Method for obtaining strong and weak factors of metaphosphate glass
By providing metal-oxygen and phosphorus-oxygen bond lengths and fitting equations, the determination of the strength factor of metaphosphate glass is simplified, solving the problem of difficult determination in the existing technology, and achieving highly accurate results and scientific significance. connection.
Patent Information
- Application Number
- CN202410993441.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to obtain the strength factor (m value) of glassy materials in the existing technology. In particular, the viscosity test in the supercooled liquid phase region is complex and cumbersome, which affects the characteristic kinetic analysis at the glass transition temperature (Tg).
Calculate the strength of metaphosphate glass by providing the average metal-oxygen bond length and the average phosphorus-oxygen bond length, and using fitting equations (such as exponential growth fitting equation m=a0×exp(rcry/b0)+c0) sex factor, simplifying the determination process.
The accurate determination of the strength factor of metaphosphate glass has been achieved. The operation is simple and the applicability is strong. The results are basically consistent with the literature reports. It connects the characteristics of crystalline materials and glassy materials and has scientific and practical significance.
Smart Images

Figure CN118737339A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of obtaining strength and weakness factors, and in particular to a method for obtaining the strength and weakness factor of metaphosphate glass. Background Art
[0002] The strength factor (m) of a glassy material is a characteristic kinetic parameter that directly affects the relaxation of a glassy material. It measures the change in viscosity of a supercooled liquid with temperature at the glass transition temperature (T g ) deviates from the Arrhenius law. In the prior art, the following formula is usually used to obtain the m value:
[0003]
[0004] Where m is the strength factor of the glassy material, η is the viscosity of the glassy material under a certain temperature condition, T is the actual temperature, T g is the glass transition temperature.
[0005] When using the above formula to obtain the strength factor of the glassy material, η is needed, but the viscosity test in the supercooled liquid phase is more difficult, which makes it difficult to obtain the η value.
[0006] In addition, other methods such as enthalpy difference, dielectric relaxation or mechanical relaxation can also be used in the prior art to test the m value, but the above methods usually require multiple heating and cooling around the glass transition curve or obtain multiple relaxation curves, and the steps are relatively cumbersome. Summary of the invention
[0007] The object of the present invention is to provide a method for obtaining the strength factor of metaphosphate glass. The method of the present invention can accurately measure the strength factor of metaphosphate glass, and the method is simple and easy to implement.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] The present invention provides a method for obtaining a strength factor of a metaphosphate glass, comprising the following steps:
[0010] Providing a metal-oxygen average bond length and a phosphorus-oxygen average bond length, wherein the metal-oxygen average bond length is the average bond length of the chemical bond between metal and oxygen in the metaphosphate crystal, and the phosphorus-oxygen average bond length is the average bond length of the chemical bond between phosphorus and oxygen in the metaphosphate crystal;
[0011] Providing a fitting equation, wherein the fitting equation is obtained by fitting the strength factor of a known metaphosphate glass to the ratio of the metal-oxygen average bond length and the phosphorus-oxygen average bond length, and the known metaphosphate glass has the same chemical composition as the metaphosphate crystal;
[0012] According to the metal-oxygen average bond length and the phosphorus-oxygen average bond length of the metaphosphate crystal corresponding to the metaphosphate glass to be tested and the fitting equation, the strength factor of the metaphosphate glass to be tested is obtained.
[0013] Preferably, the fitting is an exponential growth type fitting.
[0014] Preferably, the fitting equation is as shown in Formula I:
[0015] m=a0×exp(r cry / b0)+c0 Formula I;
[0016] In formula I, m is the strength factor, r cry is the ratio of the average metal-oxygen bond length to the average phosphorus-oxygen bond length, and a0, b0 and c0 are coefficients.
[0017] Preferably, a0=4.644±0.764, b0=0.694±0.013, c0=-0.145±0.652.
[0018] Preferably, the metaphosphate glass to be tested includes single metal metaphosphate glass or double metal metaphosphate glass.
[0019] Preferably, the two metals in the bimetallic metaphosphate glass are respectively recorded as the first metal and the second metal. When the metaphosphate glass to be tested is a bimetallic metaphosphate glass and the average bond length of the chemical bond between the first metal and oxygen in the metaphosphate crystal corresponding to the bimetallic metaphosphate glass is greater than the average bond length of the chemical bond between the second metal and oxygen, the metal-oxygen average bond length is the average bond length of the chemical bond between the first metal and oxygen.
[0020] Preferably, the metal elements in the metaphosphate glass to be tested include one or two of alkali metal elements, alkaline earth metal elements and transition metal elements.
[0021] Preferably, the alkali metal element includes K, Na or Rb; the alkaline earth metal element includes Ca, Sr or Ba; and the transition metal element includes Zn or Ag.
[0022] Preferably, the chemical formula of the monometallic metaphosphate glass includes Zn(PO3)2, NaPO3, Ca(PO3)2, Sr(PO3)2, Ba(PO3)2 or AgPO3.
[0023] Preferably, the chemical formula of the bimetallic metaphosphate glass includes NaZn(PO3)3, KZn(PO3)3, RbZn(PO3)3 or Ba2Zn3(PO3) 10 .
[0024] The present invention provides a method for obtaining the strength factor of metaphosphate glass, comprising the following steps: providing a metal-oxygen average bond length and a phosphorus-oxygen average bond length, wherein the metal-oxygen average bond length is the average bond length of the chemical bond between metal and oxygen in the metaphosphate crystal, and the phosphorus-oxygen average bond length is the average bond length of the chemical bond between phosphorus and oxygen in the metaphosphate crystal; providing a fitting equation, wherein the fitting equation is obtained by fitting the strength factor of a known metaphosphate glass to the ratio of the metal-oxygen average bond length and the phosphorus-oxygen average bond length, and the known metaphosphate glass has the same chemical composition as the metaphosphate crystal; according to the metal-oxygen average bond length and the phosphorus-oxygen average bond length of the metaphosphate crystal corresponding to the metaphosphate glass to be tested and the fitting equation, the strength factor of the metaphosphate glass to be tested is obtained. In the past, glassy materials and crystalline materials were generally considered to be two materials with very different structures and properties, and there were few reports on the connection between the two. The present invention obtains the strength factor of metaphosphate glass with the same chemical composition based on the characteristic parameters of metaphosphate crystals (i.e., the ratio of crystal bond lengths). The operation is simple and the applicability is strong. The result is highly accurate and basically consistent with the value reported in the literature. At the same time, the two characteristics of crystalline materials and their glassy materials with the same composition are linked for the first time, which has certain scientific and practical significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the configuration diagram of Zn-O polyhedron and PO polyhedron in Zn(PO3)2 crystal. DETAILED DESCRIPTION
[0026] The present invention provides a method for obtaining a strength factor of a metaphosphate glass, comprising the following steps:
[0027] Providing a metal-oxygen average bond length and a phosphorus-oxygen average bond length, wherein the metal-oxygen average bond length is the average bond length of the chemical bond between metal and oxygen in the metaphosphate crystal, and the phosphorus-oxygen average bond length is the average bond length of the chemical bond between phosphorus and oxygen in the metaphosphate crystal;
[0028] Providing a fitting equation, wherein the fitting equation is obtained by fitting the strength factor of a known metaphosphate glass to the ratio of the metal-oxygen average bond length and the phosphorus-oxygen average bond length, and the known metaphosphate glass has the same chemical composition as the metaphosphate crystal;
[0029] According to the metal-oxygen average bond length and the phosphorus-oxygen average bond length of the metaphosphate crystal corresponding to the metaphosphate glass to be tested and the fitting equation, the strength factor of the metaphosphate glass to be tested is obtained.
[0030] In the past, glassy materials and crystalline materials were generally considered to be two materials with very different structures and properties, and there were few reports on the connection between the two. The present invention obtains the strength factor of glassy materials (such as metaphosphate glass) based on the characteristic parameters (i.e., crystal bond length ratio) of crystalline materials (such as metaphosphate crystals). The operation is simple, the applicability is strong, the result is highly accurate, and it is basically consistent with the value reported in the literature; at the same time, it is the first time to connect the two characteristics of crystalline materials and their glassy materials with the same composition, which has certain scientific and practical significance. The method of the present invention is described in detail below.
[0031] The present invention provides metal-oxygen average bond length and phosphorus-oxygen average bond length. In the present invention, the phosphorus-oxygen average bond length is the average bond length of the chemical bond between phosphorus and oxygen in the metaphosphate crystal, denoted as r(PO) cry In the present invention, the metal-oxygen average bond length is the average bond length of the chemical bond between the metal and oxygen in the metaphosphate crystal, denoted as r(MO) cry . In the present invention, the metaphosphate crystals preferably include monometallic metaphosphate crystals or bimetallic metaphosphate crystals (the two metals in the bimetallic metaphosphate crystals are respectively recorded as the first metal and the second metal). In the present invention, the metal elements in the metaphosphate crystals preferably include one or two of alkali metal elements, alkaline earth metal elements and transition metal elements; the alkali metal elements preferably include K, Na or Rb; the alkaline earth metal elements preferably include Ca, Sr or Ba; the transition metal elements preferably include Zn or Ag. In the present invention, the chemical formula of the monometallic metaphosphate crystals preferably includes Zn(PO3)2, NaPO3, Ca(PO3)2, Sr(PO3)2, Ba(PO3)2 or AgPO3; the chemical formula of the bimetallic metaphosphate crystals preferably includes NaZn(PO3)3, KZn(PO3)3, RbZn(PO3)3 or Ba2Zn3(PO3) 10 .
[0032] In the present invention, when the metaphosphate crystal is a bimetallic metaphosphate crystal and the average bond length of the chemical bond between the first metal and oxygen is greater than the average bond length of the chemical bond between the second metal and oxygen, the metal-oxygen average bond length is the average bond length of the chemical bond between the first metal and oxygen. Specifically, the two metals in the bimetallic metaphosphate crystal are respectively denoted as M1 and M2, and the average bond lengths of the chemical bonds formed by M1 and M2 with oxygen are respectively denoted as r(M1-O). cry With r(M2-O) cry , if r(M1-O) cry >r(M2-O) cry , then use r(M1-O) cry Perform subsequent processing.
[0033] The present invention does not specifically limit the method for obtaining the average metal-oxygen bond length and the average phosphorus-oxygen bond length, and a method well known to those skilled in the art can be used. In the embodiment of the present invention, the cif file of the metaphosphate crystal is imported into the diomand software to obtain its crystal structure diagram, and then the MO average bond length (r(MO)) is calculated based on the configuration of the MO polyhedron and the PO polyhedron in the metaphosphate crystal structure diagram. cry ) and the average PO bond length (r(PO) cry ); when the metaphosphate crystal contains two metals and the average bond lengths of the chemical bonds between the two metals and oxygen are different, the average bond length of the chemical bond between the metal with the larger value and oxygen is used.
[0034] The present invention provides a fitting equation, wherein the fitting equation is obtained by fitting the strength factor of a known metaphosphate glass to the ratio of the metal-oxygen average bond length and the phosphorus-oxygen average bond length, and the known metaphosphate glass has the same chemical composition as the metaphosphate crystal. In the present invention, the fitting is preferably an exponential growth fitting; the fitting equation is preferably as shown in Formula I:
[0035] m=a0×exp(r cry / b0)+c0 Formula I;
[0036] In formula I, m is the strength factor, r cry is the ratio of the average metal-oxygen bond length to the average phosphorus-oxygen bond length (i.e., r cry = r(MO) cry / r(PO) cry ), a0, b0 and c0 are coefficients.
[0037] In the present invention, a0 is preferably 4.644±0.764; b0 is preferably 0.694±0.013; and c0 is preferably -0.145±0.652.
[0038] After obtaining the fitting equation, the present invention obtains the strength factor of the metaphosphate glass to be tested according to the metal-oxygen average bond length, the phosphorus-oxygen average bond length of the metaphosphate crystals corresponding to the metaphosphate glass to be tested and the fitting equation. In the present invention, the metaphosphate crystals corresponding to the metaphosphate glass to be tested are metaphosphate crystals with the same chemical composition as the metaphosphate glass to be tested. In the present invention, the metaphosphate glass to be tested preferably includes monometallic metaphosphate glass or bimetallic metaphosphate glass (the two metals in the bimetallic metaphosphate glass are respectively recorded as the first metal and the second metal). In the present invention, the metal elements in the metaphosphate glass preferably include one or two of alkali metal elements, alkaline earth metal elements and transition metal elements; the alkali metal elements preferably include K, Na or Rb; the alkaline earth metal elements preferably include Ca, Sr or Ba; the transition metal elements preferably include Zn or Ag. In the present invention, the chemical formula of the monometallic metaphosphate glass preferably includes Zn(PO3)2, NaPO3, Ca(PO3)2, Sr(PO3)2, Ba(PO3)2 or AgPO3; the chemical formula of the bimetallic metaphosphate glass preferably includes NaZn(PO3)3, KZn(PO3)3, RbZn(PO3)3 or Ba2Zn3(PO3) 10 In the present invention, when the metaphosphate glass to be tested is a bimetallic metaphosphate glass and the average bond length of the chemical bond between the first metal and oxygen in the metaphosphate crystals corresponding to the bimetallic metaphosphate glass is greater than the average bond length of the chemical bond between the second metal and oxygen, the metal-oxygen average bond length is the average bond length of the chemical bond between the first metal and oxygen.
[0039] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] The m value of metaphosphate glass (chemical formula: Zn(PO3)2) is obtained by the method of the present invention, and the specific steps are as follows:
[0042] The cif file of Zn(PO3)2 crystal was imported into diomand software to obtain its crystal structure diagram. Then, according to the configuration of Zn-O polyhedron and PO polyhedron in the Zn(PO3)2 crystal structure diagram, the average bond length of Zn-O (r(Zn-O)) was calculated. cry ) and the average PO bond length (r(PO) cry ); Figure 1Figure 1 is a configuration diagram of the Zn-O polyhedron and PO polyhedron in the Zn(PO3)2 crystal, where a is a configuration diagram of the PO polyhedron (specifically, the PO4 tetrahedron), O1, O2, and O3 are oxygen atoms at different environmental sites, indicating the PO bond lengths of oxygen atoms at different environmental sites; b is a configuration diagram of the Zn-O polyhedron (specifically, the ZnO6 octahedron), O2 and O3 are oxygen atoms at different environmental sites, indicating the Zn-O bond lengths of oxygen atoms at different environmental sites. Figure 1 It can be seen that there are four types of PO bond lengths in PO4 tetrahedron. By calculating their average values, we can get the average PO bond length in Zn(PO3)2 crystal as Similarly, the average bond length of Zn-O in Zn(PO3)2 crystal is On this basis, the ratio of the average bond length of Zn-O to the average bond length of PO (r cry ) is 1.36;
[0043] The m value of Zn(PO3)2 glass is obtained according to the fitting equation shown in formula I:
[0044] m=a0×exp(r cry / b0)+c0 Formula I;
[0045] In formula I, m is the strength factor, r cry =1.36, a0=4.644±0.764, b0=0.694±0.013, c0=-0.145±0.652;
[0046] The results show that the m value of Zn(PO3)2 glass obtained by the above method of the present invention is 27-36, including the reference ( -Senovilla, L.; F., Behaviour of viscosity in metaphosphate glasses. J. Non-Cryst. Solids 2014, 385, 9-16) uses the VIF equation to fit the viscosity versus temperature data to obtain an m value (m=28), indicating that the method of the present invention has high accuracy.
[0047] Example 2
[0048] The m value of metaphosphate (chemical formula: Ca(PO3)2) glass is obtained by the method of the present invention. Specifically, the ratio of the average bond length of Ca-O to the average bond length of PO (r cry ) is 1.76, and then according to the fitting equation shown in formula I, the m value of Ca(PO3)2 glass is 48 to 64. -Senovilla, L.; F., Behaviour of viscosity in metaphosphate glasses. J. Non-Cryst. Solids 2014, 385, 9-16) reported that the m value of Ca(PO3)2 glass is 48.
[0049] Example 3
[0050] The m value of the metaphosphate (chemical formula: Sr(PO3)2) glass is obtained by the method of the present invention. Specifically, the ratio of the average bond length of Sr-O to the average bond length of PO (r cry ) is 1.76, and then the m value of Sr(PO3)2 glass is obtained to be 46-63 according to the fitting equation shown in formula I. -Senovilla, L.; F., Behaviour of viscosity in metaphosphate glasses. J. Non-Cryst. Solids 2014, 385, 9-16) reported that the m value of Sr(PO3)2 glass is 46.
[0051] Example 4
[0052] The m value of metaphosphate (chemical formula: NaZn(PO3)3) glass is obtained by the method of the present invention. Specifically, referring to the method in Example 1, based on the crystal structure of NaZn(PO3)3, the average bond length of Na-O is 2.49, and the average bond length of Zn-O is 2.07. The average bond length of the chemical bond between metal and oxygen with a larger value (i.e., 2.49) is used, and on this basis, the ratio of the average bond length to the average bond length of PO is further obtained (r cry ) is 1.62, and then according to the fitting equation shown in Formula I, the m value of NaZn(PO3)3 glass is obtained to be 40-52. The literature (Xia, Y.; Chen, H.; Aitken, B.; Sen, S., Rheological characterization of complex dynamics in Na-Zn metaphosphate glass-forming liquids. J. Chem. Phys. 2021, 155(5), 054503.) reports that the m value of NaZn(PO3)3 glass is 50.
[0053] Example 5
[0054] The method of the present invention is used to obtain metaphosphate (chemical formula is Ba2Zn3(PO3) 10) glass m value, specifically referring to the method in Example 1 based on Ba2Zn3(PO3) 10 The average bond length of Ba-O and Zn-O is 2.89 and 2.11 respectively. The average bond length of chemical bonds between metals and oxygen with a larger value (i.e., 2.89) is used to further obtain the ratio of the average bond length of PO to the average bond length of PO (r cry ) is 1.90, and then according to the fitting equation shown in formula I, the m value of NaZn(PO3)3 glass is 59-77. The literature (Striepe, S. and Deubener, J..Viscosity and kinetic fragilityofalkaline earth zinc phosphate glasses. J.Non-Cryst.Solids.2012,358(12-13),1480-1485.) reported that Ba2Zn3(PO3) 10 The m value of glass is 64.
[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for obtaining the strength factor of metaphosphate glass, characterized in that: The following steps are involved: Providing a metal-oxygen average bond length and a phosphorus-oxygen average bond length, wherein the metal-oxygen average bond length is the average bond length of the chemical bond between metal and oxygen in the metaphosphate crystal, and the phosphorus-oxygen average bond length is the average bond length of the chemical bond between phosphorus and oxygen in the metaphosphate crystal; Providing a fitting equation, wherein the fitting equation is obtained by fitting the strength factor of a known metaphosphate glass to the ratio of the metal-oxygen average bond length and the phosphorus-oxygen average bond length, and the known metaphosphate glass has the same chemical composition as the metaphosphate crystal; According to the metal-oxygen average bond length and the phosphorus-oxygen average bond length of the metaphosphate crystal corresponding to the metaphosphate glass to be tested and the fitting equation, the strength factor of the metaphosphate glass to be tested is obtained.
2. The method according to claim 1, characterized in that The fit was an exponential growth type fit.
3. The method according to claim 2, characterized in that The fitting equation is shown in Formula I: m=a0×exp(r cry / b0)+c0 Formula I; In formula I, m is the strength factor, r cry is the ratio of the average metal-oxygen bond length to the average phosphorus-oxygen bond length, and a0, b0 and c0 are coefficients.
4. The method according to claim 3, characterized in that The a0=4.644±0.764, b0=0.694±0.013, c0=-0.145±0.
652.
5. The method according to any one of claims 1 to 4, characterized in that: The metaphosphate glass to be tested includes single metal metaphosphate glass or double metal metaphosphate glass.
6. The method according to claim 5, characterized in that The two metals in the bimetallic metaphosphate glass are respectively recorded as the first metal and the second metal. When the metaphosphate glass to be tested is a bimetallic metaphosphate glass and the average bond length of the chemical bond between the first metal and oxygen in the metaphosphate crystal corresponding to the bimetallic metaphosphate glass is greater than the average bond length of the chemical bond between the second metal and oxygen, the metal-oxygen average bond length is the average bond length of the chemical bond between the first metal and oxygen.
7. The method according to claim 5, characterized in that The metal elements in the metaphosphate glass to be tested include one or two of alkali metal elements, alkaline earth metal elements and transition metal elements.
8. The method according to claim 7, characterized in that The alkali metal element includes K, Na or Rb; the alkaline earth metal element includes Ca, Sr or Ba; and the transition metal element includes Zn or Ag.
9. The method according to claim 7 or 8, characterized in that: The chemical formula of the single metal metaphosphate glass includes Zn(PO3)2, NaPO3, Ca(PO3)2, Sr(PO3)2, Ba(PO3)2 or AgPO3.
10. The method according to claim 7 or 8, characterized in that: The chemical formula of the bimetallic metaphosphate glass includes NaZn(PO3)3, KZn(PO3)3, RbZn(PO3)3 or Ba2Zn3(PO3) 10 .