Doped polycrystalline silicon layer, doping process thereof, solar cell and preparation method of solar cell

By using a gradient concentration doping process of an amorphous silicon layer with a thickness of less than 150nm in solar cells, the doping ion concentration is controlled to decrease, which solves the problem of doping ion concentration and depth control in the doped polysilicon layer and improves the conversion of solar cells. efficiency and passivating contact effects.

CN118738201APending Publication Date: 2024-10-01HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310337546.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to effectively improve the passivation contact effect, hidden open circuit voltage, filling factor and short-circuit current performance of solar cells with existing technology. In particular, it is difficult to control the doping ion concentration and depth in the doped polysilicon layer, resulting in low conversion efficiency.

Method used

A gradient concentration doping process of an amorphous silicon layer with a thickness less than 150nm is used. Through the synergy of specific temperature, large nitrogen flow, oxygen flow and small nitrogen flow carrying the doping source, the concentration of doping ions is controlled from the surface of the tunnel oxide layer. The relative surface decreases to form a doping concentration gradient, which improves the selectivity through function and passivation effect.

Benefits of technology

It significantly improves the conversion efficiency of solar cells, improves the hidden open circuit voltage, filling factor and short-circuit current performance, avoids the generation of pinhole structures in the tunnel oxide layer, and improves the effect of passivating contact structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004156938350000141
    Figure BDA0004156938350000141
Patent Text Reader

Abstract

The invention relates to a doped polycrystalline silicon layer, a doping process thereof, a solar cell and a preparation method of the solar cell. The doping process comprises the steps of boat entering, vacuumizing and heating, diffusion and junction pushing and cooling and boat exiting, and boat entering comprises the step that an amorphous silicon layer with the thickness smaller than 150 nm is placed in a diffusion device; the diffusion junction pushing comprises the steps of pre-oxidation; at the T1 temperature of 780 DEG C to 800 DEG C, large nitrogen of 400 sccm to 600 sccm, oxygen of 480 sccm to 520 sccm and small nitrogen of 830 sccm to 870 sccm carrying a doping source are introduced for primary deposition; at the temperature T2, large nitrogen with the concentration of 400 sccm to 600 sccm, oxygen with the concentration of 380 sccm to 420 sccm and small nitrogen with the concentration of 900 sccm to 1000 sccm are introduced for secondary deposition, T2 is larger than T1, and T2-T1 is smaller than or equal to 20 DEG C; and after the T2 is heated to 885 DEG C to 900 DEG C at the speed of 3.5 DEG C / min to 5.5 DEG C / min, 900 sccm to 1000 sccm of oxygen is introduced, and the constant temperature is kept. According to the doping process, gradient concentration doping of the amorphous silicon layer with the thickness smaller than 150 nm is achieved, the passivation contact effect can be improved, the performance in the aspects of hidden open-circuit voltage, short-circuit current and the like can be improved, and the conversion efficiency of a solar cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a doped polysilicon layer and a doping process thereof, a solar cell and a preparation method thereof. Background Art

[0002] The excellent tunneling oxide passivation contact effect comes from the anti-blocking layer formed at the contact interface between the doped polysilicon layer and the silicon substrate, which prevents the recombination of minority carriers. Among them, the doped polysilicon layer can achieve selective transmission of carriers, which is beneficial to improving the conversion efficiency of solar cells. When the ion doping concentration in the doped polysilicon layer is too low, it will lead to poor ohmic contact, easy burn-through and increased leakage risk. As the doping ion concentration in the doped polysilicon layer increases, the passivation effect of the polysilicon field is significantly improved, but if the doping concentration is too high, the risk of minority carrier recombination will increase.

[0003] At the same time, the magnitude of the hidden open-circuit voltage is very sensitive to the distribution of dopant ion concentration. If the penetration depth of the dopant source through the oxide layer to reach the silicon substrate is too shallow, the field passivation effect formed by the dopant ions on the silicon substrate surface is weak, and the passivation performance after annealing is also poor. Therefore, it is necessary to provide a doping process for the doped polysilicon layer that can improve the passivation contact effect of solar cells while also improving the hidden open-circuit voltage, fill factor, and short-circuit current performance. Summary of the Invention

[0004] Based on this, it is necessary to provide a doped polysilicon layer and its doping process, a solar cell and its preparation method to address the above problems; the doping process realizes gradient concentration doping of an amorphous silicon layer with a thickness of less than 150nm, which can not only improve the passivation contact effect, but also is beneficial to improve the performance in terms of hidden open circuit voltage, fill factor and short-circuit current, thereby making the solar cell have a higher conversion efficiency.

[0005] A doping process for a doped polysilicon layer in a solar cell comprises the following steps:

[0006] S1, entering the boat: placing an amorphous silicon layer with a thickness of less than 150 nm in a diffusion device;

[0007] S2, vacuuming and heating;

[0008] S3, diffusion push:

[0009] (1) pre-oxidation;

[0010] (2) At temperature T1, a large nitrogen with a flow rate of M1, an oxygen with a flow rate of N1, and a small nitrogen with a doping source with a flow rate of Q1 are introduced for a deposition, wherein T1 is 780°C-800°C, M1 is 400sccm-600sccm, N1 is 480sccm-520sccm, and Q1 is 830sccm-870sccm;

[0011] (3) At temperature T2, a large nitrogen with a flow rate of M2, an oxygen with a flow rate of N2, and a small nitrogen with a doping source with a flow rate of Q2 are introduced for secondary deposition, wherein T2>T1 and T2-T1≤20°C, M2 is 400sccm-600sccm, N2 is 380sccm-420sccm, and Q2 is 900sccm-1000sccm;

[0012] (4) After heating T2 to 885°C-900°C at a heating rate of 3.5°C / min-5.5°C / min, introduce 900 sccm-1000 sccm of oxygen and maintain constant temperature;

[0013] S4, cool down and get out of the boat.

[0014] In one embodiment, the thickness of the amorphous silicon layer is greater than or equal to 120 nm.

[0015] In one embodiment, the secondary deposition temperature T2 is 800°C-810°C.

[0016] In one embodiment, Q2-Q1≤100 sccm.

[0017] In one embodiment, the absolute value of the difference between the sum of M1, N1, and Q1 and the sum of M2, N2, and Q2 is less than or equal to 100 sccm.

[0018] In one embodiment, the doping source is selected from a phosphorus source or a boron source.

[0019] In one embodiment, the deposition time is 1100s-1300s;

[0020] And / or, the secondary deposition time is 450s-580s;

[0021] And / or, the step of introducing 900 sccm-1000 sccm of oxygen and maintaining a constant temperature lasts for 900 s-1420 s.

[0022] A doped polysilicon layer is prepared by the doping process for the doped polysilicon layer as described above, wherein the concentration of doped ions in the doped polysilicon layer decreases from the surface close to the tunnel oxide layer to the opposite surface thereof.

[0023] A method for preparing a solar cell includes the doping process of the doped polysilicon layer as described above.

[0024] A solar cell manufactured by the above-mentioned method for manufacturing a solar cell.

[0025] In the doping process described in the present invention, amorphous silicon with a thickness of less than 150 nm is placed under the synergistic effect of a specific gradient temperature, a large nitrogen flow rate, an oxygen flow rate, a small nitrogen flow rate carrying a doping source, and a slow temperature increase and pushing junction. On the one hand, the diffusion difference of the doping ions in the amorphous silicon layer with a thickness of less than 150 nm can be effectively controlled, so that the concentration of the doping ions decreases from the surface close to the tunneling oxide layer to its opposite surface, forming a certain doping concentration gradient, so that the doped polycrystalline silicon layer has excellent selective pass function and low parasitic absorption loss, while taking into account the passivation and contact performance, and is also beneficial to improving the hidden open circuit voltage, fill factor and short-circuit current of the solar cell, thereby improving the conversion efficiency of the solar cell; on the other hand, it can effectively avoid the generation of pinhole structures (pinholes) in the tunneling oxide layer, which is beneficial to further improve the passivation effect of the tunneling oxide layer passivation contact structure, thereby further improving the conversion efficiency of the solar cell.

[0026] The doping process of the present invention can be applied to the preparation of phosphorus-doped polysilicon layers or boron-doped polysilicon layers in solar cells such as IBC cells and TOPcon cells, so that the prepared solar cells such as IBC cells and TOPcon cells have higher conversion efficiency. DETAILED DESCRIPTION

[0027] To facilitate understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in this specification of the present invention are only for the purpose of describing specific embodiments or examples and are not intended to limit the present invention.

[0029] After long and in-depth research, the applicant discovered that thinning the doped polysilicon layer not only helps improve the selective transmittance of carriers, but also avoids the parasitic absorption problem caused by thicker amorphous silicon layers. However, traditional doping process research mostly focuses on amorphous silicon with a thickness of 150nm or more. However, for amorphous silicon with a thickness of less than 150nm, it is difficult to control the distribution of dopant ions in thin amorphous silicon, which is not conducive to regulating the balance between passivation performance and contact, thereby affecting the passivation effect and reducing the conversion efficiency of solar cells. To this end, the present invention provides a doping process for a doped polysilicon layer in a solar cell, comprising the following steps:

[0030] S1, entering the boat: placing an amorphous silicon layer with a thickness of less than 150 nm in a diffusion device;

[0031] S2, vacuuming and heating;

[0032] S3, diffusion push:

[0033] (1) pre-oxidation;

[0034] (2) At temperature T1, a large nitrogen with a flow rate of M1, an oxygen with a flow rate of N1, and a small nitrogen with a doping source with a flow rate of Q1 are introduced for a deposition, wherein T1 is 780°C-800°C, M1 is 400sccm-600sccm, N1 is 480sccm-520sccm, and Q1 is 830sccm-870sccm;

[0035] (3) At temperature T2, a large nitrogen with a flow rate of M2, an oxygen with a flow rate of N2, and a small nitrogen with a doping source with a flow rate of Q2 are introduced for secondary deposition, wherein T2>T1 and T2-T1≤20°C, M2 is 400sccm-600sccm, N2 is 380sccm-420sccm, and Q2 is 900sccm-1000sccm;

[0036] (4) After heating T2 to 885°C-900°C at a heating rate of 3.5°C / min-5.5°C / min, introduce 900 sccm-1000 sccm of oxygen and maintain constant temperature;

[0037] S4, cool down and get out of the boat.

[0038] Therefore, the present invention can improve the performance of solar cells in terms of hidden open circuit voltage, fill factor and short circuit by matching an amorphous silicon layer with a thickness of less than 150nm with a concentration gradient doping process, and can also enhance the passivation quality and contact effect of the doped polysilicon layer, thereby improving the conversion efficiency of the solar cell.

[0039] The specific operation methods and conditions of step S1 and step S2 can adopt traditional methods and conditions, which are not limited in the present invention and can be set by those skilled in the art according to actual preparation conditions.

[0040] Preferably, the thickness of the amorphous silicon layer is greater than or equal to 120 nm.

[0041] Specifically, the amorphous silicon layer with a thickness less than 150 nm can be prepared by a low pressure chemical vapor deposition (LPCVD) method.

[0042] In one embodiment, preheating is also performed while entering the boat. The preheating temperature is 700° C.-720° C., and 6000 sccm-8000 sccm of nitrogen is introduced to maintain a pressure of 900 mbar-1100 mbar.

[0043] In one embodiment, while evacuating in step S2, nitrogen gas with a flow rate of 1400 sccm-1600 sccm is introduced for 300s-450s, which is more conducive to removing impurity gases in the diffusion device and ensuring that there are no pollutants in the diffusion device.

[0044] In one embodiment, after evacuation and before temperature increase, the pressure of the device is stabilized at 1000 mbar to 1080 mbar for 50 seconds to 70 seconds to confirm the leak rate.

[0045] Preferably, a heating time of 900s-1100s is used to raise the temperature of the diffusion device from a preheating temperature of 700°C-720°C to 770°C-790°C for pre-oxidation in step S3. Pre-oxidation forms an oxide layer on the surface of the amorphous silicon layer, which helps improve the uniformity of dopant ion diffusion and control the doping concentration, effectively avoiding problems such as increased recombination and reduced passivation on the surface of the amorphous silicon layer due to excessive dopant ion concentration.

[0046] Specifically, the pre-oxidation temperature is less than or equal to the primary deposition temperature.

[0047] The pre-oxidation pressure is 100 mbar-130 mbar; and / or, the pre-oxidation oxygen flow rate is 935 sccm-1050 sccm, and the nitrogen flow rate is 400 sccm-600 sccm.

[0048] Then, the amorphous silicon layer with a thickness of less than 150nm is placed under the synergistic effect of a specific gradient temperature, a large nitrogen flow rate, an oxygen flow rate, a small nitrogen flow rate carrying a doping source, and a slow temperature increase and pushing junction. On the one hand, the diffusion difference of the doping ions in the amorphous silicon layer with a thickness of less than 150nm can be effectively controlled, so that the concentration of the doping ions decreases from the surface close to the tunneling oxide layer to its opposite surface, forming a certain doping concentration gradient, so that the doped polycrystalline silicon layer can have excellent selective pass function and low parasitic absorption loss while taking into account passivation and contact performance, and is also beneficial to improving the hidden open circuit voltage, fill factor and short-circuit current of the solar cell, thereby improving the conversion efficiency of the solar cell; on the other hand, it can effectively avoid the generation of pinhole structure (pinhole) in the tunneling oxide layer, which is beneficial to further improve the passivation effect of the tunneling oxide layer passivation contact structure, thereby further improving the conversion efficiency of the solar cell.

[0049] Preferably, the temperature T2 of the secondary deposition is 800° C.-810° C., which is more conducive to the formation of a doping concentration gradient of doped ions, so that the doped polysilicon layer has excellent selective pass function and low parasitic absorption loss.

[0050] More preferably, Q2-Q1≤100 sccm, which is more conducive to further coordinated regulation of the two depositions, can more accurately form a doping concentration gradient, and thus is more conducive to improving the conversion efficiency of solar cells.

[0051] It should be noted that during the two depositions, the concentration of the doping source carried by the small nitrogen is kept constant, and the doping amount of the doping source in the diffusion device per unit time can be controlled by adjusting the inlet flow rate of the small nitrogen.

[0052] Preferably, in the two depositions, the flow rates of large nitrogen, oxygen, and small nitrogen carrying the doping source satisfy the following requirements: the absolute value of the difference between the sum of M1, N1, and Q1 and the sum of M2, N2, and Q2 is less than or equal to 100 sccm. Through the synergistic effect of regulating the flow rates of the gas components during the deposition process, it is more conducive to forming a decreasing gradient in the concentration of the doped ions from the surface close to the tunneling oxide layer to its opposite surface, thereby improving the hidden open circuit voltage, fill factor, and short-circuit current of the solar cell, and improving the conversion efficiency of the solar cell.

[0053] Among them, the flow rate M1 of the bulk nitrogen in the first deposition and the flow rate M2 of the bulk nitrogen in the second deposition can be the same or different. The present invention does not limit this, and those skilled in the art can make their own selection according to actual preparation requirements.

[0054] Preferably, the time for the first deposition is 1100s-1300s; and / or the time for the second deposition is 450s-580s.

[0055] In one embodiment, the pressure of the primary deposition is 100 mbar-130 mbar; and / or the pressure of the secondary deposition is 100 mbar-130 mbar.

[0056] It should be noted that the pressure conditions for the two depositions may be the same or different, and the present invention does not limit this. Those skilled in the art may make their own selections based on actual preparation requirements.

[0057] According to the preparation requirements of PN junctions in different solar cells, the doped polysilicon layer can be an N-type doping region or a P-type doping region, and accordingly, the doping source can be selected from a phosphorus source or a boron source.

[0058] By introducing 900sccm-1000sccm of oxygen, the oxygen can react with the doping source, thereby consuming the doping ions on the surface of the secondary doped polysilicon layer, which is conducive to further controlling the doping concentration and forming a certain doping concentration gradient. It can also avoid problems such as increased recombination and reduced passivation caused by excessive surface doping ion concentration.

[0059] Preferably, the step of introducing 900 sccm-1000 sccm of oxygen and maintaining a constant temperature lasts for 900 s-1420 s.

[0060] In one embodiment, after heating T2 to 885°C-900°C at a heating rate of 3.5°C / min-5.5°C / min, 900 sccm-1000 sccm of oxygen is introduced and the temperature is maintained constant, the pressure is 600 mbar-610 mbar.

[0061] The specific operation method and conditions for cooling and removing the boat in step S4 can adopt conventional methods and conditions, which are not limited in the present invention and can be set by those skilled in the art according to actual preparation conditions.

[0062] In the present invention, the temperature is preferably lowered to 700° C.-720° C. at a cooling rate of 3.5° C. / min-5° C. / min.

[0063] The present invention provides a doped polysilicon layer produced by the doping process for the doped polysilicon layer as described above, wherein the concentration of doped ions in the doped polysilicon layer decreases from the surface close to the tunnel oxide layer to the opposite surface thereof.

[0064] In the doped polysilicon layer, the surface of the doped polysilicon layer near the tunneling oxide layer has a higher dopant ion concentration, which not only improves the tunneling effect but also allows a small amount of dopant ions to pass through the tunneling oxide layer to reach the silicon substrate, thereby facilitating excellent field passivation, increasing the tunneling current, and thus facilitating an increase in the hidden open-circuit voltage. At the same time, the dopant ion concentration in the doped polysilicon layer gradually decreases with increasing distance from the tunneling oxide layer. The surface of the doped polysilicon layer farthest from the tunneling oxide layer has the lowest dopant ion concentration, which helps reduce Auger recombination and improve contact performance.

[0065] Therefore, the doped polysilicon layer of the present invention can not only improve the passivation contact effect, but also help to increase the hidden open circuit voltage, thereby making the solar cell have a higher conversion efficiency.

[0066] The present invention also provides a method for preparing a solar cell, including the doping process for the doped polysilicon layer as described above, and a solar cell manufactured by the method for preparing a solar cell as described above.

[0067] In one embodiment, the solar cell may be an IBC cell, wherein the back structure of the IBC cell includes a tunneling oxide layer, a doped polysilicon layer, a back passivation layer, a first metal electrode, and a second metal electrode stacked in sequence on a silicon substrate, wherein the first metal electrode penetrates the back passivation layer and forms an ohmic contact with the doped polysilicon layer, and the second metal electrode penetrates the back passivation layer, the tunneling oxide layer, the doped polysilicon layer, and forms an ohmic contact with the silicon substrate.

[0068] In another embodiment, the solar cell may be a TOPcon cell, wherein the back structure of the TOPCon solar cell includes a tunneling oxide layer, a doped polysilicon layer, a back passivation layer, and a back metal electrode stacked in sequence on a silicon substrate, wherein the back metal electrode penetrates the back passivation layer and forms an ohmic contact with the doped polysilicon layer.

[0069] Hereinafter, the doped polysilicon layer and its doping process, the solar cell and its preparation method will be further described through the following specific embodiments.

[0070] Blank

[0071] An IBC cell was prepared as a blank sample according to the Baseline production line process. The specific doping process steps for the polysilicon layer are as follows:

[0072] S1, put into boat: after alkali polishing, LPCVD growth is performed to obtain an amorphous silicon layer with a thickness of 150nm, which is loaded into a quartz boat and sent into a diffusion furnace tube. 7000sccm of nitrogen is introduced, the temperature is set to 710℃, and the pressure is maintained at 1060mbar.

[0073] In step S2, the pressure was controlled at 100 mbar, 500 sccm of nitrogen was introduced, vacuum was performed, and the temperature was raised to 830°C. The whole process lasted for 1200 s.

[0074] S3, diffusion push:

[0075] (1) The pressure was kept constant at 100 mbar, 1000 sccm of oxygen and 500 sccm of nitrogen were introduced, and pre-oxidation was performed at 830°C for 400 s.

[0076] (2) Under a pressure of 100 mbar, 1000 sccm of oxygen and 935 sccm of nitrogen carrying a phosphorus source were introduced at 830°C, and a phosphorus diffusion deposition was completed after 1300 seconds.

[0077] (3) The temperature was raised from 830°C to 885°C, 1000 sccm of oxygen and 935 sccm of nitrogen carrying a phosphorus source were introduced, and the secondary phosphorus diffusion deposition was completed after 500 s.

[0078] (4) At 885°C, 1000 sccm of oxygen was introduced and a constant pressure of 600 mbar was maintained. The constant temperature was maintained for 2000 s to complete the diffusion and bonding.

[0079] S4, cooling the temperature from 885°C to 780°C at a cooling rate of 5°C / min, then filling with nitrogen and pressing back out of the boat to obtain a phosphorus-doped polysilicon layer.

[0080] The phosphorus ion doping concentration in the phosphorus-doped polysilicon layer was tested by electrochemical capacitance-voltage (ECV) method. The phosphorus ion doping concentration on the surface of the phosphorus-doped polysilicon layer near the tunnel oxide layer was 1.5E 20 , and the phosphorus ion doping concentration on the surface of the phosphorus-doped polysilicon layer farthest from the tunnel oxide layer is 1.7E 20 , which proves that the doped phosphorus ions are evenly distributed in the phosphorus-doped polysilicon layer produced by this doping process.

[0081] Example 1

[0082] The difference between Example 1 and the blank sample is that the doping process steps of the doped polysilicon layer are as follows:

[0083] S1, put into boat: after alkali polishing, LPCVD growth is performed to obtain an amorphous silicon layer with a thickness of 120nm, which is loaded into a quartz boat and sent into a diffusion furnace tube. 7000sccm of nitrogen is introduced, the temperature is set to 710℃, and the pressure is maintained at 1060mbar.

[0084] In step S2, the pressure was controlled at 100 mbar, 500 sccm of nitrogen was introduced, vacuum was performed, and the temperature was raised to 780°C. The whole process lasted for 1200 s.

[0085] S3, diffusion push:

[0086] (1) The pressure was kept constant at 100 mbar, 1000 sccm of oxygen and 500 sccm of nitrogen were introduced, and pre-oxidation was performed at 780°C for 300 s.

[0087] (2) Under a pressure of 100 mbar, 500 sccm of bulk nitrogen, 500 sccm of oxygen, and 850 sccm of small nitrogen carrying a phosphorus source were introduced at 780°C, and a phosphorus diffusion deposition was completed after 1200 seconds.

[0088] (3) Raise the temperature from 780°C to 800°C, introduce 500 sccm of bulk nitrogen, 400 sccm of oxygen, and 935 sccm of small nitrogen carrying a phosphorus source, and complete the secondary phosphorus diffusion deposition after 500 seconds.

[0089] (4) After heating from 800°C to 900°C at a heating rate of 5°C / min, 1000 sccm of oxygen was introduced and a constant pressure of 600 mbar was maintained. The constant temperature was maintained for 900 s to complete the diffusion and bonding.

[0090] S4, cooling the temperature from 900° C. to 700° C. at a cooling rate of 5° C. / min, then filling with nitrogen and pressing back out of the boat to obtain a phosphorus-doped polysilicon layer.

[0091] The phosphorus ion doping concentration in the phosphorus-doped polysilicon layer was tested by electrochemical capacitance-voltage (ECV) method. The phosphorus ion doping concentration on the surface of the phosphorus-doped polysilicon layer near the tunnel oxide layer was 1.8E 20 -3E 20 , and the phosphorus ion doping concentration on the surface of the phosphorus-doped polysilicon layer farthest from the tunnel oxide layer is 1.3E 19 -2.7E 19 , which proves that the doping process can form a certain doping concentration gradient of phosphorus ions in the phosphorus-doped polysilicon layer.

[0092] Example 2

[0093] The difference between Example 2 and the blank sample is that the doping process steps of the doped polysilicon layer are as follows:

[0094] S1, put into boat: after alkali polishing, LPCVD growth is performed to obtain an amorphous silicon layer with a thickness of 120nm, which is loaded into a quartz boat and sent into a diffusion furnace tube. 7000sccm of nitrogen is introduced, the temperature is set to 710℃, and the pressure is maintained at 1060mbar.

[0095] In step S2, the pressure was controlled at 100 mbar, 500 sccm of nitrogen was introduced, vacuum was performed, and the temperature was raised to 780°C. The whole process lasted for 1200 s.

[0096] S3, diffusion push:

[0097] (1) The pressure was kept constant at 100 mbar, 1000 sccm of oxygen and 500 sccm of nitrogen were introduced, and pre-oxidation was performed at 780°C for 300 s.

[0098] (2) Under a pressure of 100 mbar, 400 sccm of nitrogen, 500 sccm of oxygen, and 830 sccm of nitrogen carrying a phosphorus source were introduced at 780°C, and a phosphorus diffusion deposition was completed after 1000 s.

[0099] (3) Raise the temperature from 780°C to 800°C, introduce 500 sccm of bulk nitrogen, 420 sccm of oxygen, and 900 sccm of small nitrogen carrying a phosphorus source, and complete the secondary phosphorus diffusion deposition after 400 seconds.

[0100] (4) After heating from 800°C to 900°C at a heating rate of 3.5°C / min, 1000 sccm of oxygen was introduced and a constant pressure of 600 mbar was maintained. The constant temperature was maintained for 900 s to complete the diffusion and bonding.

[0101] S4, cooling the temperature from 900° C. to 700° C. at a cooling rate of 5° C. / min, then filling with nitrogen and pressing back out of the boat to obtain a phosphorus-doped polysilicon layer.

[0102] Example 3

[0103] The difference between Example 3 and the blank sample is that the doping process steps of the doped polysilicon layer are as follows:

[0104] S1, put into boat: after alkali polishing, LPCVD growth is performed to obtain an amorphous silicon layer with a thickness of 120nm, which is loaded into a quartz boat and sent into a diffusion furnace tube. 7000sccm of nitrogen is introduced, the temperature is set to 710℃, and the pressure is maintained at 1060mbar.

[0105] In step S2, the pressure was controlled at 100 mbar, 500 sccm of nitrogen was introduced, vacuum was performed, and the temperature was raised to 780°C. The whole process lasted for 1200 s.

[0106] S3, diffusion push:

[0107] (1) The pressure was kept constant at 100 mbar, 1000 sccm of oxygen and 500 sccm of nitrogen were introduced, and pre-oxidation was performed at 780°C for 300 s.

[0108] (2) Under a pressure of 100 mbar, 600 sccm of bulk nitrogen, 500 sccm of oxygen, and 830 sccm of small nitrogen carrying a phosphorus source were introduced at 780°C, and a phosphorus diffusion deposition was completed after 1400 seconds.

[0109] (3) Raise the temperature from 780°C to 800°C, introduce 600 sccm of bulk nitrogen, 410 sccm of oxygen, and 900 sccm of small nitrogen carrying a phosphorus source, and complete the secondary phosphorus diffusion deposition after 600 seconds.

[0110] (4) After heating from 800°C to 885°C at a heating rate of 5.5°C / min, 1000 sccm of oxygen was introduced and a constant pressure of 600 mbar was maintained. The constant temperature was maintained for 1200 s to complete the diffusion and bonding.

[0111] S4, cooling the temperature from 885°C to 700°C at a cooling rate of 5°C / min, then filling with nitrogen and pressing back out of the boat to obtain a phosphorus-doped polysilicon layer.

[0112] Example 4

[0113] The difference between Example 4 and Example 1 is that the temperature of the first phosphorus diffusion deposition is 790°C.

[0114] Example 5

[0115] The difference between Example 5 and Example 1 is that the temperature of the first phosphorus diffusion deposition is 800°C, and the temperature of the second phosphorus diffusion deposition is 810°C.

[0116] Example 6

[0117] The difference between Example 6 and Example 1 is that the thickness of the amorphous silicon layer is 130 nm, and in the first phosphorus diffusion deposition step, the oxygen flow rate is 520 sccm; in the second phosphorus diffusion deposition step, the small nitrogen flow rate carrying the phosphorus source is 950 sccm.

[0118] Example 7

[0119] The difference between Example 7 and Example 1 is that the thickness of the amorphous silicon layer is 145 nm, and in the first phosphorus diffusion deposition step, the small nitrogen flow carrying the phosphorus source is 870 sccm, and the oxygen flow is 480 sccm; in the second phosphorus diffusion deposition step, the small nitrogen flow carrying the phosphorus source is 1000 sccm, and the oxygen flow is 380 sccm.

[0120] Example 8

[0121] The difference between Example 8 and Example 1 is that the thickness of the amorphous silicon layer is 110 nm, 900 sccm of oxygen is introduced, and a constant pressure of 600 mbar is maintained, and the constant temperature is maintained for 1420 s to complete the diffusion and junction.

[0122] Example 9

[0123] The difference between Example 9 and Example 1 is that a boron source is used as a doping source to prepare a boron-doped polysilicon layer.

[0124] Comparative Example 1

[0125] The difference between Comparative Example 1 and Example 1 is that the temperature in the secondary phosphorus diffusion deposition step is 810°C.

[0126] Comparative Example 2

[0127] The difference between Comparative Example 2 and Example 1 is that in the step of one phosphorus diffusion deposition, the small nitrogen flow rate carrying the phosphorus source is 900 sccm.

[0128] Comparative Example 3

[0129] The difference between Comparative Example 3 and Example 1 is that in the step of secondary phosphorus diffusion deposition, the small nitrogen flow rate carrying the phosphorus source is 1100 sccm.

[0130] Comparative Example 4

[0131] The difference between Comparative Example 4 and Example 1 is that in the first phosphorus diffusion deposition step, the oxygen flow rate is 400 sccm; in the second phosphorus diffusion deposition step, the oxygen flow rate is 500 sccm.

[0132] Comparative Example 5

[0133] The difference between Comparative Example 5 and Example 1 is that in the first phosphorus diffusion deposition step, the maximum nitrogen flow rate is 650 sccm; in the second phosphorus diffusion deposition step, the maximum nitrogen flow rate is 700 sccm.

[0134] Comparative Example 6

[0135] The difference between Comparative Example 6 and Example 1 is that the temperature is increased from 800° C. to 920° C. at a heating rate of 10° C. / min.

[0136] Comparative Example 7

[0137] The difference between Comparative Example 7 and Example 1 is that after heating from 800°C to 900°C at a heating rate of 5°C / min, 800 sccm of oxygen is introduced, and a constant pressure of 600 mbar is maintained, and the constant temperature is maintained for 900 seconds to complete the diffusion and bonding.

[0138] IBC battery samples 1-15 were prepared according to the doping process provided in Examples 1-8 and Comparative Examples 1-7, and the blank samples and samples 1-15 were subjected to performance tests. The test results are shown in Table 1.

[0139] Table 1

[0140]

[0141] Table 1 shows that Sample 1 achieves a conversion efficiency (Eta) of 24.03%, approximately 0.08% higher than the blank sample produced using the baseline process. Furthermore, the open-circuit voltage (Voc) increases by approximately 1.9 mV, the short-circuit current (Isc) by approximately 4 mA, and the fill factor (FF) by approximately 0.03. Furthermore, a comparison of Samples 1-8 with Samples 9-15 demonstrates that the proposed doping process can produce highly efficient solar cells.

[0142] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0143] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.

Claims

1. A doping process for doping a polysilicon layer in a solar cell, characterized in that: The doping process comprises the following steps: S1, entering the boat: placing an amorphous silicon layer with a thickness of less than 150 nm in a diffusion device; S2, evacuate and heat up; S3, diffusion push knot: (1) pre-oxidation; (2) At temperature T1, a large nitrogen with a flow rate of M1, an oxygen with a flow rate of N1, and a small nitrogen with a doping source with a flow rate of Q1 are introduced for a deposition, wherein T1 is 780°C-800°C, M1 is 400sccm-600sccm, N1 is 480sccm-520sccm, and Q1 is 830sccm-870sccm; (3) At temperature T2, a large nitrogen with a flow rate of M2, an oxygen with a flow rate of N2, and a small nitrogen with a doping source with a flow rate of Q2 are introduced for secondary deposition, wherein T2>T1 and T2-T1≤20°C, M2 is 400sccm-600sccm, N2 is 380sccm-420sccm, and Q2 is 900sccm-1000sccm; (4) After heating T2 to 885°C-900°C at a heating rate of 3.5°C / min-5.5°C / min, 900sccm-1000sccm of oxygen was introduced and the temperature was maintained constant; S4, cool down and get out of the boat.

2. The doping process of the doped polysilicon layer according to claim 1, characterized in that: The thickness of the amorphous silicon layer is greater than or equal to 120 nm.

3. The doping process of the doped polysilicon layer according to claim 1, characterized in that: The temperature T2 of the secondary deposition is 800°C-810°C.

4. The doping process of the doped polysilicon layer according to claim 1, characterized in that: Q2-Q1≤100sccm.

5. The doping process of the doped polysilicon layer according to claim 1, characterized in that: The absolute value of the difference between the sum of M1, N1, Q1 and the sum of M2, N2, Q2 is less than or equal to 100 sccm.

6. The doping process of the doped polysilicon layer according to claim 1, characterized in that: The doping source is selected from a phosphorus source or a boron source.

7. The doping process of the doped polysilicon layer according to claim 1, characterized in that: The time of one deposition is 1100s-1300s; And / or, the secondary deposition time is 450s-580s; And / or, in the step of introducing 900 sccm-1000 sccm of oxygen and maintaining a constant temperature, the time is 900s-1420s.

8. A doped polysilicon layer obtained by the doping process for doping a polysilicon layer according to any one of claims 1 to 7, characterized in that: The concentration of doped ions in the doped polysilicon layer decreases gradually from the surface close to the tunnel oxide layer to the opposite surface thereof.

9. A method for preparing a solar cell, characterized in that: The method comprises the doping process of the doped polysilicon layer as claimed in any one of claims 1 to 7.

10. A solar cell manufactured by the method for manufacturing a solar cell according to claim 9.