Modified polybenzimidazole proton exchange membrane as well as preparation method and application thereof

By complexing polybenzimidazole with transition metal halides to form a modified precursor, and cross-linking it under high temperature conditions, the problem of solvent residue and low cross-linking degree in the existing technology is solved, and the polybenzimidazole film is improved mechanical strength and battery performance.

CN118738431APending Publication Date: 2024-10-01SHAANXI COAL & CHEM TECH INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999820.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In existing polybenzimidazole proton exchange membranes, solvent volatilization and cross-linking reactions occur simultaneously during the cross-linking process, resulting in a low degree of cross-linking in the system and easy residual solvent, which affects the mechanical strength of the membrane and battery performance.

Method used

Polybenzimidazole is complexed with transition metal halides to form a modified precursor, and is mixed with a cross-linking agent to form a casting liquid under medium and low temperature conditions, and then perform a cross-linking reaction under high temperature conditions to ensure solvent evaporation and cross-linking. separate the linking reactions and increase the degree of cross-linking.

Benefits of technology

It effectively improves the mechanical strength and battery performance of the polybenzimidazole membrane, reduces solvent residue, and improves the practical application performance of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738431A_ABST
    Figure CN118738431A_ABST
Patent Text Reader

Abstract

The invention discloses a modified polybenzimidazole proton exchange membrane as well as a preparation method and application thereof, and belongs to the technical field of polymer and high-temperature fuel cell proton exchange membranes. The invention discloses a modified polybenzimidazole proton exchange membrane which is a proton membrane with a cross-linked structure formed by a modified polybenzimidazole precursor and a cross-linking agent, and the modified polybenzimidazole precursor is obtained by complexing polybenzimidazole and transition metal halide. A polybenzimidazole polymer and a transition metal halide salt generate a latent polybenzimidazole precursor, the precursor can reduce the activity of an imine group in an imidazole group in a cross-linking reaction, and the preparation of the structure realizes that a polybenzimidazole membrane casting solution is subjected to solvent evaporation to form a membrane under medium and low temperature conditions; then cross-linking reaction is carried out under a high-temperature condition, so that the problems that the system cross-linking degree is low and the solvent is easy to remain when solvent volatilization and cross-linking reaction are carried out at the same time in a cross-linking type polybenzimidazole film forming process are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer and high-temperature fuel cell proton exchange membranes, and specifically relates to a modified polybenzimidazole proton exchange membrane and a preparation method and application thereof. Background Art

[0002] High-temperature proton exchange membrane fuel cells (HTPEMFCs) have developed rapidly due to their high operating temperature, high catalyst tolerance to impurities such as CO, and simple water and heat management systems. As the core component of HTPEMFCs, high-temperature proton exchange membrane has an important impact on the operating temperature, performance, life and system cost of fuel cells. At present, anhydrous phosphoric acid system membrane represented by polybenzimidazole (PBI) is the type of high-temperature proton exchange membrane with the highest market recognition and the fastest industrialization process. However, after the polybenzimidazole membrane absorbs phosphoric acid, due to the plasticization of phosphoric acid, the membrane has a large swelling degree and a significant decrease in mechanical strength, which greatly affects the battery performance of the membrane. To address this problem, people choose the technical means of cross-linking modification to improve the mechanical strength of the proton membrane. However, in this modification process, the temperature range of cross-linking between traditional cross-linking agents and polybenzimidazole crosses or overlaps with the temperature range of solvent volatilization during membrane formation, which brings many problems to membrane formation. On the one hand, the presence of solvent will reduce the degree of cross-linking reaction, and the mechanical properties of the cross-linked membrane will be less improved and the swelling will still be large after absorbing phosphoric acid. On the other hand, as the cross-linking reaction proceeds, the difficulty of solvent volatilization can easily cause solvent residue in the membrane, and the residual solvent can easily cause performance degradation in the actual application of the battery. Therefore, the cross-linked polybenzimidazole proton membrane still has problems such as large swelling degree, low mechanical strength and poor battery performance. Summary of the invention

[0003] The purpose of the present invention is to provide a modified polybenzimidazole proton exchange membrane and a preparation method and application thereof, so as to solve the technical problems of low system crosslinking degree and easy solvent residue in the preparation process of the existing crosslinked polybenzimidazole proton exchange membrane.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] The present invention discloses a modified polybenzimidazole proton exchange membrane, wherein the modified polybenzimidazole proton exchange membrane is a proton membrane with a cross-linked structure formed by a modified polybenzimidazole precursor and a cross-linking agent;

[0006] The modified polybenzimidazole precursor is obtained by complexing polybenzimidazole with a transition metal halide.

[0007] Furthermore, the structural formula of the modified polybenzimidazole precursor is:

[0008]

[0009] Wherein, M is a transition metal atom, and X is a halogen atom;

[0010] The cross-linking agent is a compound that cross-links with the imine group of the imidazole structure.

[0011] The present invention also discloses a method for preparing the modified polybenzimidazole proton exchange membrane, comprising the following steps:

[0012] The polybenzimidazole solution is mixed with the transition metal halide solution to carry out a complexation reaction to obtain a modified polybenzimidazole precursor solution;

[0013] The modified polybenzimidazole precursor solution is mixed with a cross-linking agent, and stirred to obtain a film casting solution;

[0014] Casting the casting solution into a film, and then volatilizing the solvent to obtain a polybenzimidazole primary film; cross-linking the polybenzimidazole primary film to obtain a cross-linked polybenzimidazole film;

[0015] The cross-linked polybenzimidazole membrane is sequentially subjected to a transition metal ion removal treatment, a cross-linking treatment and a curing treatment to obtain a modified polybenzimidazole proton exchange membrane.

[0016] Furthermore, the preparation method of the polybenzimidazole solution is: dissolving polybenzimidazole in an organic solvent, stirring and fully dissolving the polybenzimidazole at 50-80° C. under the protection of an inert gas to obtain a polybenzimidazole solution with a mass fraction of 2%-4%;

[0017] The preparation method of the transition metal halide solution is: dissolving the transition metal halide in an organic solvent and stirring for 15-30 minutes to obtain the transition metal halide solution;

[0018] The temperature of the complex reaction is 50-80° C. and the time is 6-10 hours.

[0019] Further, the polybenzimidazole is one or both of mPBI and OPBI containing an ether bond; the chemical formula of the transition metal halide is MX2, wherein one of copper, nickel and cobalt, and X is one of chlorine and bromine;

[0020] The organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone;

[0021] The molar ratio of the polybenzimidazole to the transition metal halide is 1:(0.01-0.1).

[0022] Furthermore, the modified polybenzimidazole precursor solution is mixed with a cross-linking agent and mechanically stirred for 3-5 hours to obtain a casting solution;

[0023] Casting the casting solution into a film, and then volatilizing the solvent at 70-90°C;

[0024] Cross-linking the polybenzimidazole primary film at 130-160° C. for 10-20 minutes to obtain a cross-linked polybenzimidazole film;

[0025] The cross-linking agent is a small molecule compound or a macromolecular polymer; the small molecule compound and the macromolecular polymer both contain bifunctional or trifunctional epoxy groups.

[0026] Furthermore, the step of removing transition metal ions is: immersing the cross-linked polybenzimidazole membrane in deionized water at 40-50° C. for 4 hours, during which the water is changed every 1 hour.

[0027] Furthermore, the curing treatment temperature is 150-180° C. and the curing treatment time is 3 hours.

[0028] The invention also discloses a modified polybenzimidazole proton exchange membrane prepared by the preparation method. The thickness of the modified polybenzimidazole proton exchange membrane is 35-45 μm.

[0029] The invention also discloses the application of the modified polybenzimidazole proton exchange membrane in a high-temperature fuel cell.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The invention discloses a modified polybenzimidazole proton exchange membrane, which is a proton membrane with a cross-linked structure formed by a modified polybenzimidazole precursor and a cross-linking agent. The modified polybenzimidazole precursor is obtained by complexing polybenzimidazole with a transition metal halide. A latent polybenzimidazole precursor is generated by reacting a polybenzimidazole polymer with a transition metal halide salt. The precursor can reduce the activity of an imine group in an imidazole group in a cross-linking reaction, so that the polybenzimidazole is stable within a certain temperature range. The preparation of the structure realizes that a polybenzimidazole casting liquid is first volatilized by solvent under medium and low temperature conditions to form a film, and then a cross-linking reaction occurs under high temperature conditions, which effectively solves the problems of low system cross-linking degree and easy solvent residue when solvent volatilization and cross-linking reaction occur simultaneously in the film-forming process of the cross-linked polybenzimidazole. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a cross-sectional SEM image of the modified polybenzimidazole proton exchange membrane prepared by the present invention;

[0033] Figure 2 It is a data diagram of solubility test of film samples obtained in Examples and Comparative Examples;

[0034] Wherein: a-Example 1 is cross-linked at 70°C; b-Example 1 is cross-linked at 130°C; c-Comparative Example 1;

[0035] Figure 3 The dry film tensile strength data of the film samples obtained in the examples and comparative examples are shown in FIG.

[0036] Figure 4 The battery performance test data of the membrane samples obtained in the examples and comparative examples are shown. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0038] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0039] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0040] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0041] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0042] The present invention provides a modified polybenzimidazole proton exchange membrane for a high-temperature fuel cell. The modified polybenzimidazole proton exchange membrane is a proton membrane with a cross-linked structure formed by a polybenzimidazole precursor and a cross-linking agent. The modified polybenzimidazole precursor is obtained by complexing polybenzimidazole with a transition metal halide.

[0043] The structural formula of the modified polybenzimidazole precursor is:

[0044]

[0045] Wherein, M is a transition metal atom, and X is a halogen atom; the cross-linking agent is a compound cross-linked with the imine group of the imidazole structure, and the compound can be a small molecule or a macromolecular polymer, and is not easy to volatilize or decompose during the whole process.

[0046] The present invention also provides a method for preparing the modified polybenzimidazole proton exchange membrane, comprising the following steps:

[0047] Step 1: Preparation of modified polybenzimidazole precursor

[0048] Dissolve polybenzimidazole in an organic solvent, and stir to fully dissolve at 50-80° C. under the protection of an inert gas to obtain a polybenzimidazole solution with a mass fraction of 2-4%;

[0049] Dissolving a transition metal halide in an organic solvent and stirring at room temperature for 15-30 minutes to obtain a transition metal halide solution;

[0050] The transition metal halide solution is slowly added dropwise to the polybenzimidazole solution under stirring, and after the addition is completed, the complexation reaction is carried out at 50-70° C. for 6-10 hours;

[0051] After the reaction is completed, the solid by-products are filtered out, and the filtered solution components are distilled under reduced pressure to increase the solute mass fraction to 8-10%, thereby obtaining a modified polybenzimidazole precursor solution;

[0052] Step 2: Preparation of cross-linked polybenzimidazole membrane

[0053] The modified polybenzimidazole precursor solution and the crosslinking agent are mixed and mechanically stirred for 3-5 hours to ensure that the mixture is evenly mixed to obtain a viscous casting solution;

[0054] The casting solution is cast into a film in a casting machine, the solvent is first volatilized in a medium-low temperature drying oven for 20-30 minutes to obtain a polybenzimidazole primary film, and then cross-linked in a high-temperature drying oven for 10-20 minutes to obtain a cross-linked polybenzimidazole film;

[0055] Step 3: Preparation of dense modified polybenzimidazole proton exchange membrane

[0056] The cross-linked polybenzimidazole membrane was immersed in deionized water at 40-50°C for 4 hours, during which the water was changed every hour to remove transition metal ions;

[0057] The surface water is then wiped clean with dust-free paper, and the membrane is placed in an oven at 150-180° C. for cross-linking and curing for 3 hours. During the high-temperature treatment, the volume shrinkage of the membrane is controlled to be 10%-15%, thereby obtaining a modified polybenzimidazole proton exchange membrane.

[0058] Preferably, the chemical formula of the transition metal halide is MX2, wherein M is copper, nickel or cobalt, and X is chlorine or bromine.

[0059] Preferably, the organic solvent is one or more solvents selected from the group consisting of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.

[0060] Preferably, the molar ratio of polybenzimidazole to transition metal halide is 1:(0.01-0.1).

[0061] Preferably, the crosslinking agent is a small molecule compound or a macromolecular polymer containing a bifunctional or trifunctional epoxy group, and the epoxy resin preferably has a viscosity of 500-1200 mPa.s.

[0062] Preferably, the molar ratio of the crosslinking agent to the polybenzimidazole precursor is (0.01-0.1):1.

[0063] Preferably, the low temperature for solvent volatilization is 70-90°C, and the high temperature for cross-linking is 130-160°C.

[0064] Preferably, the obtained dense modified polybenzimidazole proton exchange membrane has a thickness of 35-45 microns.

[0065] The invention also discloses the application of the modified polybenzimidazole proton exchange membrane in a high-temperature fuel cell.

[0066] The present invention also discloses a method for testing the phosphoric acid doping amount of the modified polybenzimidazole proton exchange membrane:

[0067] In the step of immersing the polybenzimidazole proton exchange membrane dry film in phosphoric acid to obtain the polybenzimidazole proton exchange membrane wet film, 85% mass fraction phosphoric acid is used for immersion at 80-120° C. for 8h-12h, so that the cross-linked polybenzimidazole membrane material fully absorbs the phosphoric acid, and a polybenzimidazole proton exchange membrane wet film with a phosphoric acid doping amount of 350-450% can be obtained.

[0068] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0069] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples that do not specify specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples, unless otherwise specified, are conventional commercially available products, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0070] The performance rules of the films prepared from polybenzimidazoles of different structures by the method of the present invention are similar, and OPBI with relatively good solubility is taken as an example for comparison and verification.

[0071] Example 1

[0072] A method for preparing a modified polybenzimidazole proton exchange membrane comprises the following steps:

[0073] S1: 40 g (0.1 mol) of polybenzimidazole (OPBI) was dissolved in 960 g of N, N-dimethylacetamide, and fully dissolved at 50° C. under the protection of inert gas to obtain a polybenzimidazole solution with a mass fraction of 4%; 0.425 g (0.0025 mol) of CuCl2 was dissolved in 10 g of N, N-dimethylacetamide, and stirred at room temperature for 30 min to obtain a CuCl2 solution, and the CuCl2 solution was slowly added dropwise to the polybenzimidazole solution under stirring. After the addition was completed, the mixture was reacted at 60° C. for 8 hours, and then the solid by-products were removed by filtration. The solution components obtained by filtration were subjected to reduced pressure distillation to increase the solute content to 10%, and a modified polybenzimidazole precursor solution was obtained;

[0074] S2: The modified polybenzimidazole precursor solution obtained in S1 was mixed with 2g of epoxy resin, and mechanically stirred for 4 hours to obtain a viscous casting solution; the casting solution was cast into a film in a casting machine, the solvent was evaporated in a drying oven at 70°C for 30 minutes, and then cross-linked in a drying oven at 130°C for 20 minutes to obtain a cross-linked polybenzimidazole film;

[0075] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in deionized water at 40°C for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and then placed in an oven at 170°C for cross-linking and curing for 3 hours. During the high-temperature treatment, the volume shrinkage of the membrane is controlled to be 15%, thereby obtaining a dense modified polybenzimidazole proton exchange membrane.

[0076] Example 2

[0077] A method for preparing a modified polybenzimidazole proton exchange membrane comprises the following steps:

[0078] S1: 40 g (0.1 mol) of ether-bonded polybenzimidazole (OPBI) was dissolved in 960 g of N, N-dimethylacetamide, and fully dissolved at 50° C. under the protection of inert gas to obtain a polybenzimidazole solution with a mass fraction of 4%; 0.595 g (0.0025 mol) of CoCl26H2O was dissolved in 10 g of N, N-dimethylacetamide, and stirred at room temperature for 30 min to obtain a CoCl2 solution, and the CuCl2 solution was slowly added dropwise to the polybenzimidazole solution under stirring. After the addition was completed, the mixture was reacted at 80° C. for 8 hours, and then the solid by-products were removed by filtration. The solution components obtained by filtration were subjected to reduced pressure distillation to increase the solute content to 10%, and a modified polybenzimidazole precursor solution was obtained;

[0079] S2: The modified polybenzimidazole precursor solution obtained in S1 was mixed with 2g of epoxy resin, and mechanically stirred for 4 hours to obtain a viscous casting solution; the casting solution was cast into a film in a casting machine, the solvent was evaporated in a drying oven at 70°C for 30 minutes, and then cross-linked in a drying oven at 130°C for 20 minutes to obtain a cross-linked polybenzimidazole film;

[0080] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in deionized water at 40°C for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and then placed in an oven at 170°C for cross-linking and curing for 3 hours. During the high-temperature treatment, the volume shrinkage of the membrane is controlled to be 15%, thereby obtaining a dense modified polybenzimidazole proton exchange membrane.

[0081] Example 3

[0082] A method for preparing a modified polybenzimidazole proton exchange membrane comprises the following steps:

[0083] S1: mPBI is dissolved in N,N-dimethylformamide, and fully dissolved at 70°C under the protection of inert gas to obtain a polybenzimidazole solution with a mass fraction of 2%; CoCl2 solution is slowly added dropwise to the polybenzimidazole solution under stirring, and after the addition is completed, the mixture is reacted at 50°C for 6 hours, and then the solid by-products are filtered out, and the solute content of the filtered solution components is increased to 10% by vacuum distillation to obtain a modified polybenzimidazole precursor solution; wherein the molar ratio of the polybenzimidazole to the transition metal halide is 1:0.01;

[0084] S2: The modified polybenzimidazole precursor solution obtained in S1 was mixed with 2g of epoxy resin, and mechanically stirred for 3 hours to obtain a viscous casting solution; the casting solution was cast into a film in a casting machine, the solvent was evaporated in a drying oven at 90°C for 30 minutes, and then cross-linked in a drying oven at 160°C for 10 minutes to obtain a cross-linked polybenzimidazole film;

[0085] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in 50°C deionized water for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and then placed in a 150°C oven for cross-linking and curing for 3 hours. During the high-temperature treatment, the volume shrinkage of the membrane is controlled to be 15%, thereby obtaining a dense modified polybenzimidazole proton exchange membrane.

[0086] Example 4

[0087] A method for preparing a modified polybenzimidazole proton exchange membrane comprises the following steps:

[0088] S1: dissolving polybenzimidazole (OPBI) in dimethyl sulfoxide, and fully dissolving it at 50°C under the protection of inert gas to obtain a polybenzimidazole solution with a mass fraction of 3%; slowly dropping NiCl2 solution into the polybenzimidazole solution under stirring, reacting at 50°C for 10 hours after the dropping is completed, and then filtering to remove solid by-products, and increasing the solute content of the filtered solution components to 10% by vacuum distillation to obtain a modified polybenzimidazole precursor solution; wherein the molar ratio of the polybenzimidazole to the transition metal halide is 1:0.1;

[0089] S2: The modified polybenzimidazole precursor solution obtained in S1 was mixed with 2g of epoxy resin, and mechanically stirred for 5 hours to obtain a viscous casting solution; the casting solution was cast into a film in a casting machine, the solvent was evaporated in a drying oven at 70°C for 30 minutes, and then cross-linked in a drying oven at 130°C for 15 minutes to obtain a cross-linked polybenzimidazole film;

[0090] S3: The cross-linked polybenzimidazole membrane obtained in S2 is immersed in deionized water at 45°C for 4 hours, during which the water is changed every 1 hour. After removing the transition metal ions, the membrane surface is wiped clean with dust-free paper, and then placed in an oven at 150°C for cross-linking and curing for 3 hours. During the high-temperature treatment, the volume shrinkage of the membrane is controlled to be 15%, thereby obtaining a dense modified polybenzimidazole proton exchange membrane.

[0091] Comparative Example 1

[0092] S1: Dissolve 40 g (0.1 mol) (OPBI) in 360 g N,N-dimethylacetamide, and under the protection of inert gas, stir at 50-80° C. to fully dissolve to obtain a solution with a mass fraction of 10%.

[0093] S2: The polybenzimidazole solution obtained in S1 was mixed with 2g of epoxy resin and mechanically stirred for 4 hours; the casting solution was cast into a film in a casting machine, and the solvent was evaporated in a low-temperature drying oven at 70°C for 30 minutes to obtain a cross-linked polybenzimidazole film.

[0094] Comparative Example 2

[0095] The cross-linked film in Comparative Example 1 was placed in an oven at 170° C. for drying and cross-linking and curing for 3 hours. During the high temperature treatment, the volume shrinkage of the film was controlled to be 15%, thereby obtaining a dense cross-linked polybenzimidazole film.

[0096] The modified polybenzimidazole proton exchange membrane prepared in the embodiment of the present invention, taking Example 1 as an example, the cross-sectional SEM image of the sample membrane is as follows: Figure 1 As shown, it can be seen from the figure that except for the cracks caused by brittle fracture at the edge, there are no obvious pores in the middle part of the cross section, and the thickness is 35-45 microns.

[0097] The film sample of S2 in Example 1, which was subjected to solvent evaporation in a drying oven at 70°C for 30 minutes, and the film sample which was subjected to crosslinking in a drying oven at 130°C for 20 minutes, were sampled respectively, and the solubility test was conducted in N,N-dimethylacetamide with the sample of Comparative Example 1, and the film was dissolved by stirring at 60°C for 8 hours. Figure 2 As shown, it can be seen that after the solvent of S2 in Example 1 is volatilized in a drying oven at 70°C, the film is only slightly cross-linked, part of it is dissolved in the solvent, and part of it exists in the solvent in the form of small fragments. After S2 in Example 1 is cross-linked at 130°C, the film is completely insoluble in the solvent, and the film of comparative sample 1 is also insoluble in the solvent, indicating that the cross-linking reaction of the film in Example 1 is mainly carried out in the drying oven at 130°C, the precursor increases the temperature of the cross-linking reaction of polybenzimidazole, and the film of comparative example 1 has undergone cross-linking reaction during the process of drying the solvent at 70°C.

[0098] The dry film tensile strength, phosphoric acid absorption, tensile strength of the wet film after being soaked in phosphoric acid, and volume swelling rate of the samples in Example 1, Example 2 and Comparative Example 1 and Comparative Example 2 were tested. The test results are shown in Table 1. The dry film tensile strength is shown in Table 1. Figure 3 .

[0099] In Table 1, the phosphoric acid absorption amount = (mass of wet film after absorbing phosphoric acid - mass of dry film) / mass of dry film * 100%, and the volume swelling rate = (volume of wet film - volume of dry film) / volume of dry film * 100%.

[0100] Table 1 Performance test results of samples of Example 1, Example 2 and Comparative Example 1, Comparative Example 2

[0101]

[0102] As can be seen from Table 1, the tensile strength of the dry film and the wet film of Example 1 and Example 2 are not much different, but higher than that of Comparative Example 2. The phosphoric acid absorption and volume swelling rate are lower than those of Comparative Example 1, indicating that the degree of crosslinking of the films of Example 1 and Example 2 is higher than that of Comparative Example 1 and Comparative Example 2.

[0103] from Figure 3From the tensile strength of the dry film, it can be seen that the tensile strength of the dry films of Examples 1 and 2 is significantly higher than that of Comparative Example 1; the fracture deformation rates of Examples 1 and 2 are significantly lower than that of Comparative Example 1, indicating that the residual solvent molecules in the films of Examples 1 and 2 are very low or absent, while there are more non-volatile solvent molecules in the dry film of Comparative Example 1, and the solvent plays a plasticizing role in the film material, reducing the tensile strength of the film and increasing the fracture deformation rate. After Comparative Example 1 is cured at 170°C (i.e., Comparative Example 2), the solvent molecules evaporate, the tensile strength is improved, and the fracture deformation rate is reduced.

[0104] The sample membranes of Example 1, Example 2 and Comparative Example 1, Comparative Example 2 were subjected to battery performance tests. In the single-cell test, 0.3 L / min hydrogen and 0.5 L / min air were supplied without back pressure. The test temperature was 160°C. The carbon paper used was 060 type carbon paper produced by Toray. The platinum loadings of the cathode and anode were 0.6 mg / cm 2 , the results are as follows Figure 4 .Depend on Figure 4 It can be seen that the peak power density of the membrane electrode assembled by using the precursor technology to prepare the proton membrane (Example 1 and Example 2) is higher than that of the comparative example, which is 594 mW / cm 2 and 593mW / cm 2 , indicating that the proton membrane of the present invention has excellent performance in practical applications of batteries.

[0105] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A modified polybenzimidazole proton exchange membrane, characterized in that: The modified polybenzimidazole proton exchange membrane is a proton membrane with a cross-linked structure formed by a modified polybenzimidazole precursor and a cross-linking agent; The modified polybenzimidazole precursor is obtained by complexing polybenzimidazole with a transition metal halide.

2. A modified polybenzimidazole proton exchange membrane according to claim 1, characterized in that: The structural formula of the modified polybenzimidazole precursor is: Wherein, M is a transition metal atom, and X is a halogen atom; The cross-linking agent is a compound that cross-links with the imine group of the imidazole structure.

3. A method for preparing a modified polybenzimidazole proton exchange membrane as claimed in claim 1 or 2, characterized in that: The following steps are involved: The polybenzimidazole solution is mixed with the transition metal halide solution to carry out a complexation reaction to obtain a modified polybenzimidazole precursor solution; The modified polybenzimidazole precursor solution is mixed with a cross-linking agent, and stirred to obtain a film casting solution; Casting the casting solution into a film, and then volatilizing the solvent to obtain a polybenzimidazole primary film; cross-linking the polybenzimidazole primary film to obtain a cross-linked polybenzimidazole film; The cross-linked polybenzimidazole membrane is sequentially subjected to a transition metal ion removal treatment, a cross-linking treatment and a curing treatment to obtain a modified polybenzimidazole proton exchange membrane.

4. The method for preparing a modified polybenzimidazole proton exchange membrane according to claim 3, characterized in that: The preparation method of the polybenzimidazole solution is as follows: dissolving polybenzimidazole in an organic solvent, stirring and fully dissolving at 50-80° C. under the protection of an inert gas to obtain a polybenzimidazole solution with a mass fraction of 2%-4%; The preparation method of the transition metal halide solution is: dissolving the transition metal halide in an organic solvent and stirring for 15-30 minutes to obtain the transition metal halide solution; The temperature of the complex reaction is 50-80° C. and the time is 6-10 hours.

5. The method for preparing a modified polybenzimidazole proton exchange membrane according to claim 4, characterized in that: The polybenzimidazole is one or two of mPBI and OPBI containing an ether bond; the chemical formula of the transition metal halide is MX2, wherein X is one of copper, nickel and cobalt, and chlorine and bromine; The organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone; The molar ratio of the polybenzimidazole to the transition metal halide is 1:(0.01-0.1).

6. The method for preparing a modified polybenzimidazole proton exchange membrane according to claim 3, characterized in that: The modified polybenzimidazole precursor solution is mixed with a cross-linking agent and mechanically stirred for 3-5 hours to obtain a casting solution; Casting the casting solution into a film, and then volatilizing the solvent at 70-90°C; Cross-linking the polybenzimidazole primary film at 130-160° C. for 10-20 minutes to obtain a cross-linked polybenzimidazole film; The cross-linking agent is a small molecule compound or a macromolecular polymer; the small molecule compound and the macromolecular polymer both contain bifunctional or trifunctional epoxy groups.

7. The method for preparing a modified polybenzimidazole proton exchange membrane according to claim 3, characterized in that: The process of removing transition metal ions is as follows: the cross-linked polybenzimidazole membrane is immersed in deionized water at 40-50° C. for 4 hours, during which the water is changed every 1 hour.

8. The method for preparing a modified polybenzimidazole proton exchange membrane according to claim 3, characterized in that: The temperature of the curing treatment is 150-180° C.; the time of the curing treatment is 3 hours.

9. A modified polybenzimidazole proton exchange membrane, characterized in that: The thickness of the modified polybenzimidazole proton exchange membrane is 35-45 μm.