Positive electrode material, preparation method of positive electrode material and battery

By doping the FeF2 cathode material with nitrogen and coating it with a carbon layer, the problems of bulk phase rupture and coating layer shedding are solved, the conductive performance and capacity retention rate of the battery are improved, and more efficient electrochemical performance is achieved.

CN118738318APending Publication Date: 2024-10-01JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410688307.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing cathode materials can easily cause bulk phase rupture and coating peeling off during cycling, affecting the conductivity, rate performance and capacity retention of the battery.

Method used

FeF2 material is used as the core layer, doped with nitrogen element, and its outer layer is coated with carbon material. Nitrogen and oxygen elements are doped in the shell layer to improve the bulk phase stability and conductive properties of the material.

Benefits of technology

Through the carbon coating layer and nitrogen and oxygen doping, the mechanical bonding force and electrical conductivity of the core layer are enhanced, bulk phase rupture and coating layer shedding are avoided, and the capacity retention rate and rate performance of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738318A_ABST
    Figure CN118738318A_ABST
Patent Text Reader

Abstract

The invention relates to the field of batteries, and provides a positive electrode material, a preparation method of the positive electrode material and a battery. The positive electrode material comprises a core layer and a shell layer wrapping the core layer, the core layer material is a FeF2 material doped with a first doping element, the shell layer material is a carbon material doped with a second doping element, the first doping element comprises an N element, and the second doping element comprises an N element and / or an O element. According to the positive electrode material provided by the invention, the core layer contains the FeF2 material, the shell layer is the carbon coating layer, the nitrogen element is doped in the core layer, and the nitrogen element and / or the oxygen element are / is doped in the shell layer, so that the bulk phase of the core layer material is not easy to break, and the conductivity and the capacity retention rate of the battery are also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a positive electrode material, a method for preparing the positive electrode material, and a battery. Background Art

[0002] With the continuous development of the market, long battery life is an inevitable development trend for electric vehicles and power tools in the future, so finding cathode materials with higher capacity and energy density has become an inevitable requirement for the current industry development. At present, most of the cathode materials for power batteries on the market are ternary cathode materials. FeF2 cathode materials have a higher theoretical specific capacity (571mAh·g -1 ), low cost and high conversion potential have good application prospects, but its conductivity is relatively poor. In existing research, the electrochemical properties of materials are mainly improved by nano-materials and composites with conductive carbon. However, the prepared nanomaterials often have problems such as large size and agglomeration of nanoparticles, which affect the rate performance of the materials, and the conversion reaction during the cycle process is prone to bulk fragmentation, which can easily lead to material failure. Although the bulk rupture can be weakened to a certain extent by coating the outer layer of the positive electrode material with carbon material, the coating layer is easy to fall off and cause the positive electrode material to fail, further affecting the conductivity, capacity retention rate and rate performance of the battery.

[0003] Therefore, there is an urgent need to develop a positive electrode material that is not easy to break, the coating layer is not easy to fall off, and the battery has good conductivity, rate performance and capacity retention. Summary of the invention

[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a positive electrode material, a method for preparing the positive electrode material and a battery. The core layer of the positive electrode material of the present invention contains FeF2 material, the shell layer is a carbon coating layer, and the core layer is doped with nitrogen, and the shell layer is doped with nitrogen and / or oxygen, so that the bulk phase of the core layer material is not easy to break, and it is also beneficial to improve the conductivity and capacity retention rate of the battery.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a positive electrode material, which includes a core layer and a shell layer wrapping the core layer, the core layer material is a FeF2 material doped with a first doping element, and the shell layer material is a carbon material doped with a second doping element, the first doping element includes N element, and the second doping element includes N element and / or O element.

[0006] Optionally, the particle size of the positive electrode material meets 1 / 3≤Dv50 / Dv90≤3 / 4.

[0007] Optionally, the particle size of the positive electrode material meets the requirement of 3μm≤Dv90≤20μm.

[0008] Optionally, the particle size of the positive electrode material meets the requirement of 3.5 μm≤Dv90≤5 μm.

[0009] Optionally, the specific surface area of ​​the positive electrode material is 20m 2 / g≤S A ≤25m 2 / g.

[0010] Optionally, the shell layer thickness is TS, 20nm≤TS≤100nm.

[0011] Optionally, the second doping element includes N element and O element.

[0012] Optionally, the content A of the N element and the content B of the O element meet the following conditions: 1%≤(AB) / (A+B)≤90%.

[0013] Optionally, the mass ratio of the core layer to the shell layer in the positive electrode material is 1:(0.01-0.1).

[0014] Optionally, based on the mass of the core layer, the content of the first doping element in the core layer is 0.01%-0.05%.

[0015] Optionally, based on the mass of the shell layer, the content of the second doping element in the shell layer is 0.5%-2%.

[0016] Optionally, the mass ratio of the first doping element in the core layer to the second doping element in the shell layer is 1:(0.1-20).

[0017] A second aspect of the present invention provides a method for preparing a positive electrode material, the method comprising: (1) obtaining a first material containing an iron source, a fluorine source, a first doping element source and water, wherein the first doping element source comprises a first nitrogen source;

[0018] (2) mixing the first material with a first organic solvent to cause a precipitation reaction to form a solid first intermediate product;

[0019] (3) mixing the first intermediate product with a second material and ball milling the mixture to obtain a solid second intermediate product; the second material contains a second doping element source, a carbon source and water, and the second doping element source includes a second nitrogen source and / or an oxygen source;

[0020] (4) Heat-treating the second intermediate product to obtain the positive electrode material.

[0021] Optionally, the water in step (1) is added at least twice.

[0022] Optionally, the first material is obtained by: dividing the water in step (1) into a first portion of water and a second portion of water; mixing the iron source, the fluorine source, the first doping element source and the first portion of water to obtain a suspension A; mixing the suspension A with the second portion of water to obtain the first material.

[0023] Optionally, the viscosity of the suspension A is 200 cP-500 cP.

[0024] Optionally, the viscosity of the first material is 20 cP-100 cP.

[0025] Optionally, the iron source in step (1) is selected from iron powder and / or iron salt, and the iron salt is selected from at least one of ferrous chloride, ferric chloride, ferrous sulfate, ferrous sulfate, ferrous nitrate, ferric nitrate, ferrous acetate and ferric acetate.

[0026] Optionally, the fluorine source is selected from at least one of H2SiF6, 1-butyl-3-methylimidazolium tetrafluoroborate, hydrofluoric acid and polyvinylidene fluoride.

[0027] Optionally, the first nitrogen source is selected from at least one of urea, ethylenediamine, melamine, acetonitrile, acrylonitrile and phenbutylamine. Preferably, the first nitrogen source is urea.

[0028] Optionally, in step (2), the first solvent is selected from at least one of anhydrous ethanol, ethylene glycol, NN-dimethylformamide, nitrogen-methylpyrrolidone, dimethyl carbonate, isopropanol and 1,3-butanediol.

[0029] Optionally, the first solvent is a combination of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone.

[0030] Optionally, the volume ratio of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone is (1-97):(1-97):(1-97):(1-97).

[0031] Optionally, the carbon source in step (3) is selected from at least one of glucose, asphalt, polydopamine, resorcinol, formaldehyde, starch, sucrose, sodium carboxymethyl cellulose, polyvinylidene fluoride, polyvinyl pyrrolidone, tannic acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, anthracene and aniline.

[0032] Optionally, the second nitrogen source is selected from at least one of urea, ethylenediamine, ammonium chloride, melamine, acetonitrile, acrylonitrile and phenbutylamine. Preferably, the second nitrogen source is urea.

[0033] Optionally, the heat treatment conditions in step (4) include: heating to 240°C-270°C, keeping warm for 2h-6h, then heating to 600°C-900°C, and keeping warm for 1h-5h.

[0034] A third aspect of the present invention provides a battery, which comprises the positive electrode material described in the first aspect and / or the positive electrode material obtained by the preparation method described in the second aspect.

[0035] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0036] (1) The positive electrode material provided by the present invention has a core layer containing FeF2 material, a shell layer being a carbon coating layer, and the core layer is doped with nitrogen, and the shell layer is doped with nitrogen and / or oxygen. The carbon coating layer on the outer layer of the core layer makes the bulk phase of the core layer difficult to break, and can also suppress the volume change of the core layer during the conversion reaction. In addition to the mechanical bonding between the core layer and the shell layer, the van der Waals force between the nitrogen doped in the core layer and the nitrogen and / or oxygen doped in the shell layer makes the core layer and the shell layer tightly bonded, strengthens the anchoring effect of the carbon layer, makes the shell layer difficult to fall off, makes the bulk phase of the core layer material difficult to break, and improves the capacity retention rate of the battery. In addition, the nitrogen doped in the core layer and the nitrogen and / or oxygen doped in the shell layer are also beneficial to improving the conductivity of the battery.

[0037] (2) In the positive electrode material provided by the present invention, when the nitrogen element doped in the core layer is urea, urea has a small molecular structure and can provide smaller crystal nuclei during the growth of the core layer material, so that the obtained core layer material has a smaller particle size, making it less likely for the positive electrode material to have problems such as nanoparticle agglomeration, which helps to improve the rate performance of the battery.

[0038] (3) When the nitrogen element doped in the positive electrode material provided by the present invention is urea, the urea decomposes at high temperature, so that the shell layer has a high specific surface area and a rich pore structure. The large porosity can promote the absorption and infiltration of the electrolyte and improve the wetting effect of the electrode.

[0039] (4) The positive electrode plate obtained by the preparation method provided by the present invention is prepared by combining a first organic solvent and a first doping element to obtain a micro-nano core layer material with a smaller particle size, thereby avoiding agglomeration of nanoparticles and avoiding bulk phase rupture during the cycle. The micro-nano structure can reduce the volume expansion of the material, increase the contact area, and improve the rate performance of the material.

[0040] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a SEM image of the FeF2 material in Example 1, in which the core layer is not doped with nitrogen and is not coated with a shell layer.

[0042] Figure 2 This is the SEM image of the FeF2 material doped with nitrogen in the core layer in Example 1.

[0043] Figure 3 This is a SEM image of the N-FeF2@C material in Example 1, in which the core layer is doped with nitrogen and the core layer is covered with a shell layer, and the shell layer is doped with nitrogen and oxygen. DETAILED DESCRIPTION

[0044] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0045] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0046] A first aspect of the present invention provides a positive electrode material, which includes a core layer and a shell layer wrapping the core layer, the core layer material is a FeF2 material doped with a first doping element, the shell layer material is a carbon material doped with a second doping element, the first doping element includes N element, and the second doping element includes N element and / or O element.

[0047] The bulk phase of the positive electrode material of the present invention is FeF2 doped with N element, and the coating layer is a carbon layer doped with N element and / or O element. The shell layer is wrapped around the outside of the core layer, so that the bulk phase of the core layer is not easy to break. In addition to being tightly combined by mechanical force, the nitrogen element in the core layer exists as a nitrogen-containing functional group, which is combined with the oxygen-containing functional group and / or nitrogen-containing functional group in the shell layer by van der Waals force, which is more conducive to making the core layer and the shell layer tightly combined, so that the bulk phase is not easy to break.

[0048] In some embodiments, the particle size of the positive electrode material meets 1 / 3≤Dv50 / Dv90≤3 / 4. The particle size test method in the present invention is tested by referring to the standard GB / T 21524-2008 Determination of particle size in inorganic chemical products by sieving method.

[0049] In some embodiments, the particle size of the positive electrode material meets 3μm≤Dv90≤20μm, such as 3μm, 4μm, 6μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm and 20μm; preferably, the particle size of the positive electrode material meets 3.5μm≤Dv90≤5μm.

[0050] In some embodiments, the specific surface area of ​​the positive electrode material is 20 m 2 / g≤S A ≤25m 2 / g, such as 20m 2 / g, 21m 2 / g, 22m 2 / g, 23m 2 / g, 24m 2 / g and 25m 2 / g. The test method for specific surface area in the present invention is GB / T 19587-2017 gas adsorption BET method for determining specific surface area of ​​solid substances.

[0051] In some embodiments, the shell thickness is TS, 20nm≤TS≤100nm, such as 20nm, 40nm6, 0nm, 80nm and 100nm. The thickness test method is to measure the shell thickness using an SEM image and a ruler. In the present invention, when the shell thickness is within the above range, it is beneficial to make the bulk phase of the core layer material less likely to break, improve the stability of the positive electrode material, and thus improve the capacity retention rate of the battery and the conductivity of the battery.

[0052] In the present invention, the shell material is a carbon material doped with N element and / or O element. Preferably, the shell material is a carbon material doped with N element and O element.

[0053] In some embodiments, the shell material is a carbon material doped with N element.

[0054] In some embodiments, the shell material is a carbon material doped with O element.

[0055] In some embodiments, the second doping element includes N and O; preferably, the content A of the N element and the content B of the O element meet 1%≤(AB) / (A+B)≤90%. Further preferably, the content A of the N element and the content B of the O element meet 1%≤(AB) / (A+B)≤70%. This is beneficial to improving the wettability of the electrolyte to the electrode sheet, and also beneficial to improving the capacity retention rate and conductivity of the battery.

[0056] In some embodiments, the mass ratio of the core layer to the shell layer in the positive electrode material is 1:(0.01-0.1), such as 1:0.01, 1:0.02, 1:0.04, 1:0.06, 1:0.08 and 1:0.1. The mass ratio of the core layer to the shell layer in the positive electrode material will affect the particle size and porosity of the positive electrode material, and will also affect the thickness of the shell layer. When the mass ratio of the core layer to the shell layer in the present invention is 1:(0.01-0.1), it is beneficial to improve the initial efficiency, capacity retention rate and conductivity of the battery, and is also beneficial to improve the wetting ability of the battery liquid to the battery.

[0057] The core layer material in the present invention is FeF2 material doped with N element.

[0058] In some embodiments, based on the mass of the core layer, the content of the first doping element in the core layer is 0.01%-0.05%, such as 0.01%, 0.02%, 0.03%, 0.04% and 0.05%. In the present invention, the content of the first doping element in the core layer will affect the particle size of the positive electrode material and the first efficiency of the battery. When the content of the first doping element in the core layer is 0.01%-0.05%, it is beneficial to improve the first efficiency, capacity retention rate and conductivity of the battery, and it is also beneficial to improve the wetting performance of the electrolyte on the electrode sheet.

[0059] In some embodiments, based on the mass of the core layer, the content of FeF2 material in the core layer is 99.95%-99.99%.

[0060] In some embodiments, based on the mass of the shell layer, the content of the second doping element in the shell layer is 0.5%-2%, for example, 0.5%, 1%, 1.5% and 2%. In the present invention, when the content of the second doping element in the shell layer is 0.5%-2%, it is beneficial to improve the first efficiency of the battery, the capacity retention rate of the battery and the conductivity, and it is also beneficial to improve the wetting performance of the electrolyte on the electrode.

[0061] In some embodiments, the mass ratio of the first doping element in the core layer to the second doping element in the shell layer is 1:(0.1-20), for example, it can be 1:0.1, 1:0.4, 1:1, 1:4, 1:8, 1:10, 1:16 and 1:20.

[0062] In some embodiments, based on the mass of the shell layer, the carbon content in the shell layer is 98%-99.5%.

[0063] A second aspect of the present invention provides a method for preparing a positive electrode material, the method comprising:

[0064] (1) obtaining a first material containing an iron source, a fluorine source, a first doping element source and water, wherein the first doping element source includes a first nitrogen source;

[0065] (2) mixing the first material with a first organic solvent to cause a precipitation reaction to form a solid first intermediate product;

[0066] (3) mixing the first intermediate product with a second material and ball milling the mixture to obtain a solid second intermediate product; the second material contains a second doping element source, a carbon source and water, and the second doping element source includes a second nitrogen source and / or an oxygen source;

[0067] (4) Heat-treating the second intermediate product to obtain the positive electrode material.

[0068] In some embodiments, the water in step (1) is added at least twice.

[0069] In some embodiments, the first material is obtained by: dividing the water in step (1) into a first portion of water and a second portion of water; mixing the iron source, the fluorine source, the first doping element source and the first portion of water to obtain a suspension A; and mixing the suspension A with the second portion of water to obtain the first material.

[0070] The iron source, the fluorine source, the first doping element source and the first portion of water are mixed to obtain a suspension A, and the fluorine source weak electrolyte is partially ionized to form HSiF6 - or SiF6 2- With hydronium ion H3O + A gel structure is formed to stabilize the dispersion and stability of the iron source in the system, and the first doping element source is dissolved to form small molecules uniformly dispersed in the mixed system.

[0071] In some embodiments, the mass ratio of the iron source, fluorine source, first doping element source and first portion of water in step (1) is (1-4, for example, 1, 2, 3, 4): (3-10, for example, 3, 5, 7, 9, 11): (0.1-2, for example, 0.1, 0.5, 1, 1.5, 2): (3-6, for example, 3, 4, 5, 6). When the mass ratio of the iron source, fluorine source, first doping element source and first portion of water in the present invention is within the above range, it is beneficial to improve the first efficiency, capacity retention rate and conductivity of the battery.

[0072] In some embodiments, the volume ratio of the suspension A to the second portion of water is 1:(1-20), such as 1:1, 1:5, 1:10, 1:15 and 1:20. In the present invention, when the volume ratio of the suspension A to the second portion of water is 1:(1-20), it is beneficial to improve the first effect, capacity retention rate and conductivity of the positive electrode material, and it is also beneficial to improve the wetting ability of the electrolyte to the electrode sheet.

[0073] In some embodiments, the viscosity of the suspension A is 200cP-500cP, such as 200cP, 300cP, 400cP and 500cP; and / or the viscosity of the first material is 20cP-100cP, such as 20cP, 50cP, 70cP, 90cP and 100cP.

[0074] In some embodiments, the iron source is selected from iron powder and / or iron salt. Preferably, the iron salt is selected from at least one of ferrous chloride, ferric chloride, ferrous sulfate, ferrous sulfate, ferrous nitrate, ferric nitrate, ferrous acetate and ferric acetate.

[0075] In some embodiments, the fluorine source is selected from at least one of H2SiF6, 1-butyl-3-methylimidazolium tetrafluoroborate, hydrofluoric acid, and polyvinylidene fluoride.

[0076] In some embodiments, the first nitrogen source is selected from at least one of urea, ethylenediamine, melamine, acetonitrile, acrylonitrile and phenylbutylamine, and preferably, the first nitrogen source is urea. When the first nitrogen source doped in the core layer is urea, urea is a small molecule, which can provide a smaller crystal nucleus for the precipitated first intermediate product, making the crystal size of the positive electrode material smaller, more conducive to bulk stability, making it less prone to rupture, and more conducive to improving the capacity retention rate.

[0077] In step (2) of the present invention, the first material is mixed with a first organic solvent, and a precipitation reaction occurs to form a solid first intermediate product; a precipitate is formed which is a mixture comprising a fluorine source, an iron source, and a first nitrogen source. The fluorine source has a low solubility in the organic solvent and is rapidly crystallized and precipitated. During the crystallization process, the attached iron powder is precipitated together. If the iron source is an iron salt, the iron salt and the fluorine source generate a FeSiF6 precipitate, and at this time, the precipitate phase contains small molecules of the first nitrogen source.

[0078] In some embodiments, the first solvent in step (2) is selected from at least one of anhydrous ethanol, ethylene glycol, NN-dimethylformamide, nitrogen-methylpyrrolidone, dimethyl carbonate, isopropanol and 1,3-butanediol.

[0079] In some embodiments, the first solvent is a combination of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone. The solvents in the first solvent are mutually soluble and allow the first material to precipitate. The first organic solvent is a mixture of multiple solvent components. When the solubility is appropriate, the crystal precipitation rate is appropriate, the crystal size is uniform, and the particle size of the first intermediate product precipitated is uniform, the particle size is small, it is not easy to agglomerate, and the bulk phase is not easy to break. When the nitrogen element doped in the first material is urea, urea is a small molecule, and the size of the crystal nucleus formed is small, which is more conducive to promoting the uniform growth of the crystal. Therefore, the selection of the first solvent is related to the size of the prepared positive electrode material and the uniformity of the particles of the positive electrode material, and further has a great influence on the agglomeration, bulk stability and conductivity of the positive electrode material.

[0080] In some embodiments, the volume ratio of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone is (1-97):(1-97):(1-97):(1-97). Preferably, the volume ratio of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone is one of 25:25:25:25, 25%:25:15:35, 15:15:35:35 or 35:35:15:15.

[0081] In step (3) of the present invention, the first intermediate product is mixed with the second material and ball-milled to obtain a solid second intermediate product; the second material contains a second doping element source, a carbon source and water, and the second doping element source includes a second nitrogen source and / or an oxygen source. After ball milling, the second intermediate product is a carbon layer doped with the second doping source wrapped around the outer layer of the first intermediate product.

[0082] In some embodiments, the second doping element source in step (3) comprises a second nitrogen source and an oxygen source.

[0083] In some embodiments, the content A of the N element and the content B of the O element meet 1%≤(AB) / (A+B)≤90%. Preferably, the content A of the N element and the content B of the O element meet 1%≤(AB) / (A+B)≤70%.

[0084] In some embodiments, in step (3), the first intermediate product is mixed with the second doping element source, the carbon source and water in the second material, and the mass ratio of the first intermediate product to the second doping element source and the carbon source in the second material is 1:(0.2-10), for example, it can be 1:0.2, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 and 1:10.

[0085] In some embodiments, the mass ratio of the second doping element source to the carbon source is 1:(0.02-50), for example, it can be 1:0.02, 1:0.5, 1:1, 1:5, 1:10 and 1:50.

[0086] In some embodiments, the mass ratio of the first intermediate product to the second doping element source and the carbon source in the second material is 1:(0.1-5):(0.1-5), preferably, the mass ratio of the first intermediate product to the second doping element source in the second material is 1:0.1, 1:1, 1:2, 1:3, 1:4 and 1:5; the mass ratio of the first intermediate product to the carbon source in the second material is 1:0.1, 1:1, 1:2, 1:3, 1:4 and 1:5. When the mass ratio of the second doping element source, the carbon source and water in the first intermediate product, the second material is 1:(0.1-5):(0.1-5), it is beneficial to improve the first efficiency, capacity retention rate and conductivity of the battery, and it is also beneficial to improve the wetting ability of the electrolyte to the electrode.

[0087] In some embodiments, the method or equipment of ball milling in step (3) is not particularly limited, and ball milling can be performed in a ball mill, for example.

[0088] In some embodiments, the ball milling atmosphere is an inert atmosphere, such as argon or nitrogen.

[0089] In some embodiments, after the first intermediate product and the second material are mixed and ball-milled, vacuum drying is performed.

[0090] In some embodiments, the carbon source in step (3) is selected from at least one of glucose, asphalt, polydopamine, resorcinol, formaldehyde, starch, sucrose, sodium carboxymethyl cellulose, polyvinylidene fluoride, polyvinyl pyrrolidone, tannic acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, anthracene and aniline.

[0091] In some embodiments, the second nitrogen source is selected from at least one of urea, ethylenediamine, ammonium chloride, melamine, acetonitrile, acrylonitrile and phenylbutylamine, and preferably, the second nitrogen source is urea. Urea exists in the form of small molecules and is more easily doped into the first intermediate product during the growth process, and exists in the first intermediate product in the form of atomic doping.

[0092] In some embodiments, the oxygen source is selected from urea and / or hydrogen peroxide.

[0093] In the present invention, in step (4), the second intermediate product is heat treated to obtain the positive electrode material. The carbon layer is oxidized to form an outer carbon layer, the nitrogen source reacts at high temperature to generate nitrogen-containing groups, and when the iron source is iron powder, the iron powder undergoes an oxidation reaction at high temperature and reacts with the fluorine source decomposed at high temperature to generate FeF2. If the iron source is an iron salt, the FeSiF6 generated in step (3) is decomposed to generate F2 and then generate FeF2.

[0094] In some embodiments, the heat treatment conditions in step (4) include: heating to 240°C-270°C, such as 240°C, 250°C, 260°C and 270°C, keeping warm for 2h-6h, such as 2h, 3h, 4h, 5h and 6h, then heating to 600°C-900°C, such as 600°C, 700°C, 800°C and 900°C, keeping warm for 1h-5h, such as 1h, 2h, 3h, 4h and 5h.

[0095] A third aspect of the present invention provides a battery, which comprises the positive electrode material described in the first aspect and / or the positive electrode material obtained by the preparation method described in the second aspect.

[0096] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0097] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0098] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0099] Example 1

[0100] This example is used to illustrate the preparation method of the positive electrode material of the present invention.

[0101] (1) 2g iron powder, 7g H2SiF6 aqueous solution (35%), 1g urea and 3mL deionized water were stirred in a beaker for 24h. The mass ratio of iron source, fluorine source and first doping element source was 2:7:1. Then 10mL of the above solution was added with deionized water to 20ml to obtain a first material containing iron source, fluorine source, first doping element source and water.

[0102] (2) Add the first material to 5 times the volume of the mixed solvent (V 无水乙醇 :V 乙二醇 :V N,N-二甲基甲酰胺 :V 氮甲基吡咯烷酮=25:25:25:25), stirred for 10 min to obtain a white precipitate, which was washed with anhydrous ethanol and dried in vacuum to form a solid first intermediate product.

[0103] (3) The first intermediate product was mixed with 1 g of urea, 0.5 g of glucose and 2 ml of deionized water, stirred evenly, and placed in a ball mill for ball milling in an argon atmosphere at a speed of 600 rpm for 1 h, and then dried in a vacuum oven at 80° C. for 12 h for use to obtain a solid second intermediate product.

[0104] (4) The second intermediate product is placed in a magnetic boat in a tubular furnace in an Ar atmosphere and the temperature is increased to 260°C at 3°C / min and kept at this temperature for 4 hours, and then the temperature is increased to 800°C at 5°C / min and kept at this temperature for 2 hours. After the temperature drops to room temperature, the material is taken out and ground to obtain the positive electrode material of the present invention.

[0105] The shell thickness of the positive electrode material of the present invention is 25nm, and the specific surface area of ​​the positive electrode material is 23m 2 / g, the mass ratio of the core layer to the shell layer is 1:0.02, the content of the first doping element in the core layer is 0.02%, the content of the second doping element in the shell layer is 1.5%, and the ratio of the content of the N element to the content of the O element in the shell layer is 4:1. The particle size Dv50 of the positive electrode material is 3μm, and Dv90 is 5μm.

[0106] Example 2

[0107] This example is used to illustrate the preparation of positive electrode materials when the contents of the iron source, the fluorine source, and the first nitrogen source are different.

[0108] Example 2-1

[0109] The operation was carried out according to the method described in Example 1, except that in step (1), the iron powder was 1 g, the H2SiF6 aqueous solution (35%) was 10 g, and the urea was 2 g. At this time, the mass ratio of the iron source, the fluorine source, and the first doping element source was 1:10:2. The content of the first doping element in the core layer was 0.03%, and the particle size Dv50 of the positive electrode material was 2.8 μm, and Dv90 was 4.5 μm.

[0110] Example 2-2

[0111] The operation was carried out according to the method described in Example 1, except that in step (1), the iron powder was 4 g, the H2SiF6 was 4 g aqueous solution (35%), and the urea was 0.5 g. At this time, the mass ratio of the iron source, the fluorine source, and the first doping element source was 4:4:0.5. The content of the first doping element in the core layer was 0.01%, and the particle size Dv50 of the positive electrode material was 3.2 μm and Dv90 was 4.6 μm.

[0112] Example 2-3

[0113] The operation was carried out according to the method described in Example 1, except that in step (1), the iron powder was 2 g, the H2SiF6 was 7 g aqueous solution (35%), and the urea was 1 g. At this time, the mass ratio of the iron source, the fluorine source, and the first doping element source was 2:7:1. The content of the first doping element in the core layer was 0.015%, and the particle size Dv50 of the positive electrode material was 4.6 μm and Dv90 was 8.4 μm.

[0114] Example 3

[0115] This example is used to illustrate the preparation of positive electrode materials when the contents of the second doping element source and the carbon source are different.

[0116] Example 3-1

[0117] The operation was carried out according to the method described in Example 1, except that in step (3), the second doping element source was urea, urea was 2g, and the carbon source was glucose, glucose was 0.1g. The shell thickness in the positive electrode material was 30nm, the mass ratio of the core layer to the shell layer was 1:0.03, the content of the second doping element in the shell layer was 1.8%, and the content of the N element in the shell layer was A, and the content ratio of the O element was 5:1.

[0118] Example 3-2

[0119] The operation was carried out according to the method described in Example 1, except that in step (3), the second doping element source was urea, 0.5 g of urea, and the carbon source was glucose, 0.1 g of glucose. The shell thickness of the positive electrode material was 20 nm, the mass ratio of the core layer to the shell layer was 1:0.012, the content of the second doping element in the shell layer was 1%, and the content of the N element in the shell layer was A, and the ratio of the content of the O element was 2:1.

[0120] Example 4

[0121] This example is used to illustrate the preparation of positive electrode materials with different solvent components and contents.

[0122] Example 4-1

[0123] The operation was carried out according to the method described in Example 1, except that the solvent V in step (2) 无水乙醇 :V 乙二醇 :V N,N-二甲基甲酰胺 :V 氮甲基吡咯烷酮 =35:35:15:15. The particle size Dv50 of the positive electrode material is 5.3 μm, and Dv90 is 9.6 μm.

[0124] Example 4-2

[0125] The method described in Example 1 was followed, except that in step (2), V 无水乙醇 :V 乙二醇:V N,N-二甲基甲酰胺 :V 氮甲基吡咯烷酮 =15:15:35:35. The particle size Dv50 of the positive electrode material is 5.4 μm, and Dv90 is 8.6 μm.

[0126] Example 4-3

[0127] The method described in Example 1 was followed, except that in step (2), V 无水乙醇 :V 乙二醇 :V N,N-二甲基甲酰胺 :V 氮甲基吡咯烷酮 =45:45:5:5. The particle size Dv50 of the positive electrode material is 4.1 μm, and Dv90 is 8.6 μm.

[0128] Example 4-4

[0129] The operation was carried out according to the method described in Example 1, except that the solvent in step (2) was anhydrous ethanol and ethylene glycol, V 无水乙醇 :V 乙二醇 =50:50. The particle size Dv50 of the positive electrode material is 6.8 μm, and Dv90 is 12.8 μm.

[0130] Example 5

[0131] This embodiment is used to illustrate the preparation of positive electrode materials when the first doping element source is different.

[0132] Example 5-1

[0133] The method described in Example 1 was followed, except that in step (1), the first nitrogen source was acrylonitrile and the second nitrogen source was ethylenediamine. The particle size Dv50 of the positive electrode material was 3.1 μm and Dv90 was 5.4 μm.

[0134] Example 5-2

[0135] The method described in Example 1 was followed, except that in step (1), the first nitrogen source was melamine and the second nitrogen source was ethylenediamine. The particle size Dv50 of the positive electrode material was 4.8 μm and Dv90 was 8.5 μm.

[0136] Example 6

[0137] This embodiment is used to illustrate the preparation of positive electrode materials when the second doping element source is different.

[0138] Example 6-1

[0139] The process is carried out in accordance with the method described in Example 1, except that in step (3), the second doping element source is ammonium chloride.

[0140] Example 6-2

[0141] The method described in Example 1 is followed, except that the second doping element source in step (1) is hydrogen peroxide.

[0142] Comparative Example 1

[0143] This comparative example is used to illustrate the preparation of a positive electrode material without a shell layer.

[0144] The process was carried out in accordance with the method described in Example 1, except that step 3 was not performed.

[0145] Comparative Example 2

[0146] This comparative example is used to illustrate the preparation of a positive electrode material without a shell layer and without nitrogen doping in the core layer.

[0147] The process described in Example 1 was followed, except that the first nitrogen source was not added in step (1) and step 3 was not performed.

[0148] Comparative Example 3

[0149] This comparative example is used to illustrate the preparation of a positive electrode material when the core layer material is not doped with the first doping element and the shell layer is not doped with the second doping element.

[0150] The operation was carried out according to the method described in Example 1, except that the first nitrogen source was not added in step (1) and urea was not added in step (3). The particle size Dv50 of the positive electrode material was 4.6 μm and Dv90 was 7.9 μm.

[0151] Comparative Example 4

[0152] This comparative example is used to illustrate the preparation of a positive electrode material when the shell material is not doped with the second doping element.

[0153] The process described in Example 1 was followed, except that no urea was added in step (3).

[0154] Comparative Example 5

[0155] This comparative example is used to illustrate the preparation of a positive electrode material when the core layer material is not doped with the first doping element.

[0156] The method described in Example 1 was followed, except that the first nitrogen source was not added in step (1). The particle size Dv50 of the positive electrode material was 5.6 μm, and Dv90 was 9.4 μm.

[0157] Test Case

[0158] Preparation of negative electrode sheet: Graphite material is used as the negative electrode active material, mixed with conductive agent, binder, etc., coated on copper foil, and made into negative electrode sheet through drying, sheet pressing and other processes. The size of negative electrode sheet is (100mm×55mm). The size of positive electrode sheet is 96mm×51mm.

[0159] Preparation of positive electrode sheet: The prepared positive electrode material is used as the positive electrode, the positive electrode material is mixed with conductive carbon black, polyvinylidene fluoride, etc., coated on aluminum foil, and made into a positive electrode sheet through processes such as drying and pressing. The size of the positive electrode sheet is 96mm×51mm.

[0160] The separator is Celgard 2320 microporous polypropylene film.

[0161] The electrolyte is 1 mol / L LiPF6 dissolved in a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a 1:1 volume ratio.

[0162] Battery assembly: stack the positive electrode sheets, separators, and negative electrode sheets in the above embodiments and comparative examples in order to obtain a battery. Heat-press the stacked battery and place it in an aluminum-plastic film for top and side sealing. Inject the electrolyte into the battery. Seal the battery after injection, with an injection coefficient of 3g / Ah. Formation: Perform formation treatment on the packaged battery. Set the charge and discharge cut-off voltage to 2.8-4.2V, the charge and discharge current to 1A / g, and end the test after 200 cycles.

[0163] The batteries obtained in the examples and comparative examples were tested for the first coulombic efficiency, energy density and 2000 cycle capacity retention rate. The experimental results are shown in Table 1.

[0164] (1) First efficiency test method: After the battery is manufactured, it is first charged to 3.75V at a constant current of 0.1C to obtain the formation capacity C0. Then the battery is divided into different capacities, charged to 4.25V at a constant current of 0.33C, and then charged to I≤0.05C at a constant voltage of 4.25V to obtain the battery capacity C1 after the capacity division. After standing for 5 minutes, the battery is discharged to 2.8V at a constant current of 1C to obtain the discharge capacity C2, and then discharged to 2.8V at a constant current of 0.1C to obtain the discharge capacity C3, and then discharged to 2.8V at a constant current of 0.01C to obtain the discharge capacity C4; the first coulomb efficiency (first efficiency) is calculated according to (C2+C3+C4) / (C0+C1)*100%.

[0165] (2) 2000 cycle capacity retention rate test method: 1. After the capacity division is completed, the battery is first charged to 4.25V at a constant current rate of 1C, and then charged to I≤0.05C at a constant voltage of 4.25V; 2. After standing for 5 minutes, the battery is discharged to 2.8V at a constant current rate of 1C to obtain the discharge capacity C1; 3. Stand for 30 minutes. Repeat steps 1-3 1999 times to obtain the discharge capacity C2000; the 2000 cycle capacity retention rate is calculated as (C2000) / (C1)*100%.

[0166] (3) Contact angle test method: This is done using an optical contact angle measuring instrument, ranging from manual instruments to fully automatic systems. In the sessile drop method, a drop of liquid (usually water) is placed on a solid sample, an image of the drop is captured by a high-resolution camera, and the angle is then automatically measured by software.

[0167] (4) ACIR (AC internal resistance in mΩ) test method: The impedance behavior of the battery cell is tested under a high-frequency sinusoidal AC current with a frequency of 1 kHz and an excitation amplitude of 5 mV.

[0168] Table 1

[0169]

[0170]

[0171] Figure 1 This is an SEM image of the FeF2 material in Example 1, in which the core layer is not doped with nitrogen and is not coated with a shell layer. No nitrogen doping is performed and no multiple solvents are used for regulation. The FeF2 particles are large in size and have serious agglomeration. This structure will reduce the material rate performance, and the larger particles and agglomeration will aggravate the bulk fragmentation.

[0172] Figure 2 This is a SEM image of the FeF2 material doped with nitrogen in the core layer in Example 1. Using multiple solvents for regulation, the particle size of the N-FeF2 material is small and uniform.

[0173] Figure 3 This is a SEM image of the N-FeF2@C material in Example 1, in which the core layer is doped with nitrogen and the shell layer is coated with nitrogen and oxygen. The carbon layer has a uniform thickness and a porous structure, which can promote electrolyte infiltration and rapid ion transfer, and enhance the rate performance and capacity retention of the battery cell.

[0174] In the present invention, the mass ratio of the core layer material to the shell layer material, the type and content of the first doping element source in the core layer material, and the type and content of the second doping element in the shell layer material will all affect the particle size of the positive electrode material. When the molecular weight of the first doping element source and the second doping element source is small, the crystal size of the generated positive electrode material is also small, which is beneficial to maintain the stability of the positive electrode material, and the first doping element source and the second doping element source also help to increase the specific surface area and porosity of the positive electrode material. The large porosity is beneficial to improve the wetting ability of the electrolyte to the electrode sheet. When the content of the first doping element source in the core layer and the second doping element source in the shell layer is within the range of the present invention, it is beneficial to improve the first efficiency and capacity retention rate of the battery.

[0175] The different types of solvents and volume ratios of the solvents in the present invention will result in different sizes and speeds of crystal growth. The solvents in the present invention are conducive to obtaining positive electrode materials with smaller particle sizes, making the bulk phase of the core layer less likely to break, which is conducive to improving the capacity retention rate of the battery, reducing the AC internal resistance of the battery and reducing the contact angle between the electrolyte and the positive electrode sheet (improving the wetting ability of the electrolyte on the electrode sheet).

[0176] By conducting electrochemical tests on the electrodes assembled into battery cells, after 2,000 cycles, the composite electrode battery cells have obvious advantages in first efficiency, capacity retention rate and contact angle after 2,000 cycles compared with those without the first doping element and without the second doping element. When the first doping element is urea and the second doping element contains both nitrogen and oxygen, the particle size of the positive electrode material is smaller, less likely to agglomerate, and the bulk phase is not easy to rupture, and the advantages in first efficiency, capacity retention rate and contact angle are more obvious.

[0177] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0178] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A positive electrode material, characterized in that: The positive electrode material includes a core layer and a shell layer wrapping the core layer, the core layer material is a FeF2 material doped with a first doping element, the shell layer material is a carbon material doped with a second doping element, the first doping element includes N element, and the second doping element includes N element and / or O element.

2. The positive electrode material according to claim 1, characterized in that The particle size of the positive electrode material meets 1 / 3≤Dv50 / Dv90≤3 / 4; and / or, The particle size of the positive electrode material meets the requirement of 3μm≤Dv90≤20μm, preferably, the particle size of the positive electrode material meets the requirement of 3.5μm≤Dv90≤5μm; and / or, The specific surface area of ​​the positive electrode material is 20 m 2 / g≤S A ≤25m 2 / g.

3. The positive electrode material according to claim 1, characterized in that The shell thickness is TS, 20nm≤TS≤100nm; and / or, The second doping element includes N element and O element; preferably, the content A of the N element and the content B of the O element meet 1%≤(AB) / (A+B)≤90%.

4. The positive electrode material according to any one of claims 1 to 3, characterized in that The mass ratio of the core layer to the shell layer in the positive electrode material is 1:(0.01-0.1); and / or, Based on the mass of the core layer, the content of the first doping element in the core layer is 0.01%-0.05%; and / or, Based on the mass of the shell layer, the content of the second doping element in the shell layer is 0.5%-2%; and / or, The mass ratio of the first doping element in the core layer to the second doping element in the shell layer is 1:(0.1-20).

5. A method for preparing a positive electrode material, characterized in that: The method comprises: (1) obtaining a first material containing an iron source, a fluorine source, a first doping element source and water, wherein the first doping element source includes a first nitrogen source; (2) mixing the first material with a first organic solvent to cause a precipitation reaction to form a solid first intermediate product; (3) mixing the first intermediate product with a second material and ball milling the mixture to obtain a solid second intermediate product; the second material contains a second doping element source, a carbon source and water, and the second doping element source includes a second nitrogen source and / or an oxygen source; (4) Heat-treating the second intermediate product to obtain the positive electrode material.

6. The method according to claim 5, characterized in that The water in step (1) is added at least twice; Preferably, the first material is obtained by the following method: dividing the water in step (1) into a first portion of water and a second portion of water; mixing the iron source, the fluorine source, the first doping element source and the first portion of water to obtain a suspension A; mixing the suspension A with the second portion of water to obtain the first material; Preferably, the viscosity of the suspension A is 200 cP-500 cP; and / or the viscosity of the first material is 20 cP-100 cP.

7. The method according to claim 5, characterized in that The iron source in step (1) is selected from iron powder and / or iron salt, and the iron salt is selected from at least one of ferrous chloride, ferric chloride, ferrous sulfate, ferrous sulfate, ferrous nitrate, ferric nitrate, ferrous acetate and ferric acetate; and / or, The fluorine source is selected from at least one of H2SiF6, 1-butyl-3-methylimidazolium tetrafluoroborate, hydrofluoric acid and polyvinylidene fluoride; and / or, The first nitrogen source is selected from at least one of urea, ethylenediamine, melamine, acetonitrile, acrylonitrile and phenbutylamine. Preferably, the first nitrogen source is urea.

8. The method according to claim 5, characterized in that In step (2), the first solvent is selected from at least one of anhydrous ethanol, ethylene glycol, NN-dimethylformamide, nitrogen-methyl pyrrolidone, dimethyl carbonate, isopropanol and 1,3-butanediol; Preferably, the first solvent is a combination of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone; The volume ratio of anhydrous ethanol, ethylene glycol, NN-dimethylformamide and nitrogen methyl pyrrolidone is (1-97):(1-97):(1-97):(1-97).

9. The method according to claim 5, characterized in that The carbon source in step (3) is selected from at least one of glucose, asphalt, polydopamine, resorcinol, formaldehyde, starch, sucrose, sodium carboxymethyl cellulose, polyvinylidene fluoride, polyvinyl pyrrolidone, tannic acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, anthracene and aniline; and / or, The second nitrogen source is selected from at least one of urea, ethylenediamine, ammonium chloride, melamine, acetonitrile, acrylonitrile and phenbutylamine. Preferably, the second nitrogen source is urea.

10. The method according to claim 5, characterized in that The heat treatment conditions in step (4) include: heating to 240°C-270°C, keeping the temperature for 2h-6h, then heating to 600°C-900°C, and keeping the temperature for 1h-5h.

11. A battery, characterized in that: The battery comprises the positive electrode material according to any one of claims 1 to 4 and / or the positive electrode material obtained by the preparation method according to any one of claims 5 to 10.

Citation Information

Cited By

  • Surface-functionalized lithium manganese iron phosphate, positive pole piece containing surface-functionalized lithium manganese iron phosphate and battery containing surface-functionalized lithium manganese iron phosphate

    CN121506910A