Surface modification method and application of cobalt-free lithium-rich positive electrode material

The crystal structure of the cobalt-free lithium-rich cathode material is controlled through hydrothermal treatment, inducing the generation of oxygen vacancies and spinel phases on the surface, which solves the problem of material structural degradation and oxygen loss, significantly improves the electrochemical performance and cycle stability, and is suitable for industrial applications.

CN118738256APending Publication Date: 2024-10-01ZHEJIANG UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410708693.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Cobalt-free lithium-rich cathode materials suffer from structural degradation, voltage attenuation and irreversible oxygen loss during the charge and discharge process, which affects their specific capacity and life. The existing surface modification methods are complex, energy-consuming and have limited improvement in electrochemical performance.

Method used

The hydrothermal treatment method is used to regulate the crystal structure of cobalt-free lithium-rich cathode materials, inducing the generation of oxygen vacancies and spinel phases on the surface, forming a surface heterogeneous layer, and improving structural stability and electrochemical performance.

Benefits of technology

The structural stability and electrochemical performance of the cobalt-free lithium-rich cathode material are significantly improved through hydrothermal treatment, especially the rate performance and voltage drop suppression, which simplifies the process, reduces the cost, and improves the cycle stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738256A_ABST
    Figure CN118738256A_ABST
Patent Text Reader

Abstract

The invention discloses a surface modification method and application of a cobalt-free lithium-rich positive electrode material. The surface modified lithium-rich positive electrode material comprises a cobalt-free lithium-rich positive electrode bulk phase and a surface heterogeneous layer with oxygen vacancies and spinel phases. The crystal structure of the cobalt-free lithium-rich positive electrode material is regulated and controlled through hydrothermal treatment, so that the structural stability and the cycle performance of the cobalt-free lithium-rich positive electrode material are improved; a heterogeneous passivation layer containing oxygen vacancies and a spinel phase is generated on the surface of the cobalt-free lithium-rich positive electrode material through hydrothermal treatment, so that the cobalt-free lithium-rich positive electrode material is protected, the reversibility of anion redox of the cobalt-free lithium-rich positive electrode material is regulated and controlled, the rate capability is improved, and the reversibility of anion redox is improved; and the voltage drop is suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium-ion battery positive electrode materials and relates to a method for surface modification of cobalt-free lithium-rich positive electrode materials and applications. Background Art

[0002] In today's era, lithium-ion batteries play a vital role as sustainable energy storage systems in various battery products and devices. Importantly, lithium-ion batteries are widely used in electric vehicles due to their high specific energy, low weight and resource sustainability. Due to the low specific capacity and unstable structure of the cathode material, the specific capacity, life and safety of lithium-ion batteries are mainly limited by the cathode material. Among them, cobalt-free lithium-rich cathode materials have high specific capacity (>250mAh g -1 ) and low cost are regarded as potential candidates for the next generation of power battery cathode materials. Anion redox is the reason for the high specific capacity. However, there are still many key issues to be solved in cobalt-free lithium-rich cathode materials, such as low first-cycle coulombic efficiency (ICE), unsatisfactory rate performance, and structural degradation during the cycle. Among them, the main obstacles affecting commercial applications are continuous voltage decay and irreversible oxygen loss, which will continuously reduce the specific capacity and life of the battery throughout the cycle.

[0003] During the charge and discharge process of cobalt-free lithium-rich materials, oxygen ions undergo chemical reactions under high pressure to generate oxygen, which escapes from the oxygen lattice. When lithium ions are embedded, the migration of transition metals will produce cation mixing, which will cause structural degradation, capacity and voltage decay of cobalt-free lithium-rich materials. Common doping and surface coating methods have only very limited inhibitory effects on the structural degradation of cobalt-free lithium-rich cathode materials. The strategy of pre-constructing oxygen vacancies and spinels on the surface of cobalt-free lithium-rich cathode materials has an extremely effective stabilizing effect on the material structure. When lattice oxygen is oxidized to form O2, lattice oxygen will be lost on the surface of the particles to form oxygen vacancies, and the surface will be densified to form a spinel phase. However, inside the particles, oxygen will be trapped and reduced to lattice oxygen during discharge. This surface modification method protects the interior of the material by forming a heterogeneous passivation layer with oxygen vacancies and spinels on the surface of cobalt-free lithium-rich, reducing oxygen escape during the cycle and improving the electrochemical stability of cobalt-free lithium-rich cathode materials.

[0004] At present, the most common methods for inducing the pre-generation of spinel phase and oxygen vacancies on the surface are gas (CO2, NH3, etc.) treatment, organic solvent treatment, molybdate, and nitrate treatment. These methods are not only complex and energy-intensive, but also involve high costs for chemicals and are more likely to cause environmental pollution. In addition, the comprehensive electrochemical performance of the cobalt-free lithium-rich cathode materials modified by these methods is relatively limited.

[0005] Therefore, it is of great significance for commercial applications to develop a surface modification strategy with simple steps, green process, which can effectively regulate the reversibility of anion redox in cobalt-free lithium-rich cathode materials and improve their comprehensive electrochemical performance. Summary of the Invention

[0006] To solve the above problems, the present invention provides a method and application for surface modification of cobalt-free lithium-rich cathode materials. The present invention regulates the crystal structure of cobalt-free lithium-rich cathode materials through hydrothermal treatment to improve the structural stability of cobalt-free lithium-rich cathode materials; through hydrothermal treatment, oxygen vacancies and spinel phases are induced on the surface of cobalt-free lithium-rich cathode materials to regulate the reversibility of anion redox and improve the electrochemical performance of cobalt-free lithium-rich materials.

[0007] The present invention adopts the following technical solutions:

[0008] A method for surface modification of cobalt-free lithium-rich cathode materials, comprising the following steps:

[0009] Put the cobalt-free lithium-rich cathode material into a reaction kettle, add deionized water, stir, and then perform heat treatment. After cooling, washing, and drying, a surface-modified cobalt-free lithium-rich cathode material is obtained; the surface-modified cobalt-free lithium-rich cathode material includes a cobalt-free lithium-rich cathode bulk phase and a surface heterolayer with oxygen vacancies and spinel phases.

[0010] Further, the molecular formula of the cobalt-free lithium-rich cathode material is Li 1+x TM 1-x O2, where 0 < x < 0.35, and TM is one or more of Ni and Mn. The cobalt-free lithium-rich cathode material is preferably a cobalt-free lithium-rich manganese-based cathode material, and the source materials of the cobalt-free lithium-rich manganese-based cathode material are preferably lithium carbonate and nickel cobalt manganese precursors, and the nickel manganese precursor is preferably Mn 0.75 Ni 0.25 CO3 or Mn 0.75 Ni 0.25 (OH)2.

[0011] Further, the ratio of the cobalt-free lithium-rich cathode material to deionized water is 0.5 - 5 g: 30 - 80 mL.

[0012] Further, the stirring time is 2 - 5 hours.

[0013] Further, the heat treatment is carried out at 100 - 220 °C for 1 - 25 hours.

[0014] Further, the cobalt-free lithium-rich cathode material is prepared by a solid-phase sintering method, specifically:

[0015] After the cobalt-free lithium-rich positive electrode material precursor and the lithium source are evenly mixed, the cobalt-free lithium-rich positive electrode material is obtained through high-temperature calcination; the conditions of the high-temperature calcination are: pre-calcining at 350-550°C for 2-7 hours in an air atmosphere, and then sintering at 600-1000°C for 7-15 hours, with a heating rate of 2-8°C / min, and then naturally cooling with the furnace.

[0016] Preferably, the cobalt-free lithium-rich cathode material precursor and the lithium source are mixed evenly by physical grinding, that is, grinding evenly with a mortar.

[0017] Preferably, the cobalt-free lithium-rich positive electrode material precursor is a combination of one or more of hydroxide, oxalate, and carbonate precipitates; the lithium source is a combination of one or more of lithium hydroxide, lithium carbonate, lithium acetate, lithium carbonate, and lithium chloride.

[0018] A surface-modified cobalt-free lithium-rich positive electrode material is prepared by the method.

[0019] An electrode sheet is made from the surface modified cobalt-free lithium-rich positive electrode material.

[0020] A lithium-ion battery is made using the surface-modified cobalt-free lithium-rich positive electrode material.

[0021] The beneficial effects of the present invention are:

[0022] 1. The present invention induces the formation of a surface heterogeneous layer with oxygen vacancies and spinel phase on the surface of the cobalt-free lithium-rich cathode material through hydrothermal treatment, and regulates the composition of the surface heterogeneous layer through the hydrothermal treatment time, wherein the pre-generated oxygen vacancies can effectively inhibit the escape of oxygen during the cycle; the generation of the spinel phase can effectively protect the structure of the cobalt-free lithium-rich cathode material and reduce the generation of side reactions. Thus, the structural stability and electrochemical stability of the cobalt-free lithium-rich cathode material are improved.

[0023] 2. The hydrothermal treatment of the present invention induces the generation of lithium vacancies and oxygen vacancies on the surface of the cobalt-free lithium-rich positive electrode material, thereby regulating the rearrangement of cations to form a spinel phase, effectively regulating the anion redox activity in the cobalt-free lithium-rich positive electrode material, and the formation of the spinel phase also provides a three-dimensional lithium ion transmission channel, increases the lithium ion deintercalation rate, and improves the electrochemical properties of the cobalt-free lithium-rich positive electrode material, especially the improvement of rate performance and the effective suppression of voltage drop. The method of the present invention has simple steps and significant effects. Compared with the existing technology, it shortens the post-processing time and reduces the production cost.

[0024] 3. The invention has a simple strategy, a green and harmless process, low energy consumption, high safety, obvious modification effect, good economic benefit prospects, and is suitable for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 11 is an X-ray diffraction (XRD) pattern of the cobalt-free lithium-rich positive electrode material of the test group in the embodiment of the present invention.

[0026] Figure 2 It is the XRD pattern of the cobalt-free lithium-rich positive electrode material of the control group in the embodiment of the present invention.

[0027] Figure 3 It is a scanning electron microscope (SEM) morphology picture of the cobalt-free lithium-rich positive electrode material of the test group in the embodiment of the present invention.

[0028] Figure 4 This is a scanning electron microscope (SEM) morphology picture of the cobalt-free lithium-rich positive electrode material of the control group in the embodiments of the present invention.

[0029] Figure 5 It is a transmission electron microscope (TEM) high-resolution picture of the cobalt-free lithium-rich positive electrode material of the test group in the embodiment of the present invention.

[0030] Figure 6 It is a transmission electron microscope (TEM) high-resolution picture of the cobalt-free lithium-rich positive electrode material of the control group in the embodiments of the present invention.

[0031] Figure 7 This is the X-ray photoelectron spectrum (XPS) of the cobalt-free lithium-rich manganese-based positive electrode material of the lithium-ion battery of the test group in the embodiment of the present invention.

[0032] Figure 8 This is the X-ray photoelectron spectrum (XPS) of the cobalt-free lithium-rich manganese-based positive electrode material of the lithium-ion battery in the control group of the embodiments of the present invention.

[0033] Fig. 9 It is a comparison chart of the cycle performance of the cobalt-free lithium-rich positive electrode materials of lithium-ion batteries in the test group and the control group in the embodiment of the present invention.

[0034] Fig.10 3 is a comparison diagram of the voltage drop of the lithium-ion battery cobalt-free lithium-rich positive electrode materials of the test group and the control group in the embodiment of the present invention.

[0035] Fig.11 It is a comparison chart of the rate performance of the lithium-ion battery cobalt-free lithium-rich positive electrode material at 0.05C-10C for the test group and the control group in the embodiment of the present invention.

[0036] Fig.12 This is a SEM image of the cobalt-free lithium-rich positive electrode material of the lithium-ion battery in the test group of the embodiment of the present invention after 150 cycles.

[0037] Fig.13 This is a SEM image of the cobalt-free lithium-rich positive electrode material of the lithium-ion battery in the control group of the embodiment of the present invention after 150 cycles. DETAILED DESCRIPTION

[0038] The present invention uses hydrothermal treatment to modify the surface of the prepared cobalt-free lithium-rich positive electrode material. This method is green, environmentally friendly, low-cost, simple in process, low in energy consumption, and has a very ideal modification effect. For example, a cobalt-free lithium-rich positive electrode material is synthesized by a solid-phase sintering method, and then subjected to hydrothermal treatment after natural cooling. The cobalt-free lithium-rich positive electrode material is placed in a reactor, deionized water is added, stirred for 2 to 5 hours, and then moved to a blast oven, heat treated at 100 to 220°C for 1 to 25 hours, and the product is washed and dried after natural cooling. The thickness of the surface heterogeneous layer with oxygen vacancies and spinel phases is adjusted by adjusting the hydrothermal treatment time, hydrothermal treatment temperature, etc. The hydrothermal treatment method induces the directional removal of Li2O by water to generate lithium hydroxide, thereby generating lithium vacancies and oxygen vacancies, and then generates cation rearrangement to form spinel. The generated lithium hydroxide can be directly removed by subsequent cleaning, so that the lithium vacancies and oxygen vacancies are exposed. The equations involved are as follows:

[0039] Li2O+H2O=2LiOH (1)

[0040] Li 1.2 Mn 0.6 Ni 0.2 O2→0.4LiMn 1.5 Ni 0.5 O4(spinel)+0.4Li2O (2)

[0041] The generation of lithium vacancies can be obtained through ICP testing:

[0042]

[0043]

[0044] The nickel and manganese contents did not change significantly, but the lithium content gradually decreased with the increase of treatment time, which shows that the hydrothermal treatment is effective.

[0045] The present invention uses green and harmless hydrothermal treatment to modify the surface of the cobalt-free lithium-rich positive electrode material, and produces a heterogeneous layer with oxygen vacancies and spinel phase on the surface of the cobalt-free lithium-rich positive electrode material, thereby inhibiting the structural degradation and irreversible oxygen loss that occur during the cycle, and improving the structure and cycle stability of the material. The generation of oxygen vacancies will cause the generation of a small amount of trivalent manganese, thereby forming a spinel phase, increasing the energy barrier for manganese ion migration, and improving the structural stability of the cobalt-free lithium-rich material. In addition, the presence of the spinel phase provides a three-dimensional lithium ion transmission channel, accelerates the transmission rate of lithium ions, improves the rate performance, and has an almost negligible voltage drop. In addition, the heterogeneous passivation layer generated on the surface can protect the bulk phase from the influence of side reactions and reduce the lattice strain of the cobalt-free lithium-rich positive electrode material.

[0046] The solid phase sintering method is widely used in the synthesis of cobalt-free lithium-rich cathode materials due to its low cost and simple process. However, the cobalt-free lithium-rich cathode material particles synthesized by this method have some unsatisfactory aspects in terms of diffusion kinetics and cycle stability. Therefore, the present application further utilizes a hydrothermal treatment method to modify the surface thereof, and regulates the crystal structure of the cobalt-free lithium-rich cathode material through hydrothermal treatment to improve the structural stability of the cobalt-free lithium-rich cathode material; and induces the generation of oxygen vacancies and spinel phases on the surface of the cobalt-free lithium-rich cathode material through hydrothermal treatment, regulates the reversibility of anion redox, and improves the electrochemical performance of the cobalt-free lithium-rich material.

[0047] The technical solution of the present invention is further described in detail below with reference to the accompanying drawings and specific examples.

[0048] Example 1

[0049] The cobalt-free lithium-rich cathode material of the lithium-ion battery in this example is a cobalt-free lithium-rich manganese-based material, and its molecular formula is Li 1.2 Mn 0.6 Ni 0.2 O2.

[0050] Li 1.2 Mn 0.6 Ni 0.2 The preparation method of O2 specifically comprises the following steps:

[0051] According to Li 1.2 Mn 0.6 Ni 0.2 O2 stoichiometric ratio, the lithium source and the nickel manganese precursor are mixed, wherein the lithium salt is lithium carbonate and the nickel manganese precursor is Mn 3 / 4 Ni 1 / 4 CO3. Specifically, according to Li2CO3:Mn 3 / 4 Ni 1 / 4 The two substances were ground in a mortar at a ratio of CO3=0.4751 for 30 minutes. After being evenly ground, they were transferred to a quartz boat and then placed in a muffle furnace for calcination in an air atmosphere. The specific calcination conditions were: heating from room temperature to 450°C at a heating rate of 5°C per minute, keeping warm for 5 hours, then heating from 450°C to 850°C at a heating rate of 5°C per minute, keeping warm for 12 hours, and finally cooling to room temperature with the furnace to obtain a cobalt-free lithium-rich positive electrode material.

[0052] Then, the cobalt-free lithium-rich positive electrode material is subjected to hydrothermal treatment. The specific method is as follows: 1 g of cobalt-free lithium-rich positive electrode material is placed in a reactor, 50 mL of deionized water is added, and after stirring for 5 hours, it is moved to a forced air oven and heated at 200°C for 5 hours. After natural cooling, the product is washed and dried to obtain a surface-modified cobalt-free lithium-rich positive electrode material having a surface heterogeneous layer of oxygen vacancies and spinel phases.

[0053] The surface modified cobalt-free lithium-rich cathode material (marked as the experimental group) and the unmodified cobalt-free lithium-rich cathode material (marked as the control group) synthesized by solid phase sintering were subjected to X-ray diffraction (XRD), scanning electron microscopy (SEM), transmission electron microscopy (TEM), X-ray photoelectron spectroscopy (XPS) analysis and electrochemical testing. The experimental group and the control group were subjected to the same detection and testing to compare the effects of hydrothermal treatment on the cobalt-free lithium-rich cathode material. The details are as follows:

[0054] 1. Comparison of structural composition

[0055] The crystal structure of the lithium-ion cobalt-free lithium-rich cathode materials in the experimental group and the control group was characterized by an X-ray diffractometer (XRD, Rigaku Ultima IV), and the following results were obtained: Figure 1 and Figure 2 Results shown.

[0056] By observation Figure 1 and Figure 2 It can be found that both figures have relatively clear diffraction peaks, which indicates that the samples in the experimental group and the control group have good crystallinity; Figure 1 The (400) peak at 44.8° and the (440) peak at 64.6° clearly indicate the generation of the spinel phase belonging to the Fd-3m space group. Figure 2 The remaining diffraction peaks of the two groups of sample powders can correspond one-to-one with the hexagonal layered phase (R-3m space group) LiTMO2 composition and the monoclinic phase (C / 2m space group) Li2MnO3 composition, which fully conforms to the diffraction peak characteristics of cobalt-free lithium-rich cathode materials.

[0057] 2. Particle morphology characterization

[0058] The cobalt-free lithium-rich cathode materials of the test group and the control group were investigated using a scanning electron microscope (SEM, HITACHIRegulus8230), and the SEM images corresponding to a magnification of 6000 times were obtained, as shown in Figure 3 and Figure 4 shown.

[0059] Through SEM observation, it was found that the particles of the two groups of samples were regular spheres, the particle size was in the range of 10-15μm, and there was no obvious difference in appearance, which shows that hydrothermal treatment does not change the macroscopic morphology of the particles.

[0060] 3. Microstructure characterization

[0061] The microscopic lattice structure of the cobalt-free lithium-rich cathode materials of the experimental group and the control group was characterized using a transmission electron microscope (TEM, FEI Talos F200X), and the TEM images corresponding to the 5 nm scale were obtained, such as Figure 5 and Figure 6 shown.

[0062] Through TEM observation, it was found that both groups of samples had a layered phase lattice composition. In particular, in the TEM image of the experimental group, a surface heterogeneous layer appeared in the 2-5nm region on the surface of the particles. This layer contained a spinel phase composition, which was not observed in the control group.

[0063] 4. Characterization of oxygen vacancy defects

[0064] The O1s energy spectrum of the cobalt-free lithium-rich cathode materials in the experimental group and the control group was characterized by X-ray photoelectron spectroscopy (XPS, SHIMADZUAXIS Supra+). The specific results are as follows Figure 6 and Figure 7 shown.

[0065] By observing the O1s of XPS, we found that three peaks can be found in both the experimental group and the control group: the peak at 529.5eV belongs to lattice oxygen, the peak at 531.2eV belongs to LiOH, and the peak at 532.3eV belongs to Li2CO3. In particular, we also found that there is a characteristic peak at 530eV in the O1s energy spectrum of the experimental group, which belongs to oxygen vacancies, which is not observed in the control group. This shows that the experimental group samples after hydrothermal surface modification have generated oxygen vacancies through the induction of water.

[0066] 5. Comparison of electrochemical performance

[0067] The cobalt-free lithium-rich cathode materials of the test group and the control group were assembled into batteries for electrochemical performance testing. Here, the specific assembly process of the test group is introduced as an example. The control group is the same. The specific assembly process is as follows:

[0068] (1) Preparation of positive electrode sheet

[0069] The surface-modified cobalt-free lithium-rich cathode material Li 1.123 Mn 0.588 Ni 0.190 O 2-x(The specific data of the metal molar ratio is obtained from the ICP test data of inductively coupled plasma mass spectrometry. However, due to the charge compensation mechanism, a small amount of trivalent manganese will be generated along with the release of lithium. Therefore, the specific amount of oxygen escape cannot be calculated specifically, so it is represented by X). Conductive carbon black (Super P) and binder polyvinylidene fluoride (PVDF) are added in a mass ratio of 8:1:1, wherein the mass fraction of PVDF is 5%, and the solvent is NMP. After addition, the mixture is placed in a high-speed homogenizer and homogenized at a speed of 2500r / min for 5 minutes. The homogenized slurry is evenly coated on the aluminum foil, and then the aluminum foil is transferred into a forced air drying oven for preliminary drying at 80°C for 2 hours, and then moved into a vacuum oven for drying at 100°C for 12 hours. The active material loading of the electrode is 2-4mg cm -2 The dried electrode is cut into small discs with a diameter of 12 mm using a tablet press for later use.

[0070] (2) Preparation of lithium-ion battery negative electrode

[0071] The negative electrode of the lithium-ion battery uses a lithium sheet with a diameter of 14mm purchased directly from CROOD.

[0072] (3) Button battery assembly

[0073] The button cell was assembled in a glove box under a high-purity argon atmosphere (H2O<0.01ppm, O2<0.01ppm), and the battery shell model was CR2032. The electrolyte used in this embodiment is 1M LiPF6 dissolved in a solvent of ethylene carbonate (EC): dimethyl carbonate (DMC): ethyl methyl carbonate (EMC) = 1:1:1 (volume ratio), and the diaphragm used is a PE diaphragm. The assembly steps are: positive electrode shell, positive electrode sheet, diaphragm, negative electrode (lithium sheet), gasket, shrapnel, negative electrode shell, and the lithium-ion battery is assembled and left to stand for 10 hours for use.

[0074] (4) Battery performance test

[0075] The electrochemical test of lithium-ion batteries uses the Xinwei test system. The spare battery is placed on the battery channel of the Xinwei test system. The voltage test window is 2.0V-4.8V. The cycle performance and rate performance of the lithium-ion battery are compared and tested.

[0076] (5) Cycle performance comparison

[0077] The battery assembled with lithium-rich manganese-based cathode materials in the experimental group and the control group was subjected to charge and discharge cycle performance test at a charge and discharge rate of 1C (1C = 250mAh / g) in the voltage window of 2.0-4.8V. The number of test cycles was 150 cycles, and the long cycle stability comparison was Fig. 9 As shown in the figure, the voltage drop during the cycle is Fig.10shown.

[0078] By observation Fig. 9 We can see that the initial discharge capacity of the test group's battery is 189.43mAh / g. After 150 cycles, the discharge capacity is still 183.94mAh / g, and the capacity retention rate is as high as 97.12%. The initial discharge capacity of the control group is only 180.42mAh / g. After 150 cycles, the discharge capacity decays to only 145.71mAh / g, and the capacity retention rate is only 80.76%. From the above comparison, it can be seen that the cycle stability of the hydrothermal-induced surface-modified material is greatly improved, and the discharge capacity and capacity retention rate are higher than those of the control group without surface modification.

[0079] By observation Fig.10 It can be obtained that after 150 cycles, the average rate of voltage drop in the test group is 0.91 mV per cycle, while the average rate of voltage drop in the control group is 1.85 mV per cycle. From the above comparison, we can see that the average rate of voltage drop in the test group is much smaller than that in the control group. This shows that during the cycle, the sample structure of the hydrothermally induced surface modification test group is better maintained, the anion redox reversibility is better improved, and no serious structural decay and oxygen loss occur.

[0080] (6) Rate performance test

[0081] According to the above voltage window, the test group and the control group were charged and discharged at rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 1C to obtain a comparison of the rate performance of the two groups, as shown in Figure 2. Fig.11 shown.

[0082] By observation Fig.11 It can be obtained that the discharge specific capacity of the test group at each rate test is higher than that of the control group. Specifically, the discharge specific capacity of the test group at 0.05C, 0.1C, 0.2, 0.5, 1C, 2C, 5C, and 10C is 261.8mAh / g, 242.5mAh / g, 227.7mAh / g, 209.4mAh / g, 193.5mAh / g, 174.6mAh / g, 140.2mAh / g, and 96.3mAh / g. Moreover, after rapid charge and discharge, the charge and discharge test of 1C is carried out, and its capacity is still 193.7mAh / g, without capacity loss. The discharge specific capacity of the control group under 5C and 10C tests is only 88.4mAh / g and 45.5mAh / g. Through the above comparison, we can obtain that the rate performance of the test group after hydrothermal induced surface modification is greatly improved, and the generation of spinel provides a three-dimensional channel for Li transmission, which greatly accelerates the rate of Li transmission.

[0083] (7) Structural stability test

[0084] By observation Fig.12 It can be seen that after the test group was cycled 150 times at a rate of 1C, its particle structure was not significantly damaged, and its particle morphology was a complete, smooth sphere. This shows that the structure of the test group that underwent hydrothermal-induced surface modification was well maintained during the cycle, and no obvious structural degradation occurred. This also proves that hydrothermal treatment is very effective in alleviating lattice strain and interface corrosion.

[0085] By observation Fig.13 It can be seen that after the control group was cycled 150 times at a rate of 1C, its particle structure was obviously damaged, with a large number of breakages and cracks appearing on the particle surface and even spreading to the bulk phase. This shows that the structure of the control group that has not been hydrothermally treated has seriously deteriorated during the cycle, and obvious lattice strain and interface corrosion have occurred.

[0086] The above structure and specific implementation methods are further detailed descriptions of the present invention, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art to which the present invention belongs, without departing from the concept and scope of the present invention, several deductions or replacements of the above embodiments are within the protection scope of the present invention.

Claims

1. A method for surface modification of cobalt-free lithium-rich cathode materials, characterized in that: The following steps are involved: The cobalt-free lithium-rich positive electrode material is placed in a reactor, deionized water is added, stirred, and then heat-treated. After cooling, washing, and drying, a surface-modified cobalt-free lithium-rich positive electrode material is obtained; the surface-modified cobalt-free lithium-rich positive electrode material includes a cobalt-free lithium-rich positive electrode bulk phase and a surface heterogeneous layer with oxygen vacancies and a spinel phase.

2. The method according to claim 1, characterized in that The molecular formula of the cobalt-free lithium-rich cathode material is Li 1+x TM 1- x O2, where 0 < x < 0.35, and TM is one or more of Ni and Mn.

3. The method according to claim 1, characterized in that The ratio of the cobalt-free lithium-rich positive electrode material to deionized water is 0.5-5 g: 30-80 mL.

4. The method according to claim 1, characterized in that The stirring time is 2 to 5 hours.

5. The method according to claim 1, characterized in that The heat treatment is performed at 100 to 220° C. for 1 to 25 hours.

6. The method according to claim 1, characterized in that The cobalt-free lithium-rich positive electrode material is prepared by a solid phase sintering method, comprising the following steps: After the cobalt-free lithium-rich positive electrode material precursor and the lithium source are evenly mixed, the cobalt-free lithium-rich positive electrode material is obtained through high-temperature calcination; the conditions of the high-temperature calcination are: pre-calcining at 350-550°C for 2-7 hours in an air atmosphere, and then sintering at 600-1000°C for 7-15 hours, with a heating rate of 2-8°C / min, and then naturally cooling with the furnace.

7. The method according to claim 6, characterized in that The cobalt-free lithium-rich positive electrode material precursor is a combination of one or more of hydroxide, oxalate, and carbonate precipitates; the lithium source is a combination of one or more of lithium hydroxide, lithium carbonate, lithium acetate, lithium carbonate, and lithium chloride.

8. A surface modified cobalt-free lithium-rich cathode material, characterized in that: Prepared by the method according to any one of claims 1 to 7.

9. An electrode sheet, characterized in that: It is made using the surface-modified cobalt-free lithium-rich positive electrode material as claimed in claim 8.

10. A lithium ion battery, characterized in that: It is made using the surface-modified cobalt-free lithium-rich positive electrode material as claimed in claim 8.

Citation Information

Cited By

  • Cobalt-free lithium-rich manganese-based positive electrode material and preparation method thereof

    CN119890290A