Structural member

By adjusting the void ratio in the cross section of the protective film, the problem of aging of the protective film due to differential thermal expansion after the plasma resistance is improved is solved, and a more durable structural component in the plasma etching device is realized.

CN118737792APending Publication Date: 2024-10-01TOTO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410015398.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-01-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In a plasma etching apparatus, when the plasma resistance is sufficiently improved, the protective film is prone to aging due to difference in thermal expansion.

Method used

By adjusting the void ratio on the cross section of the protective film so that the void ratio is smaller on the surface side and larger on the base material side, the stress is reduced when the temperature changes and the aging of the protective film is suppressed.

Benefits of technology

It ensures plasma resistance, while reducing the aging of the protective film accompanied by differential thermal expansion, extending the service life of structural components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737792A_ABST
    Figure CN118737792A_ABST
Patent Text Reader

Abstract

Provided is a structural member capable of suppressing aging of a protective film associated with a difference in thermal expansion. A structural member (10) is provided with: a base material (100); and a protective film (200) that covers the surface (110) of the substrate (100). In a cross-section when the protective film (200) is cut perpendicular to the surface (110), when the ratio of voids per unit area is defined as the void ratio, the void ratio in a first portion (201), which is a part of the cross-section, is smaller than the void ratio in a second portion (202), which is a portion of the cross-section closer to the base material (100) than the first portion (201).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a structural member. Background Art

[0002] A structural member having a protective film on the surface of a substrate is used in various fields such as semiconductor manufacturing devices. For example, in a plasma etching device, a protective film for protecting the substrate from plasma is formed on the surface of the substrate constituting the inner wall of the cavity. As such a protective film, for example, oxide ceramics such as yttrium oxide or fluoride ceramics such as yttrium fluoride are used. As described in the following patent document 1, the protective film is formed by various methods such as physical vapor deposition (PVD), chemical vapor deposition (CVD) and aerosol deposition.

[0003] Patent Literature Patent Document 1: International Publication No. 2021 / 102075 Summary of the invention

[0004] In the process of forming a protective film on the surface of a substrate, bubbles may be contained in the protective film. In order to fully exert the functions of the protective film such as plasma resistance, it is desirable that there are no bubbles in the protective film. Therefore, when forming a protective film, the film forming conditions are usually set so that the bubbles in the protective film are as small or as few as possible.

[0005] On the other hand, according to experiments conducted by the present inventors, it was found that if the entire protective film is formed too densely (that is, without any bubbles), the plasma resistance is sufficiently improved, but a new problem of degradation of the protective film due to thermal expansion differences when the temperature changes is likely to occur.

[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a structural member which can ensure plasma resistance and suppress deterioration of a protective film due to a difference in thermal expansion.

[0007] In order to solve the above-mentioned problem, the structural member of the present invention comprises: a substrate; and a protective film covering the surface of the substrate. With respect to a cross section when the protective film is cut perpendicularly to the surface, when the proportion of voids per unit area is taken as the void ratio, in the structural member, the void ratio in a first portion, which is a part of the cross section, is smaller than the void ratio in a second portion, which is a part of the cross section closer to the substrate side than the first portion.

[0008] In such a structural member, the porosity of the protective film is not uniform throughout the entire film, but varies according to the position in the thickness direction. Specifically, the porosity of the first portion located on the surface side is smaller than the porosity of the second portion located on the substrate side.

[0009] In such a configuration, the porosity is relatively small in the portion of the surface side of the protective film exposed to plasma, so that, for example, the same level of plasma resistance as in the past can be ensured. The "plasma resistance" mentioned here refers to, for example, the ability to suppress the generation of particles accompanying aging of the protective film to a small amount after the protective film is exposed to plasma under predetermined conditions.

[0010] The part on the substrate side of the protective film has a relatively large porosity, so the elastic modulus is smaller than other parts. In other words, it is easy to absorb deformation. Therefore, when the temperature of the structural member changes, if a thermal expansion difference occurs between the substrate and the protective film, although the part on the substrate side of the protective film deforms along with the substrate, the stress generated in this part is also relatively small. As a result, the aging of the protective film accompanied by the thermal expansion difference can be suppressed more than before.

[0011] According to the present invention, it is possible to provide a structural member capable of suppressing deterioration of a protective film due to a difference in thermal expansion while ensuring plasma resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a diagram schematically showing a cross section of a structural member according to the present embodiment. Figure 2 This is an image obtained by observing a cross section of the structural member according to the present embodiment using a scanning electron microscope. Figure 3 It is a diagram schematically showing a cross section of a structural member according to the present embodiment. Figure 4 It is a diagram schematically showing a cross section of a structural member according to the present embodiment. Figure 5 It is a diagram schematically showing a cross section of a structural member according to a modification of the present embodiment. Figure 6 It is a diagram schematically showing a cross section of a structural member according to a modification of the present embodiment. Explanation of symbols 10-structural member; 100-substrate; 110-surface; 200-protective film; 201-part 1; 202-part 2; P-void. DETAILED DESCRIPTION

[0013] Hereinafter, the present embodiment will be described with reference to the drawings. In order to facilitate the description, the same components in the drawings are denoted by the same reference numerals as much as possible, and repeated descriptions are omitted.

[0014] The structural member 10 according to the present embodiment is used as a member constituting the inner wall of a processing chamber in a semiconductor manufacturing device (not shown) such as a plasma etching device. Moreover, the use of such a structural member 10 is ultimately just an example, and although it is not limited to the use in semiconductor manufacturing devices, it is preferred that the structural member 10 be used as a member for an application requiring durability against plasma.

[0015] like Figure 1 As shown, the structural member 10 includes: a substrate 100; and a protective film 200 formed to cover a surface 110 of the substrate 100. In the plasma etching apparatus, the surface 210 of the protective film 200 is exposed to the space in the chamber. The protective film 200 of this embodiment is provided for the purpose of protecting the substrate 100 from plasma. Figure 1 The cross section shown is a cross section when the structural member 10 is cut perpendicularly to the surface 110 .

[0016] The substrate 100 is a member that occupies substantially the entirety of the structural member 10. In the present embodiment, the substrate 100 is formed as a ceramic sintered body containing high-purity aluminum oxide (Al2O3). The substrate 100 may be a ceramic sintered body formed of a material different from the above, or may be a metal depending on the purpose of the structural member 10.

[0017] The protective film 200 is formed to cover the surface 110 of the substrate 100 as described above. In the present embodiment, the protective film 200 is formed as a film containing polycrystalline yttrium oxide (Y2O3). The protective film 200 may also be a ceramic film formed of a material different from the above.

[0018] The protective film 200 of the present embodiment is formed on the surface 110 of the sintered substrate 100 by an aerosol deposition method. As is well known, in the aerosol deposition method, the material of the protective film 200, i.e., tiny particles, are dispersed in a gas to form an "aerosol", and then sprayed onto the surface 110 to generate a collision. On the surface 110, the tiny particles are deformed and broken due to the impact of the collision, so that the tiny particles are combined with each other and accumulated little by little as a protective film 200. Although the surface 210 of the protective film 200 can also be the surface itself at the end of film formation, it can also be a surface that is polished after film formation. The protective film 200 can also be a film formed by a method other than the aerosol deposition method (such as PVD, etc.).

[0019] Figure 1 The portion surrounded by the dotted line DL1 is the portion of the protective film 200. Figure 1 Hereinafter, this portion is also referred to as "first portion 201". The portion surrounded by the dotted line DL2 in the same figure is the portion of the protective film 200. Figure 1 The part of the cross section shown is a part closer to the substrate 100 side than the first part 201. Hereinafter, this part is also expressed as "second part 202".

[0020] Although the first part 201 is a portion near the surface 210 in the protective film 200, it may also be a portion including the surface 210. In addition, although the second part 202 is a portion near the surface on the substrate 100 side (the interface with the substrate 100) in the protective film 200, it may also be a portion including the surface. And, such a definition of the first part 201 and the second part 202 is ultimately just an example. As long as the first part 201 is a portion of the protective film 200 that is closer to the surface 210 side than the second part 202, it may also be a portion other than the above-mentioned position. Similarly, as long as the second part 202 is a portion of the protective film 200 that is closer to the substrate 100 side than the first part 201, it may also be a portion other than the above-mentioned position.

[0021] Figure 2 , an example of an image obtained by observing a cross section of the protective film 200 using a scanning electron microscope is shown. Figure 2 (A) shows an image of the first portion 201. Figure 2 (B) shows an image of the second portion 202. The images have the same magnification and area.

[0022] like Figure 2 As shown in FIG. 1 , a plurality of voids P included in the protective film 200 appear in each cross section. The voids P are formed inside the protective film 200 during the process of forming the protective film 200 , for example.

[0023] As in Figure 2 (A) Figure 2 As is clear from the comparison of (B), the shape and distribution of each void P are not uniform in the entire cross section of the protective film 200, but vary depending on the position. Figure 2 The respective gaps P of the first part 201 of (A) are smaller than those contained in Figure 2 (B) Respective gaps P of the second portion 202.

[0024] Here, regarding the cross section of the protective film 200 when it is cut perpendicularly to the surface 110, the proportion of voids in the unit area is defined as "void ratio". The void ratio is an indicator calculated separately for each part of the cross section of the protective film 200 including the first part 201 or the second part 202. As long as the above-mentioned "unit area" is an area that can include a plurality of voids P, it can be set arbitrarily. For example, Figure 2The same area of ​​the first portion 201 or the second portion 202 shown is set as the above-mentioned "unit area".

[0025] In the present embodiment, the shape and distribution of the voids P in the cross section of the protective film 200 are adjusted so that the void ratio in the first portion 201 is smaller than the void ratio in the second portion 202 .

[0026] Figure 3 In FIG. 1 , as a cross-sectional view schematically showing the shape and distribution of the voids P, the corresponding Figure 2 A cross section of each image. Figure 3 (A) schematically shows the shape and distribution of the voids P in the first portion 201, Figure 3 (B) Schematically shows the shape and distribution of the voids P in the second portion 202 .

[0027] exist Figure 3 In the example, the number of voids P per unit area in the first portion 201 and the number of voids P per unit area in the second portion 202 are substantially equal to each other. On the other hand, the average value of the cross-sectional area per unit of each void P included in the first portion 201 is smaller than the average value of the cross-sectional area per unit of each void P included in the second portion 202. As such, in the present embodiment, as a result of the difference in the cross-sectional area per unit of the voids P, the porosity in the first portion 201 is smaller than the porosity in the second portion 202.

[0028] The reason for such a configuration is explained. In the protective film 200, in the portion on the surface 210 side including the first portion 201, that is, the portion on the surface 210 side exposed to the plasma, a dense film with a small porosity is formed. Therefore, the surface 210 is unlikely to age when exposed to the plasma, and particles from the surface 210 are unlikely to fall off (also referred to as particle generation). In other words, in at least the portion on the surface 210 of the protective film 200, at least the same level of high plasma resistance as in the past is ensured, and aging of the protective film 200 accompanied by particle shedding is unlikely to occur.

[0029] Protective film 200 preferably has a smaller porosity from the viewpoint of ensuring plasma resistance of protective film 200. Therefore, it is also considered that the porosity of the entire cross section of protective film 200 including not only first portion 201 but also second portion 202 is preferably as small as possible.

[0030] However, according to the experiments conducted by the inventors, it was found that if the entire protective film 200 is formed too densely (that is, without any bubbles), while the plasma resistance is sufficiently improved, a new problem of aging of the protective film 200 due to the difference in thermal expansion when the temperature changes is likely to occur. The "difference in thermal expansion when the temperature changes" is the difference in thermal expansion between the base material 100 and the protective film 200 when the temperature of the entire structural member 10 changes.

[0031] Therefore, in the present embodiment, as a countermeasure, the distribution and size of the voids P in each portion of the protective film 200 are adjusted so that the void ratio in the first portion 201 is smaller than the void ratio in the second portion 202 .

[0032] In the structure of this embodiment, the porosity in the part on the substrate 100 side of the protective film 200 is relatively large, so the elastic modulus is smaller than other parts. In other words, deformation is easily absorbed. Therefore, when the temperature of the structural member 10 changes, if a thermal expansion difference occurs between the substrate 100 and the protective film 200, although the part on the substrate 100 side of the protective film 200 deforms along with the substrate 100, the stress generated in this part is suppressed to be small. As a result, the aging of the protective film 200 accompanied by the thermal expansion difference can be suppressed more than before. That is to say, in the structural member 10 involved in this embodiment, at least the same degree of plasma resistance as before is ensured, and at the same time, the aging of the protective film 200 accompanied by the thermal expansion difference can be suppressed.

[0033] Figure 4 , the distribution of the voids P in the entire range from the surface 210 to the surface 110 of the protective film 200 is schematically depicted. Figure 4 After all, this is only a schematic diagram, and therefore the size of the gap P with respect to the thickness of the protective film 200 may differ from the actual one.

[0034] like Figure 4 As shown, in the protective film 200 of the present embodiment, the cross-sectional area of ​​one unit of the void P gradually decreases as it moves away from the substrate 100 over the entire span from the surface 210 to the surface 110. As a result, the value of the porosity in each portion of the protective film 200 also gradually (that is, continuously) decreases as it moves away from the substrate 100, and as a result, the porosity in each of the first portion 201 and the second portion 202 is different from each other.

[0035] Corresponding to the depth direction perpendicular to the surface 110 ( Figure 3 Depending on the position of the protective film 200 in the up-down direction, the value of the porosity in each portion of the protective film 200 may change continuously as in the present embodiment, or may change in stages.

[0036] Furthermore, it is also possible to use a method different from that of the present embodiment ( Figure 3 and Figure 4 ) form, adjusting the porosity in each of the first part 201 and the second part 202. For example, Figure 5 In the configuration of the modified example shown, the average value of the cross-sectional area per unit of each void P included in the first portion 201 and the average value of the cross-sectional area per unit of each void P included in the second portion 202 are substantially the same. On the other hand, the number of voids P per unit area in the first portion 201 is smaller than the number of voids P per unit area in the second portion 202. As in this modified example, the porosity in each of the first portion 201 and the second portion 202 can be adjusted by the arrangement density of the voids P, rather than by the cross-sectional area per unit of each void P.

[0037] Figure 6 In, with Figure 4 Similarly, the Figure 5 The distribution of the voids P in the protective film 200 according to the modified example. Figure 6 As shown, in the protective film 200 of this modified example, the number of voids P per unit area gradually decreases as the distance from the substrate 100 increases over the entire span from the surface 210 to the surface 110. As a result, the value of the void ratio in each portion of the protective film 200 gradually (that is, continuously) decreases as the distance from the substrate 100 increases, and as a result, the void ratios in the first portion 201 and the second portion 202 are different from each other.

[0038] The protective film 200 whose porosity value is adjusted as described above can be formed by stacking a plurality of types of films having different chemical compositions. However, at this time, defects due to, for example, thermal expansion differences may occur at the boundaries of the different types of films. Therefore, as in the present embodiment, it is preferred that the chemical combination of the materials in the entire protective film 200 is the same. In other words, the chemical combination of the protective film 200 in the first part 201 and the chemical combination of the protective film 200 in the second part 202 are preferably the same. The "same" chemical combination means that the ratio of the elements constituting the protective film 200 is the same in each part. Although the "elements constituting the protective film 200" may also include elements mixed into the protective film 200 as impurities, the identity of the "chemical combination" may also be evaluated on the basis of excluding the element.

[0039] In the protective film 200 of the present embodiment, the crystallite size is also substantially uniform throughout the entire film. When the protective film 200 is cut perpendicularly to the surface 110 , the “crystalline size” is the average value of the diameters of a plurality of crystallites appearing in the cross section.

[0040] For example, a transmission electron microscope (TEM) image is taken at a magnification of 400,000 times or more, and the crystallite size can be calculated based on the average value of the diameter of 15 crystallites that are approximately circular. At this time, if the sample thickness during focused ion beam (FIB) processing is made sufficiently thin to about 30nm, the crystallites can be more clearly identified. The shooting magnification can be appropriately selected within a range of 400,000 times or more.

[0041] In the protective film 200 of the present embodiment, the crystallite size measured by the above method is substantially uniform throughout the protective film 200, specifically, 50 nm or less. That is, the crystallite size of the protective film 200 in the first portion 201 and the crystallite size of the protective film 200 in the second portion 202 are both 50 nm or less. By making the crystallite size of the protective film 200 substantially uniform throughout the protective film 200, the durability of the protective film 200 can be improved.

[0042] As a method of adjusting the porosity of each portion of the protective film 200 , various methods can be adopted.

[0043] For example, when the protective film 200 is formed by the aerosol deposition method, the porosity of each part can be adjusted by changing the film forming conditions each time. For those skilled in the art who form films by the aerosol deposition method, the film forming conditions for suppressing the formation of bubbles have been accumulated as experience. In other words, film forming conditions such as increasing the cross-sectional area of ​​the bubbles or increasing the density of the bubbles have also been accumulated as experience. Therefore, by flexibly applying this knowledge to form a film, it is possible to easily form a film having the following characteristics: Figure 4 or Figure 6 An example of the porosity distribution of the protective film 200 is shown.

[0044] When the protective film 200 is formed, for example, a porous raw material may be used to form a film on the substrate 100 side in the middle of the film formation to adjust the porosity.

[0045] When forming the protective film 200, for example, a raw material containing a pore-forming material may be used to form a film on the substrate 100 side before the film is formed, thereby adjusting the porosity. As the pore-forming material, for example, a material that disappears when heated, such as resin particles, may be used. If the entire structural member 10 is heated after the film formation is completed, the protective film 200 with adjusted porosity can be obtained.

[0046] When forming the protective film 200, for example, a material mixed with a material having a different thermal expansion coefficient from the main material may be used to form a film on the substrate 100 side before film formation. After film formation, the entire structural member 10 is heated to generate voids at the interface between the different raw materials, thereby obtaining a protective film 200 with adjusted porosity.

[0047] After forming the protective film 200 by the same method as in the related art, the entire structural member 10 may be heated. If heating is performed under predetermined conditions, grain growth occurs in the protective film 200, and thus local voids may be formed in the process.

[0048] Above, the present embodiment has been described with reference to the specific examples. However, the present invention is not limited to the specific examples. With regard to these specific examples, as long as they have the characteristics of the present invention, the technology that is appropriately designed and changed by those skilled in the art is also included in the scope of the present invention. The various elements and their configurations, conditions, shapes, etc. possessed by the aforementioned specific examples are not limited to the illustrated contents, but can be appropriately changed. As long as there is no technical contradiction, the various elements possessed by the aforementioned specific examples can be appropriately changed and combined.

Claims

1. A structural member, characterized in that: With: base material; and a protective film covering the surface of the substrate, When the cross section of the protective film is cut perpendicularly to the surface, the ratio of voids per unit area is taken as the void ratio. The porosity in a portion of the cross section, i.e., portion 1, The porosity is smaller than the porosity in the second portion which is a portion closer to the substrate than the first portion in the cross section.

2. The structural member according to claim 1, Its characteristics are: an average value of the cross-sectional area of ​​one unit of the void contained in the first portion, Smaller than an average value of the cross-sectional area of ​​one unit of the void included in the second portion.

3. The structural member according to claim 1, Its characteristics are: the number of voids per unit area in the first part, Less than the number of said voids per unit area in said second portion.

4. The structural member according to claim 1, Its characteristics are: In the cross section, the porosity gradually decreases as the distance from the substrate increases.

5. The structural member according to claim 1, Its characteristics are: The chemical composition of the protective film in Part 1, The chemical composition of the protective film in the second part is the same as each other.

6. The structural member according to claim 1, Its characteristics are: The crystallite size of the protective film in the first part, The crystallite size of the protective film in the second part is 50 nm or less.

7. The structural member according to claim 1, Its characteristics are: The protective film is a film formed by an aerosol deposition method.