylsulfonium salt, o-trifluoromethylphenyltriphenylsulfonium salt, p-trifluoromethylphenyltriphenylsulfonium salt, perfluorobutyldiphenyliodonium salt, trifluoromethyldiphenyliodonium salt, o-trifluoromethylphenyldiphenyliodonium salt, p-trifluoromethylphenyldiphenyliodonium salt, bis(4-tert-butylphenyl)iodocamphorsulfonate, bis(4-tert-butylphenyl)iodotrifluoromethanesulfonate, trichloroacetophenone, tribromomethylphenylsulfone, 4-phenoxydichloroacetophenone, 4,6 -bis(trichloromethyl)-1,3,5-triazine derivatives, α,α-bis(arylsulfonyl)diazomethane, α-carbonyl-α-sulfonyldiazomethanes, N-trifluoromethylsulfonyloxyphthalimide, N-trifluoromethylsulfonyloxy-1,8-naphthalimide, succinimidyl arylene sulfonate, N-hydroxyphthalimide p-toluenesulfonate, o-nitrobenzyl sulfonate, α-aroyl sulfonate, α-sulfone acetophenones, aryl phosphate esters, more preferably one or more of perfluorobutyl triphenylsulfonium salt, o-trifluorotolyl triphenylsulfonium salt and α,α-bis(arylsulfonyl)diazomethane.
[0047] Preferably, the acid diffusion inhibitor is an amine compound, including any one or more of trioctylamine, tetrabutylammonium hydroxide, 2-methoxyethoxyethyl-2-triamine, isopropanolamine, N,N-dimethylaminoethyl acetate, N,N-dimethylglycine, 2,6-dioxaheptylamine, 4,4'-diaminodiphenyl ether, N-tert-butoxycarbonyl dioctylamine, N,N-dimethylformamide, acetamide, N-methylacetamide and benzamide.
[0048] Preferably, the organic solvent is selected from one or more of ketone solvents, polyols, alkyl ethers, alkyl acid solvents, and amide solvents, preferably one or more of acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone, 2-heptanone, ethylene glycol, ethylene glycol monoacetate, diethylene glycol, ethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol and dipropylene glycol monoacetate, as well as their monomethyl, monoethyl, monopropyl, monobutyl and monophenyl ethers, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone, more preferably one or more of diethylene glycol methyl ethyl ether, propylene glycol monomethyl ether and ethyl lactate.
[0049] The present invention also provides a method for preparing the photoresist composition: the copolymer containing tannic acid structure, natural colloid, photoacid generator, acid diffusion inhibitor and organic solvent are mixed to obtain the photoresist composition.
[0050] The photoresist composition of the invention is suitable for high-energy radiation beams, and is suitable for forming micrometer-scale or nanometer-scale patterns in integrated circuits or for use in the field of optoelectronic products.
[0051] Compared with the prior art, this application has the following beneficial effects:
[0052] The multi-hydroxyl groups of tannic acid form hydrogen bonds with natural colloids, which can effectively resist the erosion of the photoacid generator on the edge of the photoresist. The overall roughness can be reduced by about 1 times, and the surface film quality can be improved, which can greatly reduce surface defects and reduce the number of surface defects to zero at most. Description of the drawings:
[0053] Figure 1 The infrared spectra of tannic acid before and after double bond modification in Example 1;
[0054] Figure 2 is a slice diagram of the photoresist resin PR-A of Example 1;
[0055] Figure 3 It is a cross-sectional view of the photoresist resin PR-A′ in the comparative example. Specific implementation method:
[0056] The specific implementation scheme of the method is further described below in conjunction with examples. However, the present invention is not limited to the listed embodiments, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0057] In the various embodiments and comparative examples of the present invention, the sources of the main raw materials are as follows. Unless otherwise specified, other raw materials and reagents are purchased through common commercial channels:
[0058] Tannic acid, purchased from Sigma Aldrich;
[0059] Acryloyl chloride, purchased from Sigma Aldrich;
[0060] Methacryloyl chloride, purchased from Sigma Aldrich;
[0061] Ethyl acryloyl chloride, purchased from Sigma Aldrich;
[0062] Propyl acryloyl chloride was purchased from Beijing Bailingwei Technology Co., Ltd.;
[0063] p-Acetoxystyrene was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0064] 2-Methyl-p-acetoxystyrene was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0065] Tert-butyl acrylate was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0066] Tert-butoxystyrene was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0067] Cyclopentyl acrylate was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0068] Tert-Butoxycarbonylstyrene was purchased from Yantai Wanrun Fine Chemical Co., Ltd.;
[0069] 2-Methylstyrene, purchased from Beijing Bailingwei Technology Co., Ltd.;
[0070] Ethoxyethoxystyrene was purchased from Yantai Wanrun Fine Chemical Co., Ltd.;
[0071] Perfluorobutyltriphenylsulfonium salt was purchased from Shanghai Daran Chemical Co., Ltd.;
[0072] o-Trifluoromethylphenyl diphenyl iodonium salt was purchased from Changzhou Qiangli Pioneer Electronic Materials Co., Ltd.;
[0073] Perfluorobutyldiphenyliodonium salt was purchased from Changzhou Qiangli Pioneer Electronic Materials Co., Ltd.
[0074] o-Trifluoromethylphenyl triphenylsulfonium salt was purchased from Changzhou Qiangli Pioneer Electronic Materials Co., Ltd.;
[0075] Bis(p-tolylsulfonyl)diazomethane was purchased from Shanghai Daran Chemical Co., Ltd.;
[0076] Bis(p-cyclohexylsulfonyl)diazomethane was purchased from Shanghai Daran Chemical Co., Ltd.
[0077] Example 1
[0078] Preparation of acrylic acid modified tannic acid: Add 17g of tannic acid (TA) to 100mL of N,N-dimethylformamide, stir until completely dissolved, then add 6.91g of potassium carbonate, stir for 3h, then add 0.905g of acryloyl chloride dropwise into the reaction bottle, and stir at room temperature for 12h. The obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove N,N-dimethylformamide. Then the product after rotary evaporation is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then extracted three times with saturated sodium chloride solution and tetrahydrofuran, and the obtained tetrahydrofuran phase is rotary evaporated, and finally the oily product after rotary evaporation is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product (TA-DA).
[0079] The double bond grafting of the final product was confirmed by FT-IR. FT-IR was performed using a VERTEX 70 infrared spectrometer from Bruker, Germany, at room temperature with a wavelength of 2000-500 cm -1 , potassium bromide tableting method was used to prepare the sample. The infrared spectrum of the modified tannic acid was compared with that of the tannic acid before modification (refer to Figure 1 , Figure 1 The upper spectrum is the infrared spectrum after modification, and the lower spectrum is the spectrum before modification). It can be found that the infrared spectrum after modification is at 1656cm -1 There is an additional characteristic absorption peak at the position, which is the stretching vibration peak of the C=C double bond. This proves that a double bond is connected after tannic acid modification.
[0080]
[0081] Preparation of quaternary resin A: 5.265g of acrylic acid-modified tannic acid, 9.72g of para-acetoxystyrene, 1.768g of styrene, 2.56g of tert-butyl acrylate and 0.6g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin A1. The above resin A1 was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin A.
[0082] Preparation of photoresist: 10 wt % of resin A, 0.1 wt % of gelatin, 0.5 wt % of perfluorobutyl triphenylsulfonium salt, and 0.5 wt % of trioctylamine were dissolved in 88.9 wt % of propylene glycol monomethyl ether, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-A.
[0083] Example 2
[0084] Preparation of methacrylic acid modified tannic acid: Add 17g of tannic acid to 300mL of N,N-dimethylacetamide, stir until completely dissolved, then add 21.2g of sodium carbonate, stir for 5h, then add 5.225g of methacryloyl chloride dropwise into the reaction bottle, and stir at room temperature for 72h. The obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove N,N-dimethylformamide. Then the product after rotary evaporation is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then saturated sodium chloride solution and tetrahydrofuran are used for extraction three times. The obtained tetrahydrofuran phase is rotary evaporated, and finally the oily product after rotary evaporation is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product.
[0085]
[0086] Preparation of quaternary resin B: 8.845g of methacrylic acid modified tannic acid, 8.91g of acetoxystyrene, 1.04g of styrene, 5.28g of tert-butoxystyrene and 0.4g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin B1. The above resin B1 was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin B.
[0087] Preparation of photoresist: 13 wt % of resin B, 0.3 wt % of xanthan gum, 0.8 wt % of o-trifluoromethylphenyl diphenyl iodonium salt, and 0.8 wt % of tetrabutylammonium hydroxide were dissolved in 85.1 wt % of propylene glycol monomethyl ether acetate, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-B.
[0088] Example 3
[0089] Preparation of ethacrylic acid modified tannic acid: Add 17g of tannic acid to 150mL of N-methylpyrrolidone, stir until completely dissolved, then add 10g of potassium bicarbonate, stir for 4h, then add 2.37g of ethacryloyl chloride dropwise into the reaction bottle, and stir at room temperature for 24h. The obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove N,N-dimethylformamide. Then the rotary evaporated product is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then extracted three times with saturated sodium chloride solution and tetrahydrofuran, and the obtained tetrahydrofuran phase is rotary evaporated, and finally the rotary evaporated oily product is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product.
[0090]
[0091] Preparation of quaternary resin C: 17.83g of ethyl acrylic acid modified tannic acid, 8.1g of para-acetoxystyrene, 1.56g of styrene, 4.8g of ethoxyethoxystyrene and 0.5g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin C1. The above resin C1 was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin C.
[0092] Preparation of photoresist: 16 wt % of resin C, 0.5 wt % of gellan gum, 1 wt % of perfluorobutyldiphenyliodonium salt, and 0.8 wt % of isopropanolamine were dissolved in 81.7 wt % of ethyl lactate, and filtered through a filter with a pore size of 0.22 μm to obtain a photoresist composition PR-C.
[0093] Example 4
[0094] Preparation of propyl acrylic acid modified tannic acid: Add 17g of tannic acid to 200mL of N-ethylpyrrolidone, stir until completely dissolved, then add 12.6g of sodium bicarbonate, stir for 5h, then add 3.975g of propyl acryloyl chloride dropwise into the reaction bottle, and stir at room temperature for 36h. The obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove N,N-dimethylformamide. Then the rotary evaporated product is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then extracted three times with saturated sodium chloride solution and tetrahydrofuran, and the obtained tetrahydrofuran phase is rotary evaporated, and finally the rotary evaporated oily product is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product.
[0095]
[0096] Preparation of quaternary resin D: 26.955g of propyl acrylic acid modified tannic acid, 8.1g of para-acetoxystyrene, 0.52g of styrene, 4.2g of cyclopentyl acrylate and 0.2g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin D1. The above resin D1 was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin D.
[0097] Preparation of photoresist: 20 wt % of resin D, 0.7 wt % of agar, 1.5 wt % of trifluoromethylbenzene triphenylsulfonium salt, and 1.2 wt % of 2,6-dioxaheptylamine were dissolved in 76.6 wt % of diethylene glycol methyl ethyl ether, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-D.
[0098] Example 5
[0099] Preparation of acrylic acid modified tannic acid: Add 34g of tannic acid to 600mL of N,N-dimethylformamide, stir until completely dissolved, then add 41.46g of potassium carbonate, stir for 3h, then add 3.8g of acryloyl chloride dropwise into the reaction bottle, and stir at room temperature for 48h. The obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove N,N-dimethylformamide. Then the product after rotary evaporation is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then extracted three times with saturated sodium chloride solution and tetrahydrofuran, and the obtained tetrahydrofuran phase is rotary evaporated, and finally the oily product after rotary evaporation is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product.
[0100]
[0101] Preparation of quaternary resin E: 31.59g acrylic acid modified tannic acid, 9.152g 2-methyl paraacetoxystyrene, 2.08g styrene, 2.2g tert-butyloxycarbonylstyrene and 0.7g initiator AIBN were dissolved in 50mL isopropanol, reacted at 70-90°C for 8-12h, and after the reaction, the reaction solution was poured into 1.5L methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin C1. The above resin C1 was placed in a three-necked flask, and 50mL methanol was added, and then 1.5g 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin E.
[0102] Preparation of photoresist: 22wt% of resin E, 0.8wt% of carrageenan, 2wt% of bis(p-tolylsulfonyl)diazomethane, and 1.8wt% of N,N-dimethylformamide are dissolved in 33.4wt% of ethyl lactate and 40wt% of propylene glycol monomethyl ether, and filtered through a filter with a pore size of 0.22um to obtain a photoresist composition PR-E.
[0103] Example 6
[0104] Preparation of methacrylic acid tannic acid: Add 34g of tannic acid to 400mL of N,N-dimethylacetamide, stir until completely dissolved, then add 21.2g of sodium carbonate, stir for 5h, then add 5.22g of methacryloyl chloride dropwise into the reaction bottle, and stir at room temperature for 60h. The obtained reaction solution is placed on a rotary evaporator for rotary evaporation to remove N,N-dimethylformamide. Then the product after rotary evaporation is redissolved in water, hydrochloric acid is added dropwise to adjust the solution to acidity, and then extracted three times with saturated sodium chloride solution and tetrahydrofuran, and the obtained tetrahydrofuran phase is rotary evaporated, and finally the oily product after rotary evaporation is placed in a vacuum oven to remove the liquid solvent to obtain the final solid product.
[0105]
[0106] Preparation of quaternary resin F: 35.38g of methacrylic acid modified tannic acid, 4.86g of para-acetoxystyrene, 2.36g of 2-methylstyrene, 5.28g of tert-butoxystyrene and 0.8g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin F1. The above resin F1 was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain resin F.
[0107] Preparation of photoresist: 25wt% resin F, 1wt% gelatin, 3wt% bis(p-cyclohexylsulfonyl)diazomethane, and 3wt% N,N-dimethylacetamide are dissolved in 38wt% ethyl lactate and 30wt% propylene glycol monomethyl ether acetate, and filtered through a filter with a pore size of 0.22um to obtain a photoresist composition PR-F.
[0108] Comparative Example:
[0109] Preparation of poly(p-hydroxystyrene-styrene-tert-butyl acrylate): 9.72g of p-acetoxystyrene, 1.768g of styrene, 2.56g of tert-butyl acrylate and 0.6g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain a resin intermediate resin. The above resin was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain the final resin.
[0110] Preparation of poly(p-hydroxystyrene-styrene-tert-butoxystyrene): 8.91g of p-acetoxystyrene, 1.04g of styrene, 5.28g of p-tert-butoxystyrene and 0.4g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain an intermediate resin. The above resin was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain the final resin.
[0111] Preparation of poly(p-hydroxystyrene-styrene-ethoxyethoxystyrene): 8.1g of p-acetoxystyrene, 1.56g of styrene, 4.8g of ethoxyethoxystyrene and 0.5g of initiator AIBN were dissolved in 50mL of isopropanol and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain an intermediate resin. The above resin was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain the final resin.
[0112] Preparation of poly(p-hydroxystyrene-styrene-cyclopentyl acrylate): 8.1g of p-acetoxystyrene, 0.52g of styrene, 4.2g of cyclopentyl acrylate and 0.2g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain an intermediate resin. The above resin was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain the final resin.
[0113] Preparation of poly(2-methyl-p-hydroxystyrene-styrene-tert-butyloxycarbonylstyrene): 9.152g of 2-methyl-p-acetoxystyrene, 2.08g of styrene, 2.2g of tert-butyloxycarbonylstyrene and 0.7g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain an intermediate resin. The above resin was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain the final resin.
[0114] Preparation of poly(p-hydroxystyrene-2-methylstyrene-tert-butoxystyrene): 4.86g of p-acetoxystyrene, 2.36g of 2-methylstyrene, 5.28g of tert-butoxystyrene and 0.8g of initiator AIBN were dissolved in 50mL of isopropanol, and reacted at 70-90°C for 8-12h. After the reaction, the reaction solution was poured into 1.5L of methanol for precipitation. The filter cake obtained by filtration was rinsed with 500mL of methanol and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain an intermediate resin. The above resin was placed in a three-necked flask, and 50mL of methanol was added, and then 1.5g of 25% ammonia solution was added. The three-necked flask was placed in a 55°C oil bath and heated for reaction for 5 hours. After the reaction, the reaction solution was poured into 1L of deionized water for precipitation. The filter cake obtained by filtration was rinsed with 200mL of deionized water and placed in a vacuum drying oven at 55°C for vacuum drying overnight to obtain the final resin.
[0115] Comparative example PR-A′: 10 wt% of resin poly(tert-butyl p-hydroxystyrene-styrene-acrylate), 0.5 wt% of perfluorobutyl triphenylsulfonium salt, and 0.5 wt% of trioctylamine are dissolved in 89.0 wt% of propylene glycol monomethyl ether, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-A′.
[0116] Comparative example PR-B′: 13 wt% of resin poly(p-hydroxystyrene-styrene-tert-butoxystyrene), 0.8 wt% of o-trifluoromethylphenyl diphenyl iodonium salt, and 0.8 wt% of tetrabutylammonium hydroxide are dissolved in 85.4 wt% of propylene glycol monomethyl ether acetate, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-B′.
[0117] Comparative Example PR-C′: 16 wt% of resin poly(p-hydroxystyrene-styrene-ethoxyethoxystyrene), 1 wt% of perfluorobutyldiphenyliodonium salt, and 0.8 wt% of isopropanolamine are dissolved in 82.2 wt% of ethyl lactate, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-C′.
[0118] Comparative example PR-D′: 20 wt% of resin poly(p-hydroxystyrene-styrene-cyclopentyl acrylate), 1.5 wt% of o-trifluoromethylphenyl triphenylsulfonium salt, and 1.2 wt% of 2,6-dioxaheptylamine were dissolved in 77.3 wt% of diethylene glycol methyl ethyl ether, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-D′.
[0119] Comparative example PR-E′: 22 wt% of resin poly(2-methyl-p-hydroxystyrene-styrene-tert-butyloxycarbonylstyrene), 2 wt% of bis(p-tolylsulfonyl)diazomethane, and 1.8 wt% of N,N-dimethylformamide are dissolved in 34.2 wt% of ethyl lactate and 40 wt% of propylene glycol monomethyl ether, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-E′.
[0120] Comparative example PR-F′: 25 wt% of resin poly(p-hydroxystyrene-2-methylstyrene-tert-butoxystyrene), 3 wt% of bis(p-cyclohexylsulfonyl)diazomethane, and 3 wt% of N,N-dimethylacetamide are dissolved in 39 wt% of ethyl lactate and 30 wt% of propylene glycol monomethyl ether acetate, and filtered through a filter with a pore size of 0.22 um to obtain a photoresist composition PR-F′.
[0121] Test example:
[0122] Take 12 types of photoresists, including application examples PR-A to PR-F and comparative examples PR-A′ to PR-F′, and use silicon wafers treated with hexamethyldisilazane to spin-coat the photoresists. The instrument used is a coating machine, and the rotation speed is adjusted to make the film thickness after drying about 500nm. The drying process is to pre-bake the silicon wafer coated with photoresist on a 100℃ hot stage for 60s. The silicon wafer is exposed using a DUV exposure machine, and the exposure amount and focus are gradually changed. The silicon wafer is then post-baked on a 120℃ hot stage for 60s, and then the silicon wafer is sprayed with 2.38% tetramethylammonium hydroxide solution for 60s using a developer, rinsed with deionized water for 60s, and finally dried.
[0123] After the operation is completed, the exposed pattern is observed with a scanning electron microscope, and the position of the photoresist pattern boundary is determined by scanning, and the deviation between the boundary and the average boundary is determined to obtain the standard deviation of the measured photoresist pattern boundary. In the field of photolithography, the edge roughness (LWR) is quantitatively described with 3 times of the boundary standard deviation. The number of surface defects is detected by a defect detector, and the results are shown in the following table. In addition, the photoresists of Example 1 and Comparative Example 1 are sliced and observed by a high-resolution scanning electron microscope to obtain the morphology of the photoresist pattern.
[0124] LWR / nm number of defects PR-A 7.3 2 PR-B 9.8 1 PR-C 6.9 0 PR-D 8.9 0 PR-E 11.5 0 PR-F 11.1 0 PR-A′ 16.5 10 PR-B′ 19.6 9 PR-C′ 15.8 6 PR-D′ 18.7 5 PR-E′ 22.2 5 PR-F′ 20.3 6
[0125] From the comparison between PR-A~PR-F and PR-A′~PR-F′ in the table, it can be seen that after introducing modified tannic acid monomers into the ternary resin to obtain a quaternary photoresist resin and adding natural colloids into the formula, the edge roughness of the obtained photoresist pattern is significantly improved, and the overall roughness can be reduced by about 1 times, and the surface defects are also greatly reduced. It can also be clearly seen from the slice diagram that the edge roughness of the quaternary photoresist resin introduced with natural colloids and modified tannic acid is significantly better than that of the ternary resin.
[0126] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A photoresist composition, characterized in that The components include the following mass fractions: 5-50% of copolymer containing tannic acid structure, preferably 10-25%; Colloid 0.01-2%, preferably 0.1-1%; Photoacid generator 0.1-10%, preferably 0.5-3%; Acid diffusion inhibitor 0.1-10%, preferably 0.5-3%; The organic solvent is 30-92%, preferably 65-90%.
2. The composition according to claim 1, characterized in that The copolymer containing tannic acid structure comprises structural unit Q, structural unit X, structural unit Y and structural unit Z: Among them, the structure of the structural unit Q is: R1 is hydrogen, C1-C12 branched or straight chain alkyl, preferably hydrogen, C1-C5 branched or straight chain alkyl; The structure of the structural unit X is: Wherein R2 is hydrogen, C1-C30 branched or straight chain alkyl, trifluoromethyl, halogen, halogen substituted alkyl, preferably hydrogen, C1-C10 branched or straight chain alkyl; The structure of the structural unit Y is: wherein R3 is hydrogen, C1-C30 branched or straight chain alkyl, trifluoromethyl, halogen, halogen-substituted alkyl, preferably hydrogen, C1-C10 branched or straight chain alkyl, R4 has 0-5, R4 is selected from hydrogen, C1-C30 alkyl, preferably hydrogen, C1-C8 alkyl; The structural unit Z is selected from one or more of the following structures: R5, R7, R10, and R11 are each independently selected from hydrogen, C1-C30 branched or straight-chain alkyl, trifluoromethyl, halogen, and halogen-substituted alkyl, preferably hydrogen, C1-C10 branched or straight-chain alkyl; R8 is selected from hydrogen, C1-C12 alkyl, and C4-C12 cycloalkyl, preferably hydrogen and C1-C7 alkyl; R6, R9, and R12 are each independently selected from C4-C30 substituted or unsubstituted branched alkyl, and C4-C30 substituted or unsubstituted cycloalkyl, preferably C4-C10 substituted or unsubstituted branched alkyl, and C4-C10 substituted or unsubstituted cycloalkyl.
3. The composition according to claim 2, characterized in that The molar ratio of the structural unit Q, the structural unit X, the structural unit Y and the structural unit Z is 0-30:0-70:0-30:10-40, wherein the molar numbers of the structural unit Q, the structural unit X and the structural unit Y are not equal to 0; Preferably, the molar ratio of the structural unit Q, the structural unit X, the structural unit Y and the structural unit Z is 3-20:20-60:5-20:10-30.
4. The composition according to any one of claims 1 to 3, characterized in that The tetrapolymer containing tannic acid structure is prepared by copolymerization of double-bond modified tannic acid, p-hydroxystyrene compound, styrene compound and compound containing acid labile group protection structure; Preferably, the structural formula of the double bond modified tannic acid is: Wherein R1 is defined the same as above; Preferably, the structure of the p-hydroxystyrene compound is: Wherein R2 is defined the same as above; Preferably, the structure of the styrene compound is: Wherein R3 and R4 are defined the same as above; Preferably, the compound containing an acid-labile group protection structure is selected from one or more of the following structures: The definitions of substituents R5 to R12 are the same as those above.
5. The composition according to any one of claims 1 to 4, characterized in that The double bond modified tannic acid is selected from one or more of acrylic acid modified tannic acid, methacrylic acid modified tannic acid, ethacrylic acid modified tannic acid, and propylacrylic acid modified tannic acid; Preferably, the double bond modified tannic acid is prepared by reacting tannic acid with olefinic acid chloride; Preferably, the preparation method of the double-bond modified tannic acid is: dissolving tannic acid in a solvent, adding an inorganic base, and then adding an olefinic acid chloride to react to prepare the double-bond modified tannic acid; Preferably, the solvent is an amine solvent selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and N-ethylpyrrolidone; Preferably, the inorganic base is selected from alkali metal carbonates, alkali metal bicarbonates, preferably one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate; Preferably, the molar ratio of the inorganic base to tannic acid is 5 to 20:1; Preferably, the olefinic acid chloride is selected from one or more of acryloyl chloride, methacryloyl chloride, ethylacryloyl chloride, and propylacryloyl chloride; Preferably, the molar ratio of olefinic acid chloride to tannic acid is 1 to 5:1; Preferably, in the reaction for preparing double-bond modified tannic acid, the reaction is carried out at room temperature and the reaction time is 12 h to 72 h.
6. The composition according to any one of claims 1 to 5, characterized in that The p-hydroxystyrene compound is selected from p-hydroxystyrene, 2-alkyl p-hydroxystyrene, 3-alkyl p-hydroxystyrene, 2,6-alkyl p-hydroxystyrene, 2,5-alkyl p-hydroxystyrene, 3,5-alkyl p-hydroxystyrene, 3,6-alkyl p-hydroxystyrene, more preferably p-hydroxystyrene, 2-alkyl p-hydroxystyrene, 3-alkyl p-hydroxystyrene; Preferably, the styrene compound is selected from styrene, 2-alkylstyrene, 3-alkylstyrene, 2,6-alkylstyrene, 2,5-alkylstyrene, 3,5-alkylstyrene, 3,6-alkylstyrene, more preferably styrene, 2-alkylstyrene, 3-alkylstyrene; Preferably, the compound containing an acid-labile group protecting structure is selected from at least three of tert-butyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, tert-butoxystyrene, tert-butoxycarbonylstyrene, ethoxyethoxystyrene, cyclohexaneoxystyrene, propoxypropoxystyrene, cyclopentaneoxystyrene, cyclopentaneoxyethoxystyrene, propoxyethoxystyrene, tert-butoxypropoxystyrene, tetrahydropyranylstyrene and tert-butoxycarbonyl, and more preferably tert-butyl acrylate, cyclopentyl acrylate, cyclohexane acrylate, tert-butoxystyrene, tert-butoxycarbonylstyrene, ethoxyethoxystyrene, cyclohexaneoxystyrene and tetrahydropyranylstyrene.
7. The composition according to any one of claims 1 to 6, characterized in that The weight average molecular weight of the copolymer containing tannic acid structure is 1000 to 100000, preferably 5000 to 30000; Preferably, the copolymer containing tannic acid structure comprises 0-30 mol%, preferably 3-20 mol% of double bond modified tannic acid structural units; 0-70 mol%, preferably 20-60 mol% of p-hydroxystyrene compound structural units; 0-30 mol%, preferably 5-20 mol% of styrene compound structural units; and 10-40 mol%, preferably 10-30 mol% of compound structural units containing acid-labile group protection structures, and the molar numbers of the above structural units are not 0.
8. The composition according to any one of claims 1 to 7, characterized in that The colloid is a polysaccharide or a protein, preferably one or more of gelatin, xanthan gum, gellan gum, agar, and carrageenan; Preferably, the photoacid generator is selected from one or more of onium salts, triazines, sulfonyldiazomethanes, oxime esters, and nitrobenzyl sulfonates, preferably perfluorobutyltriphenylsulfonium salt, trifluoromethyltriphenylsulfonium salt, o-trifluoromethylphenyltriphenylsulfonium salt, p-trifluoromethylphenyltriphenylsulfonium salt, perfluorobutyldiphenyliodonium salt, trifluoromethyldiphenyliodonium salt, o-trifluoromethylphenyldiphenyliodonium salt, p-trifluoromethylphenyldiphenyliodonium salt, bis(4-tert-butylphenyl)iodocamphorsulfonate, bis(4-tert-butylphenyl)iodotrifluoromethanesulfonate, trichloroacetophenone, tribromomethylphenylsulfone, 4-phenoxydichloroacetophenone, 4,6 -bis(trichloromethyl)-1,3,5-triazine derivatives, α,α-bis(arylsulfonyl)diazomethane, α-carbonyl-α-sulfonyldiazomethanes, N-trifluoromethylsulfonyloxyphthalimide, N-trifluoromethylsulfonyloxy-1,8-naphthalimide, succinimidyl arylidene sulfonate, N-hydroxyphthalimide p-toluenesulfonate, o-nitrobenzyl sulfonate, α-aroyl sulfonate, α-sulfone acetophenones, aryl phosphate esters, more preferably perfluorobutyl triphenylsulfonium salt, o-trifluorotolyl triphenylsulfonium salt and α,α-bis(arylsulfonyl)diazomethane One or more; Preferably, the acid diffusion inhibitor is an amine compound, including any one or more of trioctylamine, tetrabutylammonium hydroxide, 2-methoxyethoxyethyl-2-triamine, isopropanolamine, N,N-dimethylaminoethyl acetate, N,N-dimethylglycine, 2,6-dioxaheptylamine, 4,4'-diaminodiphenyl ether, N-tert-butoxycarbonyl dioctylamine, N,N-dimethylformamide, acetamide, N-methylacetamide and benzamide; Preferably, the organic solvent is selected from one or more of ketone solvents, polyols, alkyl ethers, alkyl acid solvents, and amide solvents, preferably one or more of acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone, 2-heptanone, ethylene glycol, ethylene glycol monoacetate, diethylene glycol, ethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol and dipropylene glycol monoacetate, as well as their monomethyl, monoethyl, monopropyl, monobutyl and monophenyl ethers, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone, more preferably one or more of diethylene glycol methyl ethyl ether, propylene glycol monomethyl ether and ethyl lactate.
9. A method for preparing the photoresist composition according to any one of claims 1 to 8, comprising mixing a copolymer containing a tannic acid structure, a colloid, a photoacid generator, an acid diffusion inhibitor, and an organic solvent to obtain the photoresist composition.
Citation Information
Patent Citations
Positive photoetching material based on tannic acid, preparation method of positive photoetching material, photoresist system and application of positive photoetching material in preparation of micro-nano circuit
CN114114840A
Nano composite material based on deep eutectic solvent and preparation method of nano composite material
CN116948420A
Preparation method of hydrophilic antibacterial mildew-proof photocuring coating
CN117777822A
Photocurable resin composition for color filter and production of color filter therefrom
JP1994080744A
Coloring composition, ink for inkjet, printing method, and compound
WO2017110387A1