Graphite composite material and preparation method and application thereof

By combining vertically grown carbon nanotubes with modified graphite in lithium-ion batteries, and forming an amorphous carbon coating layer through carbonization, the cracking problem caused by expansion of the silicon anode material is solved, and the specific capacity and cycle of the battery are improved. performance, enhanced conductivity and stability.

CN118738353APending Publication Date: 2024-10-01CARBON ONE NEW ENERGY HANGZHOU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068140.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The silicon anode material in existing lithium-ion batteries cracks due to expansion/contraction stress during the charge and discharge process, resulting in specific capacity loss and low cycle efficiency. Moreover, the direct addition of carbon nanotubes is difficult to disperse evenly, affecting material performance.

Method used

Vertically grown carbon nanotubes are combined with modified graphite to form a graphite composite material, and an amorphous carbon coating layer is formed through the carbonization process to enhance the expansion buffering and conductivity of silicon and improve the stability of the solid electrolyte interface.

Benefits of technology

It significantly improves the specific capacity, rate performance and cycle performance of the graphite anode of lithium-ion batteries, reduces side reactions, and enhances conductivity and material stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738353A_ABST
    Figure CN118738353A_ABST
Patent Text Reader

Abstract

The invention discloses a graphite composite material as well as a preparation method and application thereof, and relates to the technical field of lithium ion battery materials. The graphite composite material comprises an inner core and a carbon coating layer coating the surface of the inner core, wherein the inner core comprises modified graphite and nano silicon, the modified graphite comprises graphite and a carbon nano tube vertically growing on the surface of the graphite, and the graphite and the nano silicon are connected through the carbon nano tube. According to the graphite composite material disclosed by the invention, the vertically grown carbon nanotubes play a better connecting role between graphite and silicon carbon, and provide enough space for volume expansion of silicon; the coated and carbonized carbon shell also has a buffering effect on the volume expansion of silicon, so that a stable solid electrolyte interface is favorably formed, and the transmission of lithium ions is promoted; and the graphite composite material obviously improves the specific capacity, the rate capability and the cycle performance of the graphite negative electrode of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a graphite composite material and a preparation method and application thereof. Background Art

[0002] In modern society, fossil fuels such as oil, coal and natural gas play a great role as energy sources. However, fossil fuels have problems such as resource depletion and environmental pollution. At present, sustainable development has become a global consensus. The energy field will face a huge revolution, and new energy will gradually become the pillar of the energy field. Lithium-ion batteries have the advantages of high energy density, low self-discharge, no memory effect, wide temperature range, high rate charge and discharge, long life cycle, and green environmental protection. They are widely used in power, digital, communication, energy storage and other fields. The continuous improvement and development of lithium-ion batteries is crucial to explore advanced, cost-effective and eco-friendly energy conversion and storage methods.

[0003] At present, the negative electrode material of commercial lithium-ion batteries is mainly artificial graphite, with a theoretical specific capacity of 372mAh / g and limited improvement in energy density. The theoretical specific capacity of silicon-based materials is 4200mAh / g, which is much higher than that of graphite. In addition, it has obvious advantages such as environmental friendliness, high abundance of earth elements, and easy processing, and has attracted widespread attention. However, due to the expansion / contraction stress generated during the charging and discharging process, the silicon negative electrode material suffers from severe cracking, resulting in irreversible rapid capacity loss and low initial coulomb efficiency, and the practical application of silicon negative electrodes is hindered. Combining the advantages of silicon and artificial graphite to realize the preparation of a new type of material has become the development trend of lithium battery negative electrodes in the future.

[0004] CN103247802A discloses a graphite composite negative electrode material for lithium ion batteries and a preparation method thereof, wherein the graphite composite negative electrode material has a core-shell structure; wherein the core is graphite, and the shell is carbon nanotubes and / or carbon nanofibers uniformly distributed on the graphite surface and grown in situ. The preparation method comprises: using graphite as a raw material, fully soaking it with a solution containing a catalyst, drying it, and then introducing a carbon source under high temperature and a protective atmosphere for chemical vapor deposition to generate carbon nanotubes and / or carbon nanofibers. The preparation method requires high-temperature purification or acid purification, wherein high-temperature purification at 2000 to 3000°C greatly increases the cost, which is equivalent to the cost of another high-temperature graphitization; and acid treatment is unfavorable to the environment, and improper use of the acid solution may damage the structure and performance of the graphite and reduce its service life.

[0005] CN110858642A discloses a method for preparing a silicon / graphite / solid electrolyte composite negative electrode material. Silicon powder, graphite, binder, conductive agent (carbon nanotubes, carbon nanofibers, graphene, etc.), and solid electrolyte are mixed to prepare a dispersion, which is then spray granulated and dried; asphalt is then added for kneading and high-temperature sintering to obtain a silicon / graphite / solid electrolyte composite negative electrode material. The carbon nanotubes directly added in this preparation method may not be able to effectively combine with the base material, resulting in poor fixation on the surface of the material, affecting its application performance, and the directly added carbon nanotubes are often difficult to achieve uniform dispersion and are prone to agglomeration or aggregation, resulting in uneven material performance.

[0006] Therefore, it is urgent to develop a material and a preparation method thereof that can combine the advantages of silicon and artificial graphite, so as to further significantly improve the specific capacity, rate performance and cycle performance of the graphite negative electrode of lithium-ion batteries. Summary of the invention

[0007] The purpose of the present invention is to provide a graphite composite material and a preparation method and application thereof. The vertically grown carbon nanotubes of the graphite composite material play a better role in connecting graphite and silicon carbon, and provide sufficient space for the volume expansion of silicon; the carbonized carbon shell also has a buffering effect on the volume expansion of silicon, and can also effectively prevent the material from contacting with the electrolyte, reduce side reactions, help form a stable solid electrolyte interface (SEI), and promote the transmission of lithium ions; and the graphite composite material significantly improves the specific capacity, rate performance and cycle performance of the graphite negative electrode of the lithium ion battery.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a graphite composite material, the graphite composite material comprising a core and a carbon coating layer wrapped around the surface of the core;

[0010] The inner core includes modified graphite and nano-silicon, the modified graphite includes graphite and carbon nanotubes vertically grown on the surface of the graphite, and the graphite and nano-silicon are connected through the carbon nanotubes.

[0011] Preferably, the median particle size D50 of the modified graphite is 5 to 20 μm.

[0012] Preferably, the size of the nano-silicon is 1-100 nm.

[0013] Preferably, the carbon coating layer has a thickness of 1 to 100 nm.

[0014] Preferably, the carbon coating layer is amorphous carbon.

[0015] Preferably, the amorphous carbon is amorphous carbon formed after carbonization of pitch.

[0016] Preferably, the asphalt comprises 180 asphalt.

[0017] In a second aspect, the present invention provides a method for preparing the graphite composite material as described in the first aspect, the preparation method comprising the following steps:

[0018] Sodium nanoparticles are grown on the surface of graphite, and the sodium nanoparticles are used as catalysts to catalyze the in-situ growth of carbon nanotubes on the surface of the graphite to obtain modified graphite;

[0019] Combining the modified graphite with the nano-silicon to obtain a graphite-silicon composite material;

[0020] A carbon coating layer is formed on the surface of the graphite-silicon composite material to obtain the graphite composite material.

[0021] Preferably, the sodium nanoparticles are prepared by the following steps:

[0022] The graphite and the sodium salt solution are mixed and stirred, and then filtered and dried; the dried product is subjected to a reduction reaction to grow sodium nanoparticles on the surface of the graphite.

[0023] Preferably, the sodium salt is selected from sodium carbonate and / or sodium bicarbonate, preferably sodium carbonate.

[0024] Preferably, the mass ratio of the graphite to the sodium salt solution is (1-5):10.

[0025] Preferably, the concentration of the sodium salt solution is 2-6 mol / L.

[0026] Preferably, the stirring time is 1 to 20 hours.

[0027] Preferably, the drying time is 8 to 48 hours.

[0028] Preferably, the specific process of the reduction reaction is:

[0029] The dried product was heated in an Ar atmosphere and then heated in H 2 The sodium nanoparticles are reduced at a constant temperature in a mixed atmosphere of N, N, and Ar to obtain the sodium nanoparticles.

[0030] Preferably, during the heating process, the flow rate of Ar is 100-600 μmol / s.

[0031] Preferably, the heating rate is 2-10°C / min.

[0032] Preferably, in the mixed atmosphere, the H 2The flow rate ratio of Ar is (3-5):1, preferably 4:1.

[0033] Preferably, in the mixed atmosphere, the H 2 The flow rate is 100~600μmol / s.

[0034] Preferably, in the mixed atmosphere, the flow rate of Ar is 25-150 μmol / s.

[0035] Preferably, the temperature of the isothermal reduction is 400-550° C., and the time of the isothermal reduction is 1-5 hours.

[0036] Preferably, the carbon nanotubes are prepared by the following steps:

[0037] The graphite with sodium nanoparticles grown on the surface was placed in CO 2 and C 2 H 2 In a mixed atmosphere of , the sodium nanoparticles are used as a catalyst to catalyze the in-situ growth of carbon nanotubes on the surface of the graphite at a constant temperature to obtain modified graphite.

[0038] Preferably, the C 2 H 2 The volume percentage is 5-12%, preferably 8%.

[0039] Preferably, the CO 2 The flow rate is 10~50μmol / s.

[0040] Preferably, the C 2 H 2 The flow rate is 100~500μmol / s.

[0041] Preferably, the temperature of the in-situ growth is 400-550° C., and the time of the in-situ growth is 10-60 min.

[0042] Preferably, the graphite-silicon composite material is prepared by the following steps:

[0043] The modified graphite, nano silicon and a binder are mixed in water, and then granulated by spray drying to obtain the graphite-silicon composite material.

[0044] Preferably, the binder is selected from any one of polyacrylic acid, carboxymethyl cellulose, polyvinylidene fluoride or polyvinyl pyrrolidone, or a combination of at least two thereof.

[0045] Preferably, the mass ratio of the modified graphite, nano-silicon, binder and water is (6-10):(0.1-3):(0.005-0.2):(20-50).

[0046] Preferably, the mixing process is specifically as follows:

[0047] Firstly, a binder is added into water and stirred for 0.5 to 5 hours to make the binder completely dispersed in water, and then the modified graphite and nano silicon are added and stirred for 1 to 10 hours to obtain a slurry of graphite-silicon composite material.

[0048] Preferably, the inlet temperature of the spray drying is 200-300°C.

[0049] Preferably, the outlet temperature of the spray drying is between 100 and 120°C.

[0050] Preferably, the graphite composite material is prepared by the following steps:

[0051] The graphite-silicon composite material and asphalt are mixed and carbonized to form a carbon coating layer on the surface of the graphite-silicon composite material to obtain the graphite composite material.

[0052] Preferably, the mass ratio of the graphite-silicon composite material to asphalt is 100:(2-8).

[0053] Preferably, the carbonization temperature is 1100-1300° C., and the carbonization time is 4-24 hours.

[0054] In a third aspect, the present invention provides a use of the graphite composite material according to the first aspect in preparing a negative electrode material for a lithium ion battery.

[0055] In a fourth aspect, the present invention provides an electrode sheet, comprising the graphite composite material as described in the first aspect, or the graphite composite material prepared by the preparation method as described in the second aspect.

[0056] In a fifth aspect, the present invention provides a lithium-ion battery, comprising the graphite composite material as described in the first aspect, or the graphite composite material prepared by the preparation method as described in the second aspect, or the electrode sheet as described in the fourth aspect.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] (1) The present invention grows uniformly distributed carbon nanotubes in situ on the graphite surface and can control their vertical growth, which helps to enhance conductivity while providing a better connection between graphite and silicon and providing sufficient space for the volume expansion of silicon.

[0059] (2) The carbon shell after asphalt coating and carbonization of the present invention also has a buffering effect on the volume expansion of silicon, and can also effectively prevent the material from contacting the electrolyte, reduce side reactions, help form a stable solid electrolyte interface (SEI), and promote the transmission of lithium ions.

[0060] (3) In the present invention, under the action of high temperature carbonization, the Na nanoparticles in the material evaporate, thereby achieving effective removal of the metal and avoiding side reactions.

[0061] (4) When the present invention makes graphite into electrode sheets, gaps will remain after stacking due to differences in graphite size and shape, and silicon has poor conductivity, which reduces the conductivity of the electrode sheets. Carbon nanotubes help to enhance the conductivity of the material.

[0062] (5) The product of the present invention significantly improves the specific capacity, rate performance and cycle performance of the graphite negative electrode of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0064] Figure 1 It is a schematic diagram of the structure of the graphite composite material of the present invention.

[0065] Among them, 1 is graphite, 2 is carbon nanotube, 3 is nano silicon, and 4 is carbon coating layer. DETAILED DESCRIPTION

[0066] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0067] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0068] The prior art discloses that the expansion / contraction stress generated by the graphite / silicon composite material during the charge and discharge process leads to severe cracking of the silicon negative electrode material. The added carbon nanotubes improve this problem to a certain extent, but the directly doped carbon nanotubes have poor fixation on the surface of the material and are difficult to achieve uniform dispersion. They are prone to agglomeration, which affects their application performance.

[0069] In order to solve the above problems, the present invention adopts the following technical solutions:

[0070] First, as Figure 1 As shown, the present invention provides a graphite composite material, the graphite composite material comprises a core and a carbon coating layer 4 wrapped around the surface of the core;

[0071] The core includes modified graphite and nano-silicon 3 , the modified graphite includes graphite 1 and carbon nanotubes 2 vertically grown on the surface of the graphite, and the graphite 1 and nano-silicon 3 are connected through the carbon nanotubes 2 .

[0072] In the present invention, the carbon nanotubes are in-situ grown on the surface of the graphite, which can not only control its vertical growth, but also play a better connection role between graphite and silicon, and help to make graphite and a small amount of silicon composite to form the core of the graphite composite material, while enhancing the conductivity, it also provides enough space for the volume expansion of silicon, and the specific capacity, rate performance and cycle stability of the obtained modified graphite are significantly improved. In addition, the present invention further uses a carbon coating layer formed by carbonization to coat the composite core, and the carbon shell obtained after carbonization also has a buffering effect, reduces the volume expansion of silicon, and can also effectively prevent the material from contacting with the electrolyte, reduce side reactions, help form a stable solid electrolyte interface (SEI), and promote the transmission of lithium ions.

[0073] In an optional embodiment, the median particle size D50 of the modified graphite is 5 to 20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc.

[0074] In an optional embodiment, the size of the nano-silicon is 1 to 100 nm, for example, it can be 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, etc.

[0075] In an optional embodiment, the thickness of the carbon coating layer is 1 to 100 nm, for example, it can be 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, etc.

[0076] In an optional embodiment, the carbon coating layer is amorphous carbon.

[0077] In an optional embodiment, the amorphous carbon is amorphous carbon formed after carbonization of pitch.

[0078] In an alternative embodiment, the asphalt comprises 180 asphalt.

[0079] In a second aspect, the present invention provides a method for preparing the graphite composite material as described in the first aspect, the preparation method comprising the following steps:

[0080] Sodium nanoparticles are grown on the surface of graphite, and the sodium nanoparticles are used as catalysts to catalyze the in-situ growth of carbon nanotubes on the surface of the graphite to obtain modified graphite;

[0081] Combining the modified graphite with the nano-silicon to obtain a graphite-silicon composite material;

[0082] A carbon coating layer is formed on the surface of the graphite-silicon composite material to obtain the graphite composite material.

[0083] In the present invention, sodium nanoparticles are grown on the surface of graphite, and the sodium nanoparticles are used as catalysts to make the surface of the graphite catalyze the in-situ growth of carbon nanotubes, which well solves the problem that the carbon nanotubes have poor fixing ability and are difficult to disperse, so that the in-situ grown carbon nanotubes are evenly distributed, and their vertical growth can be controlled, which helps to enhance the conductivity. Further, the graphite and the nano-silicon are combined through the in-situ grown carbon nanotubes, which effectively improves the bonding ability of graphite and silicon, plays a better connection role between graphite and silicon, and also provides enough space for the volume expansion of silicon. Furthermore, a carbon coating layer is formed on the surface of the graphite-silicon composite material to reduce the volume expansion of silicon, and can also effectively prevent the material from contacting with the electrolyte, reduce side reactions, help to form a stable solid electrolyte interface (SEI), and promote the transmission of lithium ions. Most importantly, under the action of high temperature, the sodium nanoparticles in the material evaporate, thereby achieving effective removal of metals. The graphite composite material obtained by the preparation method of the present invention significantly improves the specific capacity and rate performance and cycle performance of the graphite negative electrode of the lithium ion battery.

[0084] In an optional embodiment, the sodium nanoparticles are prepared by the following steps:

[0085] The graphite and the sodium salt solution are mixed and stirred, and then filtered and dried; the dried product is subjected to a reduction reaction to grow sodium nanoparticles on the surface of the graphite.

[0086] In an optional embodiment, the sodium salt is selected from sodium carbonate and / or sodium bicarbonate, preferably sodium carbonate.

[0087] It should be noted that the graphite described in the present invention is ordinary artificial stone, that is, ordinary artificial graphite after processes such as crushing and graphitization.

[0088] It should be noted that the process of growing sodium nanoparticles on the surface of graphite can be carried out in a CVD furnace.

[0089] In an optional embodiment, the mass ratio of the graphite and the sodium salt solution is (1-5):10, for example, it can be 1:10, 1.5:10, 2:10, 2.5:10, 3:10, 3.5:10, 4:10, 4.5:10, 5:10, etc.

[0090] In an optional embodiment, the concentration of the sodium salt solution is 2-6 mol / L, for example, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, 5.5 mol / L, 6 mol / L, etc.

[0091] In an optional embodiment, the stirring time is 1 to 20 hours, for example, it can be 1 hour, 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, etc.

[0092] In an optional embodiment, the drying time is 8 to 48 hours, for example, it can be 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h, 36h, 38h, 40h, 42h, 44h, 46h, 48h, etc.

[0093] In an optional embodiment, the specific process of the reduction reaction is:

[0094] The dried product was heated in an Ar (argon) atmosphere and then in H 2 The sodium nanoparticles are obtained by isothermal reduction in a mixed atmosphere of hydrogen and Ar.

[0095] When the sodium salt is selected from sodium carbonate, the reaction formula of sodium (Na) nanoparticles grown on graphite is: Na 2 CO 3 +2C=2Na+3CO.

[0096] When the sodium salt is selected from sodium bicarbonate, the reaction formula of sodium (Na) nanoparticles grown on graphite is: 2NaHCO 3 =Na 2 CO 3 +CO 2 +H 2 O, further Na2 CO 3 +2C=2Na+3CO; can also be written as 2NaHCO 3 +2C=2Na+3CO+CO 2 +H 2 O.

[0097] In an optional embodiment, during the heating process, the flow rate of Ar is 100-600 μmol / s, for example, it can be 100 μmol / s, 150 μmol / s, 200 μmol / s, 250 μmol / s, 300 μmol / s, 350 μmol / s, 400 μmol / s, 450 μmol / s, 500 μmol / s, 550 μmol / s, 600 μmol / s, etc.

[0098] In an optional embodiment, the heating rate is 2 to 10°C / min, for example, it may be 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min, 10°C / min, etc.

[0099] In an optional embodiment, in the mixed atmosphere, the H 2 The flow rate ratio of Ar is (3-5):1, for example, it can be 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1, 5:1, etc.

[0100] In a preferred embodiment, in the mixed atmosphere, the H 2 The flow rate ratio of Ar and Ar is 4:1.

[0101] In an optional embodiment, in the mixed atmosphere, the H 2 The flow rate is 100-600 μmol / s, for example, it can be 100 μmol / s, 150 μmol / s, 200 μmol / s, 250 μmol / s, 300 μmol / s, 350 μmol / s, 400 μmol / s, 450 μmol / s, 500 μmol / s, 550 μmol / s, 600 μmol / s, etc.

[0102] In an optional embodiment, in the mixed atmosphere, the flow rate of Ar is 25 to 150 μmol / s, for example, it can be 25 μmol / s, 30 μmol / s, 40 μmol / s, 50 μmol / s, 55 μmol / s, 60 μmol / s, 80 μmol / s, 100 μmol / s, 120 μmol / s, 140 μmol / s, 150 μmol / s, etc.

[0103] In an optional embodiment, the temperature of the isothermal reduction is 400-550°C, for example, it can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 550°C, etc.

[0104] In an optional embodiment, the isothermal reduction time is 1 to 5 hours, for example, it can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, etc.

[0105] In an optional embodiment, the carbon nanotubes are prepared by the following steps:

[0106] The graphite with sodium nanoparticles grown on the surface was placed in CO 2 (carbon dioxide) and C 2 H 2 In a mixed atmosphere of sodium and acetylene, the sodium nanoparticles are used as a catalyst to catalyze the in-situ growth of carbon nanotubes on the surface of the graphite at a constant temperature to obtain modified graphite.

[0107] Among them, the reaction formula for obtaining modified graphite is: aC 2 H 2 + bNa=cNa x C y +dH 2 , x and y can be any value; if the reaction is not complete, the acetylene molecule C 2 H 2 One H on the acetylene molecule is replaced by Na; and when the reduction is complete, the acetylene molecule C 2 H 2 Both H in the above are replaced by Na, so Na x C y x and y in can be any value; for example, when x=y=8, "cNa x C y " can represent 4 completely reacted Na 2 C 2 When x=6 and y=8, it can represent two completely reacted Na 2 C 2 molecules and 2 incompletely reacted NaHC 2 , it should be noted that Na2 C 2 It is the final product obtained after complete molecular reduction.

[0108] In an optional embodiment, the volume percentage of acetylene is 5-12%, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, etc., preferably 8%.

[0109] It should be noted that C 2 H 2 The volume percentage refers to the concentration of acetylene itself, that is, CO 2 and C 2 H 2 Its volume percentage before becoming a mixed atmosphere.

[0110] In an optional embodiment, the CO 2 The flow rate is 10 to 50 μmol / s, for example, it can be 10 μmol / s, 15 μmol / s, 20 μmol / s, 25 μmol / s, 30 μmol / s, 35 μmol / s, 40 μmol / s, 45 μmol / s, 50 μmol / s, etc.

[0111] In an optional embodiment, the C 2 H 2 The flow rate is 100-500 μmol / s, for example, it can be 100 μmol / s, 150 μmol / s, 200 μmol / s, 250 μmol / s, 300 μmol / s, 350 μmol / s, 400 μmol / s, 450 μmol / s, 500 μmol / s, etc.

[0112] In an optional embodiment, the in-situ growth temperature is 400-550°C, for example, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 550°C, etc.

[0113] In an optional embodiment, the in situ growth time is 10 to 60 min, for example, it can be 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0114] In an optional embodiment, the graphite-silicon composite material is prepared by the following steps:

[0115] The modified graphite, nano silicon and a binder are mixed in water, and then granulated by spray drying to obtain the graphite-silicon composite material.

[0116] In an optional embodiment, the binder is selected from any one of polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF) or polyvinyl pyrrolidone (PVP), or a combination of at least two thereof.

[0117] In an optional embodiment, the mass ratio of the modified graphite, nano-silicon, binder and water is (6-10):(0.1-3):(0.005-0.2):(20-50);

[0118] Among them, the modified graphite "6-10" can be, for example, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, etc.;

[0119] Among them, nano silicon "0.1-3" can be, for example, 0.5, 0.8, 1, 1.2, 1.5, 2, 2.2, 2.5, 3, etc.;

[0120] Among them, the binder "0.005-0.2" can be, for example, 0.005, 0.006, 0.008, 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.12, 0.15, 0.2, etc.;

[0121] Here, the water "20-50" can be, for example, 20, 25, 30, 35, 40, 45, 50, etc.

[0122] In an optional embodiment, the mixing process is specifically as follows:

[0123] Firstly, a binder is added into water and stirred for 0.5 to 5 hours to make the binder completely dispersed in water, and then the modified graphite and nano silicon are added and stirred for 1 to 10 hours to obtain a slurry of graphite-silicon composite material.

[0124] In an optional embodiment, the stirring time after adding the binder is 0.5 to 5 hours, for example, it can be 0.5h, 0.6h, 0.8h, 1h, 1.2h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, etc.

[0125] In an optional embodiment, the stirring time after adding the modified graphite and the nano-silicon is 1 to 10 hours, for example, it can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, etc.

[0126] In an optional embodiment, the inlet temperature of the spray drying is 200-300°C, for example, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, etc.

[0127] In an optional embodiment, the outlet temperature of the spray drying is between 100 and 120°C, for example, 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C, 120°C, etc.

[0128] In an optional embodiment, the graphite composite material is prepared by the following steps:

[0129] The graphite-silicon composite material and asphalt are mixed and carbonized to form a carbon coating layer on the surface of the graphite-silicon composite material to obtain the graphite composite material.

[0130] In an optional embodiment, the mass ratio of the graphite-silicon composite material to asphalt is 100:(2-8);

[0131] In an optional embodiment, the carbonization temperature is 1100-1300°C, for example, it can be 1100°C, 1120°C, 1150°C, 1180°C, 1200°C, 1220°C, 1240°C, 1250°C, 1260°C, 1280°C, 1300°C, etc.

[0132] In an optional embodiment, the carbonization time is 4 to 24 hours, for example, it can be 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, etc.

[0133] In an optional embodiment, the carbonization further includes breaking up, screening and demagnetization in sequence.

[0134] As an optional embodiment of the present invention, the method for preparing the graphite composite material comprises the following steps:

[0135] S1. Preparation of sodium nanoparticles:

[0136] The graphite and sodium salt solution are mixed and stirred, and then filtered and dried; the dried product is first heated in an Ar atmosphere, and then heated in a H 2 and Ar mixed atmosphere for isothermal reduction to obtain graphite with sodium nanoparticles grown on the surface;

[0137] S2. Preparation of modified graphite:

[0138] The graphite with sodium nanoparticles grown on the surface was placed in CO 2 and C 2 H 2 In a mixed atmosphere of , using the sodium nanoparticles as a catalyst, catalyzing the in-situ growth of carbon nanotubes on the surface of the graphite at a constant temperature to obtain modified graphite;

[0139] S3. Preparation of graphite-silicon composite material:

[0140] The modified graphite, nano-silicon and a binder are mixed in water, and then granulated by spray drying to obtain the graphite-silicon composite material;

[0141] S4. Preparation of finished graphite composite materials:

[0142] The graphite-silicon composite material and asphalt are mixed and carbonized to form a carbon coating layer on the surface of the graphite-silicon composite material to obtain the graphite composite material.

[0143] More specifically, as an optional embodiment of the present invention, the method for preparing the graphite composite material comprises the following steps:

[0144] S1. Preparation of sodium nanoparticles:

[0145] Graphite and 2-6 mol / L sodium carbonate solution in a mass ratio of (1-5):10 are mixed and stirred, and then filtered and dried; the dried product is first heated to 400-550°C at a rate of 2-10°C / min in an Ar atmosphere, and then heated to 400-550°C in a H 2 and Ar in a mixed atmosphere at 400-550° C. for 1-5 hours to obtain graphite with sodium nanoparticles grown on the surface;

[0146] S2. Preparation of modified graphite:

[0147] The graphite with sodium nanoparticles grown on the surface was placed in CO 2 and C 2 H 2 In a mixed atmosphere of, using the sodium nanoparticles as a catalyst, catalyzing the in-situ growth of carbon nanotubes on the surface of the graphite at a constant temperature of 400 to 550° C. for 10 to 60 minutes to obtain modified graphite; wherein, CO 2 The flow rate is 10~50μmol / s, C 2 H 2 The flow rate is 100~500μmol / s.

[0148] S3. Preparation of graphite-silicon composite material:

[0149] The modified graphite, nano-silicon and a binder in a mass ratio of (6-10):(0.1-3):(0.005-0.2):(20-50) are mixed in water, and then granulated by spray drying to obtain the graphite-silicon composite material;

[0150] S4. Preparation of finished graphite composite materials:

[0151] A graphite-silicon composite material and asphalt in a mass ratio of 100:(2-8) are mixed, and carbonized at 1100-1300° C. for 4-24 hours to form a carbon coating layer on the surface of the graphite-silicon composite material to obtain the graphite composite material.

[0152] In a third aspect, the present invention provides a use of the graphite composite material as described in the first aspect in preparing a negative electrode material for a lithium ion battery.

[0153] In a fourth aspect, the present invention provides an electrode sheet, comprising the graphite composite material as described in the first aspect, or the graphite composite material prepared by the preparation method as described in the second aspect.

[0154] In a fifth aspect, the present invention provides a lithium-ion battery, comprising the graphite composite material as described in the first aspect, or the graphite composite material prepared by the preparation method as described in the second aspect, or the electrode sheet as described in the fourth aspect.

[0155] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0156] Example 1

[0157] This embodiment provides a graphite composite material, which is prepared by the following steps:

[0158] S1. Preparation of sodium nanoparticles:

[0159] Weigh 10kg of ordinary artificial graphite and put 30kg of Na with a concentration of 5mol / L into it. 2 CO 3 The solution was stirred at room temperature for 1.5 h; the product obtained by stirring was filtered and vacuum dried for 10 h to obtain dry surface-adherent Na 2 CO 3 of graphite;

[0160] Adhere Na to the surface 2 CO 3 The graphite was placed in a CVD furnace and heated at a rate of 5 °C / min and an Ar flow rate of 350 μmol / s. After heating to 500 °C, the Ar flow rate was adjusted to 70 μmol / s and H 2 The material was reduced at a flow rate of 280 μmol / s, and the isothermal reduction time was 2.5 h to obtain graphite with sodium nanoparticles grown on the surface.

[0161] S2. Preparation of modified graphite:

[0162] Close H 2 and Ar, CO is introduced into the CVD furnace 2 and 8% C2 H 2 Gas, CO 2 The flow rate was 22.5 μmol / s, 8% C 2 H 2 The flow rate was 225 μmol / s, the reaction time was 45 min, and modified graphite with a median particle size of 5 to 20 μm was obtained.

[0163] S3. Preparation of graphite-silicon composite material:

[0164] First, add the binder (PAA and CMC in a mass ratio of 4.5:1) into pure water and stir for 1.5 hours, then add the modified graphite and nano silicon (particle size of 1-20 nm) obtained by S2, and stir again for 2 hours to obtain a slurry; wherein the mass ratio of the modified graphite, nano silicon, binder and pure water is 9:1:0.06:30;

[0165] The slurry is spray-dried, wherein the spray-drying inlet temperature is 250° C. and the outlet temperature is 110° C., and the graphite-silicon composite material is obtained by spray-drying.

[0166] S4. Preparation of finished graphite composite materials:

[0167] The graphite-silicon composite material and 180 asphalt were mixed at a mass ratio of 100:4, and then carbonized in a roller kiln at 1150° C. for 15 hours, and then dispersed, screened, and demagnetized in sequence to obtain the finished graphite composite material.

[0168] Example 2

[0169] This embodiment provides a graphite composite material, which is prepared by the following steps:

[0170] S1. Preparation of sodium nanoparticles:

[0171] Weigh 10kg of ordinary artificial graphite and put 30kg of Na with a concentration of 5mol / L into it. 2 CO 3 The solution was stirred at room temperature for 1 hour; the product obtained by stirring was filtered and vacuum dried for 8 hours to obtain dry surface-adherent Na 2 CO 3 of graphite;

[0172] Adhere Na to the surface 2 CO 3 The graphite was placed in a CVD furnace and heated at a rate of 5°C / min and an Ar flow rate of 300 μmol / s. After heating to 500°C, the Ar flow rate was adjusted to 60 μmol / s and H 2The material was reduced at a flow rate of 240 μmol / s, and the isothermal reduction time was 2 h to obtain graphite with sodium nanoparticles grown on the surface.

[0173] S2. Preparation of modified graphite:

[0174] Close H 2 and Ar, CO is introduced into the CVD furnace 2 and 8% C 2 H 2 Gas, CO 2 The flow rate was 20 μmol / s, 8% C 2 H 2 The flow rate was 200 μmol / s, the reaction time was 30 min, and modified graphite with a median particle size of 5 to 20 μm was obtained.

[0175] S3. Preparation of graphite-silicon composite material:

[0176] First, add the binder (PAA and CMC in a mass ratio of 4:1) into pure water and stir for 1 hour, then add the modified graphite and nano silicon (particle size of 1-20 nm) obtained by S2, and stir again for 1 hour to obtain a slurry; wherein the mass ratio of the modified graphite, nano silicon, binder and pure water is 16:1:0.08:40;

[0177] The slurry is spray-dried, wherein the spray-drying inlet temperature is 240° C. and the outlet temperature is 105° C., and the graphite-silicon composite material is obtained by spray-drying.

[0178] S4. Preparation of finished graphite composite materials:

[0179] The graphite-silicon composite material and 180 asphalt are mixed at a mass ratio of 100:3, and then carbonized in a roller kiln at 1100° C. for 18 hours, and then broken up, screened, and demagnetized are performed in sequence to obtain the finished graphite composite material.

[0180] Example 3

[0181] This embodiment provides a graphite composite material, which is prepared by the following steps:

[0182] S1. Preparation of sodium nanoparticles:

[0183] Weigh 10kg of ordinary artificial graphite and put 30kg of Na with a concentration of 5mol / L into it. 2 CO 3 The solution was stirred at room temperature for 2 h; the product obtained by stirring was filtered and vacuum dried for 12 h to obtain dry surface-adherent Na 2 CO 3 of graphite;

[0184] Adhere Na to the surface 2 CO 3 The graphite was placed in a CVD furnace and heated at a rate of 5 °C / min and an Ar flow rate of 400 μmol / s. After heating to 500 °C, the Ar flow rate was adjusted to 80 μmol / s and H 2 The material was reduced at a flow rate of 320 μmol / s, and the isothermal reduction time was 3 h to obtain graphite with sodium nanoparticles grown on the surface.

[0185] S2. Preparation of modified graphite:

[0186] Close H 2 and Ar, CO is introduced into the CVD furnace 2 and 8% C 2 H 2 Gas, CO 2 The flow rate was 25 μmol / s, 8% C 2 H 2 The flow rate was 250 μmol / s, the reaction time was 60 min, and modified graphite with a median particle size of 5 to 20 μm was obtained.

[0187] S3. Preparation of graphite-silicon composite material:

[0188] First, add the binder (PAA and CMC in a mass ratio of 5:1) into pure water and stir for 2 hours, then add the modified graphite and nano silicon (particle size of 1 to 20 nm) obtained by S2, and stir again for 3 hours to obtain a slurry; wherein the mass ratio of the modified graphite, nano silicon, binder and pure water is 7:1:0.07:30;

[0189] The slurry is spray-dried, wherein the spray-drying inlet temperature is 260° C. and the outlet temperature is 115° C., and the graphite-silicon composite material is obtained by spray-drying.

[0190] S4. Preparation of finished graphite composite materials:

[0191] The graphite-silicon composite material and 180 asphalt are mixed at a mass ratio of 100:5, and then carbonized in a roller kiln at 1200° C. for 12 hours, and then broken up, screened, and demagnetized are performed in sequence to obtain the finished graphite composite material.

[0192] Example 4

[0193] This embodiment provides a graphite composite material, which is different from the embodiment 1 only in that Na 2 CO 3 The concentration of the solution was 1 mol / L, and the other steps were exactly the same as in Example 1.

[0194] Example 5

[0195] This embodiment provides a graphite composite material, which is different from the embodiment 1 in that 5 mol / L Na 2 CO 3 The solution was replaced with 5 mol / L NaHCO 3 The solution was replaced with, and the other steps were exactly the same as in Example 1.

[0196] Example 6

[0197] This embodiment provides a graphite composite material, which is different from Embodiment 1 only in that the isothermal reduction time in S1 is reduced to 0.2 h, and the other steps are completely consistent with Embodiment 1.

[0198] Example 7

[0199] This embodiment provides a graphite composite material, which is different from the embodiment 1 only in that CO in S2 2 The flow rate was reduced to 5 μmol / s, 8% C 2 H 2 The flow rate was reduced to 50 μmol / s, and the other steps were completely consistent with Example 1.

[0200] Example 8

[0201] This embodiment provides a graphite composite material, which is different from Embodiment 1 only in that the reaction time in S2 is reduced to 5 minutes, and the other steps are completely consistent with Embodiment 1.

[0202] Example 9

[0203] This embodiment provides a graphite composite material, which is different from the embodiment 1 only in that the reaction time in S2 is increased to 120 min, and the other steps are completely consistent with the embodiment 1.

[0204] Example 10

[0205] This embodiment provides a graphite composite material, which is different from Embodiment 1 only in that the ratio of modified graphite, nano-silicon, binder and pure water in S3 is 1:1:0.01:10, and the other steps are completely consistent with Embodiment 1.

[0206] Embodiment 11

[0207] This embodiment provides a graphite composite material, which is different from Embodiment 1 only in that the mass ratio of the graphite-silicon composite material to 180 asphalt in S4 is 100:1.5, and the other steps are completely consistent with Embodiment 1.

[0208] Example 12

[0209] This embodiment provides a graphite composite material, which is different from Embodiment 1 only in that the 180 asphalt in S4 is replaced by polyvinyl alcohol of the same mass, and the other steps are exactly the same as those in Embodiment 1.

[0210] Comparative Example 1

[0211] This comparative example provides a graphite composite material, which differs from Example 1 only in that H is not introduced into S1. 2 The material was reduced, and the other steps were exactly the same as in Example 1.

[0212] Comparative Example 2

[0213] This comparative example provides a graphite composite material, which is different from Example 1 only in that 8% C 2 H 2 The gas is reacted, and the other steps are exactly the same as those in Example 1.

[0214] Comparative Example 3

[0215] This comparative example provides a graphite composite material, which is different from Example 1 only in that no binder is added in S3, and the other steps are completely consistent with Example 1.

[0216] Comparative Example 4

[0217] This comparative example provides a graphite composite material, which is different from Example 1 only in that nano-silicon is not added to S3, and the other steps are completely consistent with Example 1.

[0218] Comparative Example 5

[0219] This comparative example provides a composite material, which is prepared by the following steps:

[0220] S1. Preparation of mixed slurry:

[0221] First, add the binder (PAA and CMC in a mass ratio of 4.5:1) into pure water and stir for 1.5 hours. Then add ordinary artificial graphite, single-walled carbon nanotubes and nano-silicon with a median particle size of 1 to 20 nm, and stir again for 2 hours to obtain the desired slurry; among which, the mass ratio of ordinary artificial graphite, single-walled carbon nanotubes, nano-silicon, binder and pure water is 9:2:1:0.06:30.

[0222] S2. Spray drying granulation

[0223] The slurry obtained in step S1 is spray dried, wherein the spray drying inlet temperature is 250° C. and the outlet temperature is 110° C. After spray drying, a graphite-silicon composite material is obtained.

[0224] S3. Preparation of finished composite materials:

[0225] The graphite-silicon composite material and 180 asphalt were mixed at a mass ratio of 100:4, and then carbonized in a roller kiln at 1150° C. for 15 hours, and then dispersed, screened, and demagnetized in sequence to obtain the finished graphite composite material.

[0226] Comparative Example 6

[0227] This comparative example provides a composite material, which is different from Example 1 only in that the Na 2 CO 3 The solution was replaced with an equal concentration of FeCl 3 solution, and the heating of S1 from 500°C to 950°C was changed, while other conditions remained unchanged.

[0228] Comparative Example 7

[0229] This comparative example provides a composite material, which is different from comparative example 6 only in that the prepared modified graphite A is acid-washed to remove the Fe metal catalyst, and then washed with water until the pH of the solution is between 6-7.

[0230] Test Example 1

[0231] Test samples: the graphite composite materials provided in Examples 1 to 12 and the composite materials provided in Comparative Examples 1 to 7.

[0232] Particle size (D50) testing instrument: Malvern, Master Size 3000.

[0233] The specific test results are shown in Table 1 below:

[0234] Table 1

[0235]

[0236]

[0237] As shown in Table 1, the D of the modified graphite prepared by S1 of the present invention 50 The graphite composite material S4 finally prepared has a D 50 It is 11.4~15.7μm.

[0238] Test Example 2

[0239] Test samples: the graphite composite materials provided in Examples 1 to 12 and the composite materials provided in Comparative Examples 1 to 7.

[0240] Test method: The prepared graphite negative electrode material is prepared into a pole piece, specifically:

[0241] The above samples were mixed with conductive carbon black (Surper P) and NMP (N-methylpyrrolidone) binder in a mass ratio of 96.5:1.5:2.0 to obtain a slurry, which was then coated on copper foil to form a negative electrode. The prepared negative electrode and lithium metal electrode were assembled into a lithium-ion button battery. LiPF 6 The electrolyte was dissolved in ethylene carbonate / diethyl carbonate / ethyl methyl carbonate = 2:3:1 at a concentration of 1 mol / L. After the button assembly was completed, the capacity, rate performance and cycle performance tests were performed, as shown below:

[0242] (a) 0.1C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min;

[0243] (b) 3C discharge specific capacity test steps: ① Stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ Stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ Stand for 5min; ⑦ 0.1C charge to 2V; ⑧ Stand for 5min; ⑨ 3C discharge to 0.005V, ⑩ stand for 30min; 0.1C discharge to 0.005V, stand for 30min; 0.05C discharge to 0.005V stand for 30min; 3C charge to 2V.

[0244] (c) 6C discharge specific capacity test steps: ① Stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ Stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ Stand for 5min; ⑦ 0.1C charge to 2V; ⑧ Stand for 5min; ⑨ 6C discharge to 0.005V, ⑩ stand for 30min; 0.1C discharge to 0.005V, stand for 30min; 0.05C discharge to 0.005V stand for 30min; 6C charge to 2V.

[0245] (d) 0.1C 300-cycle capacity retention rate test steps: Same as the 0.1C discharge specific capacity test steps, set the program to cycle 300 times before stopping, and compare its capacity retention rate.

[0246] Data processing: Select 4 data with a range within 3mAh, remove the maximum and minimum data and calculate the average.

[0247] The specific test results are shown in Table 2 below:

[0248] Table 2

[0249]

[0250]

[0251] As shown in Table 1, the specific capacity of the battery assembled with the negative electrode prepared from the graphite composite material of the present invention at 0.1C is 552-804 mAh / g, the 3C discharge capacity retention rate is 70.24-87.74%, the 6C discharge capacity retention rate is 50.23-71.56%, and the capacity retention rate at 0.1C and 300 cycles is 50.42-96.75%. Among them, Examples 1 to 3 are preferred embodiments of the present invention, and the specific capacity of the assembled battery at 0.1C can reach more than 600 mAh / g, the 3C discharge capacity retention rate is more than 85%, the 6C discharge capacity retention rate is more than 70%, and the capacity retention rate at 0.1C and 300 cycles is more than 95%.

[0252] From the comparison between Example 1 and Comparative Example 1, it can be seen that H is not introduced into S1. 2 The reduction is impossible, that is, the sodium nanoparticles cannot grow on the surface of the graphite, and then the carbon nanotubes cannot be catalyzed to grow on the surface of the graphite. In other words, the composite material does not have carbon nanotubes growing vertically on the surface of the graphite, and graphite and nano-silicon cannot be well connected. Therefore, it is not difficult to see that the battery prepared by the invention has a significant decrease in both specific capacity and capacity retention rate.

[0253] From the comparison between Example 1 and Comparative Example 2, it can be seen that 8% C is not introduced into S2. 2 H 2 Gas, so the following reaction cannot occur: aC 2 H 2 + bNa=cNa x C y +dH 2 That is to say, the composite material does not have carbon nanotubes that can connect silicon and graphite and grow vertically on the graphite surface. Therefore, it is not difficult to see that the battery prepared by the composite material has a significant decrease in both specific capacity and capacity retention rate.

[0254] From the comparison between Example 1 and Comparative Example 3, it can be seen that without adding a binder, the modified graphite and nano-silicon cannot be connected, that is, the graphite and nano-silicon cannot be connected through the carbon nanotubes. Therefore, although the performance is improved to a certain extent compared with Comparative Examples 1 and 2, the specific capacity and capacity retention rate of the battery prepared therefrom are still significantly reduced compared with Example 1.

[0255] From the comparison between Example 1 and Comparative Example 4, it can be seen that the absence of nano-silicon in the structure of the graphite composite material will result in a significant decrease in the specific capacity of the prepared battery.

[0256] From the comparison between Example 1 and Comparative Example 5, it can be seen that the directly added carbon nanotubes may not be able to effectively combine with the base material, resulting in poor fixation on the surface of the material, affecting its application performance, and the directly added carbon nanotubes are often difficult to achieve uniform dispersion and are prone to agglomeration or aggregation, resulting in uneven material performance. Therefore, it is not difficult to see that the battery prepared therefrom has a significant decrease in both specific capacity and capacity retention.

[0257] From the comparison between Example 1 and Comparative Example 6, it can be seen that the use of iron salt as a catalyst not only requires an increase in temperature to complete the reduction, but also the capacity retention rate of the battery prepared therefrom decreases significantly. From the comparison between Example 1 and Comparative Example 7, it can be seen that acid treatment is unfavorable to the environment, and improper use of acid solution may damage the structure and performance of graphite and reduce its service life.

[0258] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A graphite composite material, characterized in that: The graphite composite material comprises a core and a carbon coating layer wrapped on the surface of the core; The inner core includes modified graphite and nano-silicon, the modified graphite includes graphite and carbon nanotubes vertically grown on the surface of the graphite, and the graphite and nano-silicon are connected through the carbon nanotubes.

2. The graphite composite material according to claim 1, characterized in that The median particle size D50 of the modified graphite is 5 to 20 μm; And / or, the size of the nano-silicon is 1-100 nm.

3. The graphite composite material according to claim 1, characterized in that: The thickness of the carbon coating layer is 1 to 100 nm; Preferably, the carbon coating layer is amorphous carbon; Preferably, the amorphous carbon is amorphous carbon formed after carbonization of pitch; Preferably, the asphalt comprises 180 asphalt.

4. A method for preparing a graphite composite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: Sodium nanoparticles are grown on the surface of graphite, and the sodium nanoparticles are used as catalysts to catalyze the in-situ growth of carbon nanotubes on the surface of the graphite to obtain modified graphite; Combining the modified graphite with the nano-silicon to obtain a graphite-silicon composite material; A carbon coating layer is formed on the surface of the graphite-silicon composite material to obtain the graphite composite material.

5. The method for preparing the graphite composite material according to claim 4, characterized in that: The sodium nanoparticles are prepared by the following steps: The graphite and the sodium salt solution are mixed and stirred, and then filtered and dried; the dried product is subjected to a reduction reaction to grow sodium nanoparticles on the surface of the graphite; Preferably, the sodium salt is selected from sodium carbonate and / or sodium bicarbonate, preferably sodium carbonate; Preferably, the mass ratio of the graphite to the sodium salt solution is (1-5):10; Preferably, the concentration of the sodium salt solution is 2 to 6 mol / L; Preferably, the stirring time is 1 to 20 hours; Preferably, the drying time is 8 to 48 hours; Preferably, the specific process of the reduction reaction is: The dried product is first heated in an Ar atmosphere, and then is isothermally reduced in a mixed atmosphere of H2 and Ar to obtain the sodium nanoparticles; Preferably, during the heating process, the flow rate of Ar is 100 to 600 μmol / s; Preferably, the heating rate is 2 to 10°C / min; Preferably, in the mixed atmosphere, the flow rate ratio of H2 to Ar is (3-5):1, preferably 4:1; Preferably, in the mixed atmosphere, the flow rate of H2 is 100 to 600 μmol / s; Preferably, in the mixed atmosphere, the flow rate of Ar is 25 to 150 μmol / s; Preferably, the temperature of the isothermal reduction is 400-550° C., and the time of the isothermal reduction is 1-5 hours; Preferably, the carbon nanotubes are prepared by the following steps: Placing graphite with sodium nanoparticles grown on the surface in a mixed atmosphere of CO2 and C2H2, using the sodium nanoparticles as a catalyst, and catalyzing the in-situ growth of carbon nanotubes on the surface of the graphite at a constant temperature to obtain modified graphite; Preferably, the volume percentage of C2H2 is 5-12%, preferably 8%; Preferably, the flow rate of CO2 is 10 to 50 μmol / s; Preferably, the flow rate of C2H2 is 100-500 μmol / s; Preferably, the temperature of the in-situ growth is 400-550° C., and the time of the in-situ growth is 10-60 min.

6. The method for preparing the graphite composite material according to claim 4, characterized in that: The graphite-silicon composite material is prepared by the following steps: The modified graphite, nano-silicon and a binder are mixed in water, and then granulated by spray drying to obtain the graphite-silicon composite material; Preferably, the binder is selected from any one or a combination of at least two of polyacrylic acid, carboxymethyl cellulose, polyvinylidene fluoride or polyvinyl pyrrolidone; Preferably, the mass ratio of the modified graphite, nano-silicon, binder and water is (6-10):(0.1-3):(0.005-0.2):(20-50); Preferably, the mixing process is specifically as follows: First, a binder is added to water, and stirred for 0.5 to 5 hours to completely disperse the binder in water, and then the modified graphite and the nano-silicon are added, and stirred for 1 to 10 hours to obtain a slurry of a graphite-silicon composite material; Preferably, the inlet temperature of the spray drying is 200-300°C; Preferably, the outlet temperature of the spray drying is between 100 and 120°C.

7. The method for preparing the graphite composite material according to claim 4, characterized in that: The graphite composite material is prepared by the following steps: The graphite-silicon composite material and asphalt are mixed and carbonized to form a carbon coating layer on the surface of the graphite-silicon composite material to obtain the graphite composite material; Preferably, the mass ratio of the graphite-silicon composite material to asphalt is 100:(2-8); Preferably, the carbonization temperature is 1100-1300° C., and the carbonization time is 4-24 hours.

8. Use of the graphite composite material according to any one of claims 1 to 3 in preparing negative electrode materials for lithium-ion batteries.

9. An electrode sheet, characterized in that: The electrode sheet comprises the graphite composite material according to any one of claims 1 to 3, or the graphite composite material prepared by the preparation method according to any one of claims 4 to 7.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the graphite composite material according to any one of claims 1 to 3, or the graphite composite material prepared by the preparation method according to any one of claims 4 to 7, or the electrode sheet according to claim 9.