Preparation method of electrolyte ceramic membrane for solid oxide battery
Through dry sintering process and multiple sintering stacking technology, the problems of toxic solvent use and high sintering temperature in the preparation of electrolyte ceramic membranes are solved, efficient and low-energy consumption electrolyte ceramic membrane preparation is achieved, the process flow is simplified and the production efficiency is improved. .
Patent Information
- Application Number
- CN202410739734.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-07
AI Technical Summary
The existing electrolyte ceramic membrane preparation process has problems such as the use of toxic organic solvents, long sintering time, high sintering temperature, cumbersome process flow, and low efficiency, resulting in long production cycles, low yields, unfriendly environment, and high energy consumption.
The dry sintering process is adopted, and through high-speed shear mixing, hot rolling treatment, hot isostatic pressing treatment and multiple sintering stacks, the use of organic solvents is avoided, the process flow is simplified, the powder packing density and sintering efficiency are improved, and the sintering efficiency is reduced. the sintering temperature.
The use of non-toxic organic solvents is realized, the green body preparation time is shortened, the powder packing density is increased, the sintering temperature and energy consumption are reduced, the process flow is simplified, and the production efficiency and the quality of the electrolyte ceramic membrane are improved.
Smart Images

Figure CN118738482A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field, and in particular to a method for preparing an electrolyte ceramic membrane for a solid oxide battery. Background Art
[0002] Solid oxide cells (SOCs) are solid ceramic devices that have the dual functions of solid oxide electrolyzers (SOECs) and solid oxide fuel cells (SOFCs). SOECs store renewable solar and wind energy in hydrogen fuel; SOFCs convert the chemical energy of fuels such as hydrogen, natural gas and other hydrocarbons into electrical energy. According to the type of support, SOCs can be divided into four categories: metal-supported, cathode-supported, electrolyte-supported and anode-supported. Among them, electrolyte-supported SOCs have attracted extensive attention and research due to their good resistance to thermal cycling and oxidation-reduction. The electrolyte support mainly uses sintered ceramic membranes such as yttria-stabilized zirconia (YSZ) and scandium-stabilized zirconia (ScSZ). The basic structure of electrolyte-supported SOCs is: cathode / electrolyte ceramic membrane / anode, in which electrolyte-supported SOCs are generally obtained by printing cathode and anode slurries on both sides of the prepared electrolyte ceramic membrane and then sintering.
[0003] Most electrolyte ceramic membranes used in electrolyte-supported SOCs in the industry are prepared by tape casting and sintering, such as the tape casting and sintering methods disclosed in Patent Nos. CN200510121311.4, CN202010544090.6, and CN202311347983.1. All of them go through processes such as tape casting slurry preparation, tape casting molding, green body drying and low-temperature debinding, and the slurry making process uses toxic organic solvents. There are problems such as long production cycle, low yield, complex process, unfriendly environment, and the use of a large amount of binders and plasticizers in the tape casting green body, which makes the powder particles have low packing density, resulting in higher sintering temperature and increased energy consumption.
[0004] Therefore, it is of great significance to develop a method for preparing an efficient and low-consumption electrolyte ceramic membrane for solid oxide batteries. Summary of the invention
[0005] The task of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing an electrolyte ceramic membrane for a solid oxide battery, which can prevent the electrolyte green body from sintering shrinkage deformation and green body shrinkage causing scratches, and can also reduce the sintering temperature, increase production efficiency, simplify the process flow of the electrolyte ceramic membrane and avoid the use of toxic organic solvents, which is environmentally friendly.
[0006] The task of the present invention is accomplished by the following technical solutions:
[0007] The preparation method of electrolyte ceramic membrane for solid oxide battery adopts dry sintering process without using organic solvent to solve the problems of using toxic organic solvent, long sintering time, high sintering temperature, complicated process flow and low efficiency in preparing electrolyte ceramic membrane by tape casting sintering method. The specific process steps and conditions are as follows:
[0008] S1. The electrolyte powder and the fiberizable binder are placed in a mixing device for high-speed shear mixing to form a binder fiberized and uniformly mixed with the electrolyte powder to form a binder - electrolyte powder mixture;
[0009] S2. The binder-electrolyte powder mixture is subjected to hot roller pressing to a set thickness to obtain an electrolyte green body;
[0010] S3. The electrolyte green body is sandwiched in a roughening medium and sealed and then hot isostatically pressed to obtain an electrolyte green body having a certain surface roughness and then cut into green sheets of a desired size;
[0011] S4. After the electrolyte green body and the primary sintering auxiliary material are stacked, debinding and primary sintering are performed to obtain a primary sintered electrolyte ceramic membrane;
[0012] S5. stacking the primary sintered electrolyte ceramic membrane and the secondary sintered auxiliary material and then performing secondary sintering to obtain a secondary sintered electrolyte ceramic membrane with good flatness.
[0013] Compared with the prior art, the present invention has the following advantages or effects:
[0014] (1) Because the dry sintering process provided by the present invention does not require the use of organic solvents to prepare the casting slurry, nor does it require the use of additives such as dispersants and plasticizers, the amount of organic matter used is reduced, the harm of toxic organic solvents to the environment and human body is avoided, the time consumption of the debinding stage is reduced, the green body preparation process is greatly simplified, and the green body preparation time is shortened;
[0015] (2) At the same time, due to the dry preparation, the powders are stacked more tightly, and the mass of powder in the electrolyte green body increases by 25-29%. The packing density of powder particles in the green body is increased, which is beneficial to reduce the temperature of mass transfer between powder particles and the sintering temperature, thus saving energy and reducing consumption;
[0016] (3) In addition, since the electrolyte green body is subjected to hot isostatic hydrostatic treatment to increase the surface roughness of the green body, the green body stacking and non-sticking, sintering efficiency and space utilization are improved;
[0017] (4) In addition, since the properties of the ceramic membrane are not changed, the physical and chemical properties remain basically the same.
[0018] In conclusion, the present invention can not only simplify the process of producing the electrolyte ceramic membrane, but also improve the production efficiency.
[0019] The % in this application document refers to mass percentage. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The present invention is a schematic diagram of a process flow of a method for preparing an electrolyte ceramic membrane for a solid oxide battery.
[0021] Figure 2 It is a schematic diagram of the one-time sintering stacking structure of the present invention.
[0022] Figure 3 It is a schematic diagram of the secondary sintering stacking structure of the present invention.
[0023] Figure 4 It is a physical schematic diagram of the electrolyte ceramic membrane after shaping of the present invention.
[0024] Figure 5 It is a schematic diagram of a cross-sectional SEM image of the electrolyte ceramic membrane after shaping according to the present invention.
[0025] The symbols in the accompanying drawings represent:
[0026] 1. Ballast plate 2. Sintered gasket 3. Electrolyte green body stack 4. Alumina support plate 10. Ballast plate 20. Sintered gasket 30. Primary sintered electrolyte ceramic membrane stack The present invention is further described in detail below with reference to the accompanying drawings. DETAILED DESCRIPTION
[0027] Reference Figures 1 to 5 , a method for preparing electrolyte ceramic membranes for solid oxide batteries, in order to solve the problems of using toxic organic solvents, long sintering time, high sintering temperature, complicated process flow and low efficiency in preparing electrolyte ceramic membranes by tape casting sintering, a dry sintering process without using organic solvents is adopted, and the specific process steps and conditions are as follows:
[0028] S1. The electrolyte powder and the fiberizable binder are placed in a mixing device for high-speed shear mixing to form a binder fiberized and uniformly mixed with the electrolyte powder to form a binder - electrolyte powder mixture;
[0029] S2. The binder-electrolyte powder mixture is subjected to hot roller pressing to a set thickness to obtain an electrolyte green body;
[0030] S3. The electrolyte green body is sandwiched in a roughening medium and sealed and then hot isostatically pressed to obtain an electrolyte green body having a certain surface roughness and then cut into green sheets of a desired size;
[0031] S4. After the electrolyte green body and the primary sintering auxiliary material are stacked, debinding and primary sintering are performed to obtain a primary sintered electrolyte ceramic membrane;
[0032] S5. stacking the primary sintered electrolyte ceramic membrane and the secondary sintered auxiliary material and then performing secondary sintering to obtain a secondary sintered electrolyte ceramic membrane with good flatness.
[0033] The specific process steps and conditions of the present invention can further be
[0034] The electrolyte powder is (Y2O3) 0.08 (ZrO2) 0.92 (8YSZ), (Sc2O3) 0.10 (CeO2) 0.01 (ZrO2) 0.89 (ScSZ), Ce 1-x G x O 2-x / 2 (GDC), Ce 1-x Sm x O 2-x / 2 (SDC), La 1-x Sr x Ga 1-y Mg y O 3-δ (LSGM) and BaCe 1-x- y Zr x M y O 3-δ At least one of (M=In, Y, Gd, Sm).
[0035] The fiberizable binder is at least one of polytetrafluoroethylene, polyimide, polyvinylidene fluoride, styrene-butadiene rubber and carboxymethyl cellulose.
[0036] In the step S1, the content of the fiberizable binder is 0.1-10%, and the content of the electrolyte powder mixture is 90-99.9%.
[0037] The binder and electrolyte mixing equipment in step S1 is at least one of a jet mill, a ball mill, a pulverizer, a screw extruder and an open mixer.
[0038] The hot rolling treatment in step S2 is performed by using an electric roller machine for multiple hot rolling treatments, and the temperature of the hot rolling treatment is 30-100°C.
[0039] In the step S2, the thickness of the electrolyte green body is set to be 30-250 μm.
[0040] In step S3, the roughening medium is at least one of emulsified glass, sulfuric acid paper, stainless steel plate and frosted acrylic plate, and the surface roughness of the roughening medium is 0.5-1.2 μm.
[0041] The isostatic pressing method in step S3 is hot isostatic water pressing or mold pressing, the hot isostatic pressing treatment pressure is 30-100 MPa, the temperature is 30-100° C., and the holding time is 20-100 min.
[0042] In the step S4 , the electrolyte green body and primary sintering auxiliary material stacking structure comprises a weight sheet 1 , a sintering gasket 2 , an electrolyte green body stack 3 , and an alumina support plate 4 .
[0043] In the step S4, the weight plate 1 is at least one of a porous aluminum oxide plate, a porous zirconium oxide plate, and a porous magnesium oxide plate, and weighs 0.3-0.9 kg.
[0044] The sintered gasket 2 in step S4 is (Y2O3) 0.03 (ZrO2) 0.97 At least one of a (3YSZ) green body, a cerium oxide green body, and a lanthanum gallate green body.
[0045] In step S4, the electrolyte green body stack 3 contains 1 to 20 electrolyte green bodies.
[0046] In the step S4, the debinding temperature of the electrolyte green body is 250-400°C, the debinding temperature insulation time is 1-5h, the primary sintering temperature is 1000-1500°C, and the primary sintering temperature insulation time is 1-8h; the heating rate from room temperature to the debinding temperature section is 0.1-1°C / min, and the heating rate from the debinding temperature to the primary sintering temperature section is 1-10°C / min.
[0047] The stacked structure of the primary sintered electrolyte ceramic membrane and the secondary sintered auxiliary materials in step S5 includes a weight plate 10 , a sintered gasket 20 , a primary sintered electrolyte ceramic membrane stack 30 and an alumina support plate 4 .
[0048] In the step S5, the weight plate 10 is at least one of a silicon carbide plate, a zirconium oxide plate, a magnesium oxide plate and an aluminum oxide plate, and has a weight of 1.0-5.0 kg.
[0049] The sintered gasket 20 in step S5 is a ceramic sheet obtained by sintering the sintered gasket 2 in step S4 once, and is at least one of a 3YSZ ceramic sheet, a cerium oxide ceramic sheet, and a lanthanum gallate ceramic sheet.
[0050] In the step S5, the stack 30 of once-sintered electrolyte ceramic membranes contains 10 to 30 pieces of once-sintered electrolyte ceramic membranes.
[0051] The temperature of the secondary sintering in step S5 is 10-30° C. higher than the temperature of the primary sintering; the secondary sintering temperature holding time is 1-5 hours, and the heating rate is 1-10° C. / min.
[0052] In the following examples, the ScSZ powder used was purchased from Jiangxi Saici, with a D50 of 0.5 μm and a specific surface area of 9-12 m 2 / g; the 3YSZ powder and 8YSZ powder used were purchased from Shenzhen Kejing, with a D50 of 0.5±0.2μm and a specific surface area of 12±2m 2 / g; the PTFE powder used was purchased from Shenzhen Kejing, with a D50 of 500 μm.
[0053] Example 1
[0054] Preparation of ScSZ electrolyte ceramic membrane
[0055] S1: ScSZ powder and PTFE powder were weighed in a mass ratio of 95:5, placed in a crusher for high-speed shear mixing, so that the PTFE powder was fiberized and fully mixed with the ScSZ powder to obtain a fiberized PTFE-ScSZ mixture; the crusher speed was 3000 rpm, and the mixing time was 20 min.
[0056] S2: The fiberized PTFE-ScSZ mixture is placed in an electric roller mill for multiple hot rolling treatments, and the roller spacing is gradually reduced so that the thickness of the electrolyte green body is finally maintained at 65 μm; the temperature of the hot rolling treatment is 70°C.
[0057] S3: The ScSZ electrolyte green body was sandwiched between two sheets of sulfuric acid paper, placed in a PET bag, vacuum-sealed, and placed in an isostatic hydraulic press for isostatic pressing to obtain a surface-roughened ScSZ electrolyte green body; the hydrostatic pressure was 80 MPa, and the holding time was 30 min.
[0058] S4: The surface roughened ScSZ electrolyte green body and the primary sintering auxiliary materials are sintered as follows: Figure 2 The structure stack shown is, from bottom to top, an alumina support plate, a 3YSZ green body, 10 surface roughened ScSZ electrolyte green bodies, a 3YSZ green body, and a 0.6 mm porous alumina ceramic sheet, which are then placed in a muffle furnace for debinding and sintering; the debinding temperature is 300 ° C, the debinding time is 2 hours, the heating rate from room temperature to debinding temperature is 0.5 ° C / min, the primary sintering temperature is 1220 ° C, the holding time is 2 hours, and the debinding temperature and sintering temperature heating rate is 5 ° C / min; after cooling, the ScSZ primary sintered ceramic membrane is obtained. The 3YSZ green body is prepared by S1 and S2 steps, except that 3YSZ powder is used instead of 8YSZ powder.
[0059] S5: The primary sintered ScSZ ceramic film and the secondary sintered auxiliary materials are mixed as follows: Figure 3The structure stack shown in the figure is, from bottom to top, an alumina support plate, a 3YSZ ceramic sheet, 20 pieces of once-sintered ScSZ ceramic membranes, a 3YSZ ceramic sheet, and a 0.7 kg silicon carbide weight plate, which are then placed in a muffle furnace; the 3YSZ ceramic sheet is sintered in step S3, the secondary sintering temperature is 1240°C, the holding time is 2h, and the heating rate is 5°C / min; after cooling, the following is obtained: Figure 4 ScSZ ceramic film shown.
[0060] Example 2
[0061] Preparation of ScSZ electrolyte ceramic membrane
[0062] The difference from Example 1 is that the mass ratio of ScSZ powder to PTFE powder is 97:3, and the thickness of the ScSZ electrolyte green body is 115 μm.
[0063] Example 3
[0064] Preparation of 8YSZ electrolyte ceramic membrane
[0065] The difference from Example 1 is that the electrolyte powder is 8YSZ powder, the primary sintering temperature of the 8YSZ green body is 1320°C, and the secondary sintering temperature is 1340°C.
[0066] Example 4
[0067] Preparation of 8YSZ electrolyte ceramic membrane
[0068] The difference from Example 3 is that the mass ratio of 8YSZ powder to PTFE powder is 97:3, and the thickness of the ScSZ electrolyte green body is 115 μm.
[0069] Comparative Example 1
[0070] Preparation of ScSZ ceramic membrane by conventional tape casting sintering method
[0071] S1: Weigh xylene: ethanol: fish oil: ScSZ powder: BBP: PAG: PVB: cyclohexanone in a mass ratio of 21:21:1.5:49:1.6:1.6:4.1:0.2; first place xylene, ethanol, fish oil and ScSZ powder in a zirconia ball mill and ball mill at 800 rpm for 24 hours, then add BBP, PAG, PVB and cyclohexanone and continue to ball mill at 800 rpm for 16 hours; use a degassing machine to perform negative pressure degassing on the slurry for 60 minutes to obtain a casting slurry.
[0072] S2: Use a wire rod coater to scrape the slurry obtained in S1 onto a PET film. The green body thickness is controlled at 65 μm. The cast green body is dried at room temperature for 12 h.
[0073] S3: The ScSZ tape-cast green body is subjected to isostatic hydrostatic pressure treatment. Except that the green body is dried at 120° C. for 120 min before hydrostatic pressure treatment, the remaining steps are the same as step S3 in Example 1.
[0074] S4: performing laminate sintering on the surface roughened ScSZ green body. Except that the debinding temperature is changed to 400°C, the debinding time is changed to 6 hours, and the primary sintering temperature is changed to 1350°C, the remaining steps are the same as step S4 in Example 1.
[0075] S5: High-temperature shaping of the primary sintered ScSZ ceramic film. Except for the secondary sintering temperature being changed to 1370° C., the remaining steps are the same as step S5 in Example 1.
[0076] Comparative Example 2
[0077] Preparation of ScSZ ceramic membrane by conventional tape casting sintering method
[0078] The difference from Comparative Example 1 is that the mass ratio of ScSZ powder to PTFE powder is 97:3, and the thickness of the ScSZ electrolyte green body is 115 μm.
[0079] Comparative Example 3
[0080] Preparation of 8YSZ ceramic membrane by conventional tape casting and sintering method
[0081] The difference from Comparative Example 1 is that the electrolyte powder is 8YSZ powder, the primary sintering temperature of the 8YSZ tape-cast green body is 1430°C, and the secondary sintering temperature is 1450°C.
[0082] Comparative Example 4
[0083] Preparation of 8YSZ ceramic membrane by conventional tape casting and sintering method
[0084] The difference from Comparative Example 3 is that the mass ratio of 8YSZ powder to PTFE powder is 97:3, and the thickness of the 8YSZ electrolyte green body is 115 μm.
[0085] Performance characterization of embodiments and comparative examples:
[0086] The thickness was measured using a micrometer; the relative density was measured using the Archimedes drainage method; the fracture strength of the electrolyte ceramic membrane was measured using a universal testing machine; and the ionic conductivity of the electrolyte ceramic membrane at 800°C was measured using an electrochemical workstation in conjunction with a high-temperature tube furnace.
[0087] The surface and cross section of the electrolyte ceramic membrane were characterized by SEM. The cross section SEM of the electrolyte ceramic membrane of Example 1 is as follows: Figure 5 shown.
[0088] The characterization results of the electrolyte ceramic membranes of Examples 1 to 4 and Comparative Examples 1 to 4 are summarized in Table 1.
[0089] Table 1 Characterization data of electrolyte ceramic membrane
[0090]
[0091] Results and evaluation:
[0092] like Figure 4 As shown, the ScSZ ceramic film prepared in Example 1 has good flatness and no obvious defects on the surface. Figure 5 As shown, the cross-sectional SEM image of the ScSZ ceramic membrane prepared in Example 1 shows that the ceramic is transgranular fractured, the grains are in close contact, there are no obvious pores, and the ScSZ ceramic membrane has a dense structure. As shown in Table 1, the relative density, fracture strength and ionic conductivity at 800°C of the electrolyte ceramic membrane prepared in the example are not significantly different from those of the sample prepared in the comparative example. This shows that the dry sintering process provided by the present invention is suitable for the preparation of electrolyte ceramic membranes, and can obtain dense, high ionic conductivity, and high fracture strength electrolyte ceramic membranes.
[0093] As described above, the present invention can be better implemented. The above embodiments are only the best implementation methods of the present invention, but the implementation methods of the present invention are not limited by the above embodiments. Other changes, modifications, replacements, combinations, and simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an electrolyte ceramic membrane for a solid oxide battery, which aims to solve the problems of using toxic organic solvents, long sintering time, high sintering temperature, complicated process flow and low efficiency in preparing electrolyte ceramic membrane by tape casting sintering method. The method is characterized in that The dry sintering process without using organic solvents is adopted. The specific process steps and conditions are as follows: S1. The electrolyte powder and the fiberizable binder are placed in a mixing device for high-speed shear mixing to form a binder fiberized and uniformly mixed with the electrolyte powder to form a binder - electrolyte powder mixture; S2. The binder-electrolyte powder mixture is subjected to hot roller pressing to a set thickness to obtain an electrolyte green body; S3. The electrolyte green body is sandwiched in a roughening medium and sealed and then hot isostatically pressed to obtain an electrolyte green body having a certain surface roughness and then cut into green sheets of a desired size; S4. After the electrolyte green body and the primary sintering auxiliary material are stacked, debinding and primary sintering are performed to obtain a primary sintered electrolyte ceramic membrane; S5. stacking the primary sintered electrolyte ceramic membrane and the secondary sintered auxiliary material and then performing secondary sintering to obtain a secondary sintered electrolyte ceramic membrane with good flatness.
2. The preparation method according to claim 1, characterized in that The electrolyte powder is (Y2O3) 0.08 (ZrO2) 0.92 (8YSZ), (Sc2O3) 0.10 (CeO2) 0.01 (ZrO2) 0.89 (ScSZ), Ce 1-x G x O 2-x / 2 (GDC), Ce 1-x Sm x O 2-x / 2 (SDC), La 1-x Sr x Ga 1-y Mg y O 3-δ (LSGM) and BaCe 1-x-y Zr x M y O 3-δ At least one of (M=In, Y, Gd, Sm).
3. The preparation method according to claim 1, characterized in that The fiberizable binder is at least one of polytetrafluoroethylene, polyimide, polyvinylidene fluoride, styrene-butadiene rubber and carboxymethyl cellulose.
4. The preparation method according to claim 1, characterized in that In the step S1, the content of the fiberizable binder is 0.1-10%, and the content of the electrolyte powder mixture is 90-99.9%.
5. The preparation method according to claim 1 or 4, characterized in that The binder and electrolyte mixing equipment in step S1 is at least one of a jet mill, a ball mill, a pulverizer, a screw extruder and an open mixer.
6. The preparation method according to claim 1, characterized in that The hot rolling treatment in step S2 is performed by using an electric roller machine for multiple hot rolling treatments, and the temperature of the hot rolling treatment is 30-100°C.
7. The preparation method according to claim 1 or 6, characterized in that In the step S2, the thickness of the electrolyte green body is set to be 30-250 μm.
8. The preparation method according to claim 1, characterized in that In step S3, the roughening medium is at least one of emulsified glass, sulfuric acid paper, stainless steel plate and frosted acrylic plate, and the surface roughness of the roughening medium is 0.5-1.2 μm.
9. The preparation method according to claim 1 or 8, characterized in that The isostatic pressing method in step S3 is hot isostatic water pressing or mold pressing, the hot isostatic pressing treatment pressure is 30-100 MPa, the temperature is 30-100° C., and the holding time is 20-100 min.
10. The preparation method according to claim 1, characterized in that The electrolyte green body and primary sintering auxiliary material stacking structure in step S4 comprises a weight plate (1), a sintering gasket (2), an electrolyte green body stack (3), and an alumina support plate (4).
11. The preparation method according to claim 10, characterized in that The weight plate (1) in step S4 is at least one of a porous aluminum oxide plate, a porous zirconium oxide plate, and a porous magnesium oxide plate, and has a weight of 0.3-0.9 kg.
12. The preparation method according to claim 10, characterized in that The sintered gasket (2) in step S4 is (Y2O3) 0.03 (ZrO2) 0.97 At least one of a (3YSZ) green body, a cerium oxide green body, and a lanthanum gallate green body.
13. The preparation method according to claim 10, characterized in that In step S4, the electrolyte green body stack (3) contains 1 to 20 electrolyte green bodies.
14. The preparation method according to claim 1 or 10 or 11 or 12 or 13, characterized in that In the step S4, the debinding temperature of the electrolyte green body is 250-400°C, the debinding temperature insulation time is 1-5h, the primary sintering temperature is 1000-1500°C, and the primary sintering temperature insulation time is 1-8h; the heating rate from room temperature to the debinding temperature section is 0.1-1°C / min, and the heating rate from the debinding temperature to the primary sintering temperature section is 1-10°C / min.
15. The preparation method according to claim 1, characterized in that The stacked structure of the primary sintered electrolyte ceramic membrane and the secondary sintered auxiliary materials in step S5 comprises a weight plate (10), a sintered gasket (20), a primary sintered electrolyte ceramic membrane stack (30) and an alumina support plate (4).
16. The preparation method according to claim 15, characterized in that The weight plate (10) in step S5 is at least one of a silicon carbide plate, a zirconium oxide plate, a magnesium oxide plate and an aluminum oxide plate, and has a weight of 1.0 to 5.0 kg.
17. The preparation method according to claim 15, characterized in that The sintered gasket (20) in step S5 is a ceramic sheet obtained after the sintered gasket (2) in step S4 is sintered once, and is at least one of a 3YSZ ceramic sheet, a cerium oxide ceramic sheet, and a lanthanum gallate ceramic sheet.
18. The preparation method according to claim 15, characterized in that In the step S5, the stack (30) of once-sintered electrolyte ceramic membranes contains 10 to 30 pieces of once-sintered electrolyte ceramic membranes.
19. The preparation method according to claim 1 or 15 or 16 or 17 or 18, characterized in that The temperature of the secondary sintering in step S5 is 10-30° C. higher than the temperature of the primary sintering; the secondary sintering temperature holding time is 1-5 hours, and the heating rate is 1-10° C. / min.
Citation Information
Patent Citations
YSZ electrolyte preparation material, casting sheet, preparation method and gas sensor
CN111761686A
Preparation method of solid electrolyte cast film
CN117417187A
Preparation method of solid oxide fuel battery electrolyte diaphram
CN1794486A
Dry preparation process of solid electrolyte
CN113880577A
Zirconia ceramic stacking and sintering method
CN116573933A
Cited By
Ceramic solid-state electrolyte film flattening method
WO2025246002A1