Method for manufacturing cell stack

By applying a specific load cycle to the storage unit of the battery stack, the return property of the non-aqueous electrolyte is ensured, which solves the problem of reduced constraint load of the battery stack under low temperature and low SOC conditions, and achieves stable constraint on the battery stack.

CN118738501APending Publication Date: 2024-10-01PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410283747.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Under the low-temperature and low-SOC conditions of the battery stack, the thickness of the storage unit becomes smaller, resulting in a lower restraint load and the inability to fully restrain the battery stack, and the existing technology fails to effectively study the return property of non-aqueous electrolytes.

Method used

By applying a load in the thickness direction of the storage unit and cyclically reducing the load, it is ensured that the thickness variation of the unit reaches more than 0.3%, ensuring that the non-aqueous electrolyte can return to the wound electrode body again, increasing the thickness of the electrode body, thereby maintaining sufficient load constraints. .

Benefits of technology

It effectively suppresses the reduction of the constraint load of the battery stack, ensures that the power storage unit is fully constrained under low temperature and low SOC conditions, and improves the stability of the battery stack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738501A_ABST
    Figure CN118738501A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a cell stack capable of suitably controlling the thickness of a power storage cell and suppressing a reduction in the constraint load of the cell stack. The technology disclosed herein is a method for manufacturing a cell stack including a plurality of power storage cells, in which a load is applied up to 0.1 MPa at a speed of 0.1 mm / min in the thickness direction of the power storage cells prepared thereby, and the power storage cells prepared in the preparation step are subjected to a load applying process for applying a load up to 0.1 MPa at a speed of 0.1 mm / min in the thickness direction of the power storage cells prepared in the preparation step, and the load is applied up to 0.1 MPa at a speed of 0.1 mm / min in the thickness direction of the power storage cells prepared in the preparation step. A process in which a load is applied up to 0.1 MPa at a speed of 0.1 mm / min in the thickness direction of the electricity storage unit and the load is reduced up to 0.01 MPa at a speed of 0.1 mm / min after the application is performed is performed as one cycle, and the process is performed for five cycles. The relationship between the thickness X1 of the power storage cell with respect to the surface pressure of 0.04 MPa in the pressure-side F-s curve of the first cycle and the thickness X5 of the power storage cell with respect to the surface pressure of 0.04 MPa in the pressure-side F-s curve of the fifth cycle satisfies the following expression: (X1-X5) / X1 * 100 > = 0.3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method of manufacturing a battery stack. Background Art

[0002] In recent years, a battery stack with multiple power storage units is suitable for use as a driving power source for vehicles such as hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), and electric vehicles (BEV). As a related prior art document, Japanese Patent Publication No. 2018-055806 can be cited. In Patent Document 1, a technology related to a non-aqueous electrolyte secondary battery (power storage unit) is disclosed, which has an electrode body including a housing, a non-aqueous electrolyte (non-aqueous electrolyte) and a positive electrode, a negative electrode, and a separator, and the electrode body also includes a low spring constant membrane having a spring constant (second spring constant) lower than the spring constant (first spring constant) of the negative electrode, thereby suppressing the extrusion of the non-aqueous electrolyte inside the electrode body accompanied by the expansion and contraction of the electrode body. So far, the battery stack has been used by stacking the power storage units and applying load constraints.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Publication No. 2018-055806 Summary of the invention

[0006] Problems to be solved by the invention

[0007] When the battery stack is in use, if the low temperature and low SOC (State of Charge) conditions are reached, the thickness of the storage cell becomes smaller. When the battery stack is in this state, the non-aqueous electrolyte extruded from the storage cell to the outside of the electrode body returns to the electrode body again, and the thickness of the storage cell becomes larger again, maintaining the constraint load of the battery stack. However, in the case where the non-aqueous electrolyte in the storage cell is difficult to return to the electrode body, the constraint load of the battery stack is reduced because the thickness of the storage cell is still small, and the storage cell cannot be fully constrained. Therefore, in the manufacture of the battery stack, it is necessary to consider not only the extrusion of the non-aqueous electrolyte of the storage cell, but also the easy return of the non-aqueous electrolyte. In this regard, in the above-mentioned Japanese Patent Publication No. 2018-055806, the easy return of the non-aqueous electrolyte to the inside of the electrode body is not studied, and the above-mentioned technology has room for improvement.

[0008] The technology disclosed herein has been accomplished in view of the above-mentioned actual situation, and its main purpose is to relate to a method for manufacturing a battery stack that can appropriately control the thickness of the power storage cells stacked in the battery stack and suppress a reduction in the restraint load of the battery stack.

[0009] Means for solving problems

[0010] The technology disclosed herein is a method for manufacturing a battery stack including a plurality of square storage cells, comprising: a preparation step of preparing the storage cells, wherein the storage cells include a flat-shaped wound electrode body in which a positive electrode and a negative electrode are stacked and wound via a separator, a non-aqueous electrolyte, and a shell for accommodating the wound electrode body and the non-aqueous electrolyte; and a stacking step of stacking a plurality of the storage cells along the thickness direction of the storage cells. Here, it is characterized in that, for the storage battery cell prepared in the preparation process, a load is applied to the storage battery cell in the thickness direction of the storage battery cell at a speed of 0.1 mm / min until it reaches 0.1 MPa, and after the application, the load is reduced to 0.01 MPa at a speed of 0.1 mm / min as one cycle, and when this treatment is performed for 5 cycles, the relationship between the storage battery cell thickness X1 relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the first cycle and the storage battery cell thickness X5 relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the fifth cycle satisfies the following formula: (X1-X5) / X1×100≥0.3.

[0011] The storage cell prepared in the preparation step is a storage cell that satisfies the above formula. In the storage cell having this structure, there is a thickness difference for the non-aqueous electrolyte extruded to the outside of the wound electrode body in the stacking step to return to the inside of the wound electrode body. Therefore, the thickness of the wound electrode body increases by re-accommodating the non-aqueous electrolyte in the storage cell, and the thickness of the storage cell increases. Therefore, the reduction of the load applied to the storage cell is suppressed, and in the battery stack, a sufficient load can be maintained on the storage cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a perspective view schematically showing a battery stack according to one embodiment.

[0013] Figure 2 A perspective view of a power storage unit.

[0014] Figure 3 For along Figure 2 Schematic longitudinal cross-sectional view along line III-III.

[0015] Figure 4 This is a perspective view schematically showing a wound electrode body attached to a sealing plate.

[0016] Figure 5 It is a perspective view schematically showing a wound electrode body.

[0017] Figure 6 Schematic diagram showing the structure of a wound electrode body.

[0018] Figure 7This is a flowchart showing a method for manufacturing a battery stack according to one embodiment.

[0019] Figure 8 This is an example of an Fs curve obtained in the preparation step in one embodiment.

[0020] Fig. 9 Schematic diagrams for explaining the thickness change of a wound electrode body according to one embodiment. (a) shows the wound electrode body before the battery stack is constrained, (b) shows the wound electrode body when the battery stack is constrained, and (c) shows the wound electrode body when the nonaqueous electrolyte returns to the wound electrode body.

[0021] Fig.10 This is a schematic diagram for explaining the measurement of the cell thickness variation in the preparation process.

[0022] Fig.11 This is a flowchart showing a method for manufacturing a power storage unit according to an embodiment.

[0023] Fig.12 This is a graph plotting the change in cell thickness under the same load between the first cycle and the fifth cycle on the horizontal axis as Δcell thickness (mm) and the applied load (kN) on the vertical axis for Examples 1 and 2 and Comparative Example 2.

[0024] Fig.13 Schematic diagrams for explaining the thickness change of the wound electrode body according to the prior art. (a) shows the wound electrode body before the battery stack is constrained, (b) shows the wound electrode body when the battery stack is constrained, and (c) shows the wound electrode body when the non-aqueous electrolyte returns to the wound electrode body.

[0025] Fig.14 This is an example of an Fs curve according to a conventional example. DETAILED DESCRIPTION

[0026] Several preferred embodiments of the battery stack disclosed herein are described below with reference to the accompanying drawings as appropriate. Matters other than those specifically mentioned in this specification, i.e., matters required for the implementation of the present disclosure (e.g., the general structure and manufacturing process of the storage unit that is not a feature of the present disclosure) can be understood as design matters for those skilled in the art based on the prior art in this field. The battery stack disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in this field.

[0027] It should be noted that in the following drawings, the same reference numerals are used for components and parts that play the same role, and repeated descriptions are sometimes omitted or simplified. In addition, the notation "A to B" indicating a range in this specification includes the meaning of greater than A and less than B, and also includes the meaning of "preferably greater than A" and "preferably smaller than B".

[0028] Figure 1 The figure is a three-dimensional diagram schematically showing a battery stack 500 involved in one embodiment. The battery stack 500 includes a plurality of storage cells 100 and a restraint mechanism 300. In addition, for the convenience of explanation, although not shown here, the plurality of storage cells 100 of the battery stack 500 are electrically connected by a busbar. It should be noted that in the following description, the reference numerals L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the reference numerals X, Y, and Z in the drawings represent the short side direction (thickness direction) of the storage cell 100, the long side direction (width direction) orthogonal to the short side direction, and the up and down direction. The short side direction X is also the arrangement direction of the storage cell 100. However, these are just directions for the convenience of explanation, and there is no limitation on the setting form of the battery stack 500.

[0029] The restraint mechanism 300 is configured to apply a predetermined restraint pressure to the plurality of storage cells 100 in the thickness direction X. The restraint mechanism 300 is composed of a pair of end plates 310, a pair of side plates 320, and a plurality of screws 330. The pair of end plates 310 are arranged in a predetermined thickness direction X. The pair of end plates 310 are arranged at both ends of the battery stack 500 in the thickness direction X. The plurality of storage cells 100 are arranged between the pair of end plates 310 along the thickness direction X. An insulating sheet, an inter-cell separator, etc. may be arranged between the plurality of storage cells 100.

[0030] A pair of side plates 320 bridges a pair of end plates 310. The pair of side plates 320 are fixed to the end plates 310 by a plurality of screws 330 while applying a load to the plurality of storage cells 100, for example. Thus, a restraining load is applied to the plurality of storage cells 100 from the thickness direction X, and the battery stack 500 is held integrally. However, the restraining mechanism is not limited thereto. For example, the restraining mechanism 300 may be provided with a plurality of restraining belts, connecting rods, etc. instead of the side plates 320.

[0031] <Power Storage Unit 100>

[0032] In this specification, the term "power storage unit" refers to a device that can be repeatedly charged and discharged. Power storage units include lithium polymer batteries, lithium ion capacitors, etc., in addition to batteries generally referred to as lithium ion batteries and lithium secondary batteries. A so-called secondary battery generally refers to a battery that can be repeatedly charged and discharged with the movement of charge carriers between the positive and negative electrodes. Here, as one form of a power storage unit, a lithium ion secondary battery can be exemplified.

[0033] Figure 2 1 is a perspective view of the power storage unit 100. Figure 1 , Figure 2 As shown, the plurality of power storage cells 100 are arranged in the thickness direction X such that first side walls 12 b described later face each other. Figure 3 For along Figure 2 Schematic longitudinal cross-sectional view of line III-III. Figure 3 As shown, the power storage unit 100 includes a case 10, a wound electrode body 20, a non-aqueous electrolyte (not shown), a positive electrode terminal 30, a negative electrode terminal 40, a positive electrode collector 50, and a negative electrode collector 60. The power storage unit 100 is a lithium ion secondary battery.

[0034] The housing 10 is a box that accommodates the wound electrode body 20 and the non-aqueous electrolyte. Figure 2 As shown in FIG. 1 , the housing 10 has a flat rectangular parallelepiped (square) shape with a bottom. The material of the housing 10 can be the same as the material used in the past, and there is no particular limitation. The housing 10 is preferably made of metal, for example, more preferably made of aluminum, aluminum alloy, iron, iron alloy, etc. Figure 2 As shown, the housing 10 includes an outer body 12 having an opening 12h and a sealing plate (lid) 14 that seals the opening 12h. As in the present embodiment, the housing 10 preferably includes an outer body 12 having an opening 12h and a sealing plate 14 that seals the opening 12h.

[0035] The outer body 12 is as follows Figure 2 As shown, it includes: a bottom 12a, a pair of first side walls 12b extending from the bottom 12a and facing each other, and a pair of second side walls 12c extending from the bottom 12a and facing each other. The bottom 12a is roughly rectangular. The bottom 12a is opposite to the opening 12h. The first side wall 12b is flat. The first side wall 12b extends from the long side of the bottom 12a. The second side wall 12c extends from the short side of the bottom 12a. When viewed from above, the area of ​​the first side wall 12b is larger than the area of ​​the second side wall 12c. There is no particular limitation on the size of the outer body 12. For example, it is preferably 300 to 330 mm in width (long side direction Y), 100 to 130 mm in height (up and down direction Z), and 30 to 50 mm in thickness (short side direction X).

[0036] The sealing plate 14 is mounted on the outer body 12 in such a manner as to plug the opening 12h of the outer body 12. The sealing plate 14 is opposite to the bottom 12a of the outer body 12. The sealing plate 14 is substantially rectangular when viewed from above. The housing 10 is integrated by joining the sealing plate 14 to the periphery of the opening 12h of the outer body 12 (preferably by welding). The housing 10 is hermetically sealed (sealed).

[0037] like Figure 3As shown, the sealing plate 14 is provided with a liquid injection hole 15, a discharge valve 17 and two terminal lead holes 18, 19. The liquid injection hole 15 is used to inject the non-aqueous electrolyte after the sealing plate 14 is installed on the outer body 12. The liquid injection hole 15 is sealed with a sealing member 16. The discharge valve 17 is configured to break when the pressure in the shell 10 becomes above a specified value to discharge the gas in the shell 10 to the outside. The terminal lead holes 18, 19 penetrate the sealing plate 14 in the up and down direction Z. The terminal lead holes 18, 19 each have an inner diameter of a size that can be inserted through the positive terminal 30 and the negative terminal 40 before being installed on the sealing plate 14 (before riveting).

[0038] The non-aqueous electrolyte can be the same as before and is not particularly limited. The non-aqueous electrolyte contains a non-aqueous solvent and a supporting salt (electrolyte salt). The non-aqueous electrolyte may further contain additives as needed. The non-aqueous solvent includes carbonates such as ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The non-aqueous solvent preferably includes carbonates. In particular, it is preferred to include cyclic carbonates and chain carbonates. The supporting salt is, for example, a fluorine-containing lithium salt such as lithium hexafluorophosphate (LiPF6). As additives that can be contained in the non-aqueous electrolyte, for example, a film former, a gas generator, a dispersant, a thickener, etc. can be used. As a film former, for example, carbonate compounds such as vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), chloroethylene carbonate, and methyl phenyl carbonate can be listed; lithium salts with oxalic acid complexes as anions such as lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiFOB), and lithium difluorobis(oxalate)phosphate (LPFO).

[0039] The positive electrode terminal 30 is disposed at an end portion ( Figure 2 , Figure 3 The negative terminal 40 is arranged at the end of the sealing plate 14 on the other side in the longitudinal direction Y ( Figure 2 , Figure 3 The right end of Figure 3 As shown, the positive terminal 30 and the negative terminal 40 are inserted through the terminal lead holes 18 and 19 and extend from the inside of the sealing plate 14 to the outside. The positive terminal 30 and the negative terminal 40 are fixed to the sealing plate 14. The positive terminal 30 and the negative terminal 40 are riveted to the peripheral portion of the sealing plate 14 surrounding the terminal lead holes 18 and 19 by riveting. At the end ( Figure 3 A rivet portion 30c, 40c is formed at the lower end portion of the rivet portion.

[0040] like Figure 3 As shown, the positive electrode terminal 30 is connected to the positive electrode 22 (see FIG. 1 ) of the wound electrode body 20 via the positive electrode current collecting portion 50 in the outer casing 12. Figure 6The negative electrode terminal 40 is electrically connected to the negative electrode 24 (see Figure 6 The positive electrode terminal 30 is insulated from the sealing plate 14 by the internal insulating member 80 and the gasket 90. The negative electrode terminal 40 is insulated from the sealing plate 14 by the internal insulating member 80 and the gasket 90.

[0041] On the outer surface of the sealing plate 14, a plate-shaped positive electrode external conductive component 32 and a negative electrode external conductive component 42 are installed. The positive electrode external conductive component 32 is electrically connected to the positive electrode terminal 30. The negative electrode external conductive component 42 is electrically connected to the negative electrode terminal 40. The positive electrode external conductive component 32 and the negative electrode external conductive component 42 are components with busbars etc. that electrically connect the plurality of storage cells 100 to each other. The positive electrode external conductive component 32 and the negative electrode external conductive component 42 are insulated from the sealing plate 14 by an external insulating component 92. It should be noted that in Figure 1 Although not shown in the figure, when the battery stack 500 is used, the adjacent storage cells 100 are electrically connected. For example, among the adjacent storage cells 100, the positive electrode external conductive member 32 of one storage cell 100 is electrically connected to the negative electrode external conductive member 42 of another storage cell 100 by a bus bar or the like. Thus, the battery stack 500 is electrically connected. The connection of the battery stack 500 may be a series connection or a parallel connection, and may also be a so-called multi-series multi-parallel connection that combines series and parallel connections.

[0042] Figure 4 The three-dimensional diagram schematically shows the wound electrode bodies 20 mounted on the sealing plate 14. The wound electrode bodies 20 here have three wound electrode bodies 20. However, the number of electrode bodies arranged inside one outer body 12 is not particularly limited, and may be one or more (two or more). The wound electrode bodies 20 are electrically connected in parallel here. The wound electrode bodies 20 are arranged on the winding axis WL (see Figure 6 ) is arranged inside the outer casing 12 in a direction roughly parallel to the long side direction Y. Here, the wound electrode body 20 is arranged in the thickness direction of the storage cell 100 (in other words, a direction roughly perpendicular to the first side wall 12b of the shell 10) and in a direction (short side direction X) that is consistent with the thickness direction of the wound electrode body 20. The outer shape of the wound electrode body 20 is preferably a flat shape. The end face of the wound electrode body 20 that is orthogonal to the winding axis WL (in other words, the stacking surface where the positive electrode 22 and the negative electrode 24 are stacked) is opposite to the second side wall 12c. In addition, although not shown in the figure, an insulating sheet is arranged between the wound electrode body 20 and the outer casing 12.

[0043] Figure 52 is a schematic perspective view of a wound electrode body 20. It should be noted that the wound electrode body 20 housed in the housing 10 may have the same structure. The wound electrode body 20 has a pair of curved portions (R portions) 20r and a flat portion 20f connecting the pair of curved portions 20r. Figure 5 The upper side) of the bent portion 20r is opposite to the sealing plate 14, and the other ( Figure 5 The bent portion 20r is opposite to the bottom 12a of the outer casing 12. The flat portion 20f is opposite to the first side wall 12b of the outer casing 12. Here, the flat portions 20f of the plurality of wound electrode bodies 20 adjacent to each other in the short-side direction X are opposite to each other.

[0044] Figure 6 Schematic diagram showing the structure of the wound electrode body 20. The wound electrode body 20 includes a positive electrode 22, a negative electrode 24, and a separator 26. The wound electrode body 20 is composed of a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 stacked via a strip-shaped separator 26, and wound in the longitudinal direction with a winding axis WL as the center. It should be noted that the winding axis WL direction is a direction substantially parallel to the long side direction Y.

[0045] Positive electrode 22 Figure 6 As shown, there is a positive electrode core 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode core 22c. However, the positive electrode protective layer 22p is not necessary and can be omitted in other embodiments. The positive electrode core 22c is strip-shaped. The positive electrode core 22c is preferably a metal foil, and more preferably composed of aluminum foil or aluminum alloy foil. The positive electrode core 22c is aluminum foil here. There is no special limitation on the thickness of the positive electrode core 22c, preferably 5 to 30 μm, more preferably 10 to 25 μm. The number of stacking layers of the positive electrode 22 is preferably 30 or more.

[0046] At one end portion ( Figure 6 A plurality of positive electrode tabs 22t are provided at the left end portion of the longitudinal direction Y. Figure 6 The plurality of positive electrode tabs 22t protrude further in the longitudinal direction Y than the separator 26. The positive electrode tab 22t is a part of the positive electrode core 22c and is made of metal foil (aluminum foil). Figure 3 to Figure 6 As shown, the plurality of positive electrode tabs 22t are arranged at one end in the longitudinal direction Y ( Figure 3 to Figure 6 The positive electrode sheet group 23 is stacked at the left end of the positive electrode sheet 23 to form the positive electrode sheet group 23. The positive electrode sheet group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode collector 50.

[0047] The positive electrode active material layer 22a is as follows Figure 6As shown, it is arranged in a strip shape along the length direction of the positive electrode core 22c. The positive electrode active material layer 22a contains a positive electrode active material that can reversibly occlude and release charge carriers. As the positive electrode active material, for example, a lithium transition metal composite oxide is preferably used, and nickel (Ni) is particularly preferably contained. The positive electrode active material layer 22a may contain any component other than the positive electrode active material, such as various additives such as a binder and a conductive material, and preferably contains a conductive material and a binder as additives. As a binder used in the positive electrode active material layer 22a, for example, polyvinylidene fluoride (PVdF) and the like can be listed. As a conductive material used in the positive electrode active material layer 22a, there is no particular limitation, and a carbon material is preferably used. The density of the positive electrode active material layer 22a is preferably 3.0 g / cc or more, and more preferably 3.5 g / cc or more. On the other hand, the density of the positive electrode active material layer 22a is preferably 3.7 g / cc or less.

[0048] The positive electrode protective layer 22p is as follows Figure 6 As shown, it is arranged at the boundary portion between the positive electrode core 22c and the positive electrode active material layer 22a in the long side direction Y. The positive electrode protective layer 22p is arranged in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (such as aluminum oxide). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additives, etc.

[0049] Negative electrode 24 Figure 6 As shown, there is a negative electrode core 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode core 24c. The negative electrode core 24c is in a strip shape. The negative electrode core 24c is preferably a metal foil, more preferably a copper foil or a copper alloy foil. The negative electrode core 24c is a copper foil here. There is no particular limitation on the thickness of the negative electrode core 24c, preferably 5 to 30 μm, more preferably 10 to 25 μm.

[0050] At one end portion ( Figure 6 A plurality of negative electrode tabs 24t are provided at the right end of the long side direction Y. Figure 6 The plurality of negative electrode tabs 24t protrude further in the longitudinal direction Y than the separator 26. The negative electrode tab 24t is a part of the negative electrode core 24c and is made of metal foil (copper foil). Figure 3 to Figure 6 As shown, the plurality of negative electrode tabs 24t are arranged at one end in the longitudinal direction Y ( Figure 3 to Figure 6 The negative electrode sheet group 25 is stacked at the right end of the positive electrode sheet group 23 to form the negative electrode sheet group 25. The negative electrode sheet group 25 is provided at a position symmetrical to the positive electrode sheet group 23 in the longitudinal direction Y. The negative electrode sheet group 25 is electrically connected to the negative terminal 40 via the negative electrode collector 60.

[0051] The negative electrode active material layer 24a is as follows Figure 6 As shown, it is arranged in a strip shape along the length direction of the negative electrode core 24c. The negative electrode active material layer 24a contains a negative electrode active material that can reversibly occlude and release charge carriers. As the negative electrode active material, for example, graphite, silicon-based materials (materials containing silicon) and their mixed oxides are preferably used. The negative electrode active material layer 24a may contain any component other than the negative electrode active material, such as various added components such as binders, thickeners, and dispersants. As binders used in the negative electrode active material layer 24a, for example, styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), etc. can be listed. As a conductive material used in the negative electrode active material layer 24a, there is no particular limitation, and carbon materials are preferably used. The density of the negative electrode active material layer 24a is preferably 1.3g / cc or more, and more preferably 1.4g / cc or more. On the other hand, the density of the negative electrode active material layer 24a is preferably 1.7g / cc or less.

[0052] The length Ln of the negative electrode active material layer 24a in the width direction Y is the same as or longer than the length La of the positive electrode active material layer 22a in the width direction Y. Here, the length Ln of the negative electrode active material layer 24a in the width direction Y is preferably 20 cm or more. Specifically, as will be described later, according to this configuration, the return of the non-aqueous electrolyte to the wound electrode body 20 can be appropriately controlled. In addition, when the length of the wound electrode body 20 in a direction perpendicular to the winding axis WL direction and perpendicular to the thickness direction X of the wound electrode body 20 (herein, the Z direction) is set as the height T of the wound electrode body 20, the ratio of the length Ln of the negative electrode active material layer 24a in the width direction to the height T of the wound electrode body 20 (hereinafter also referred to as the “electrode body aspect ratio”) is preferably 2.8 to 3.2. According to this configuration, the return of the non-aqueous electrolyte to the wound electrode body 20 can be appropriately controlled. It should be noted that in the specification, the so-called “height T of the wound electrode body 20” refers to the length of the wound electrode body 20 in the Z direction from one ( Figure 5 U side) the uppermost end of the bent portion 20r to the other ( Figure 5 D side) the distance from the lowermost end of the curved portion 20r.

[0053] The separator 26 is a member that insulates the positive electrode active material layer 22a of the positive electrode 22 from the negative electrode active material layer 24a of the negative electrode 24. The separator 26 constitutes the outer surface of the wound electrode body 20. The length Ls of the separator 26 in the long side direction Y is the same as or longer than the length Ln of the negative electrode active material layer 24a in the long side direction Y. The separator 26 has a substrate portion. For the separator 26, a heat-resistant layer including inorganic particles and a heat-resistant layer binder can be formed on at least one surface of the substrate portion. In addition, for the separator 26, an adhesive layer including an adhesive layer binder can be formed on at least one surface of the substrate portion. In addition to the adhesive layer binder, the adhesive layer can also contain inorganic particles. When viewed from above, the adhesive layer can be formed into a shape having a dot shape, a stripe shape, a wave shape, a belt shape (strip shape), a dotted line shape, or a combination thereof. Although not shown in the figure, in this embodiment, a heat-resistant layer is provided on the surface of the substrate portion of the separator 26, and an adhesive layer is further provided on the heat-resistant layer. The separator 26 preferably has a heat-resistant layer and an adhesive layer. Alternatively, the separator 26 preferably has an adhesive layer containing inorganic particles.

[0054] The base material portion of the separator 26 is a sheet-like member of a microporous film. The separator 26 is preferably made of a polyolefin resin. As the polyolefin resin, for example, polyethylene (PE), polypropylene (PP), or a mixture thereof can be used.

[0055] There is no particular limitation on the thickness of the separator 26. When the separator 26 does not contain a non-aqueous electrolyte, the thickness of the separator 26 is preferably about 10 to 30 μm. It should be noted that the "thickness of the separator 26" in this specification means the thickness including the adhesive layer and the heat-resistant layer when the separator 26 has an adhesive layer and a heat-resistant layer in addition to the base material, and unless otherwise specified, it means the thickness before the press molding process.

[0056] When the separator 26 has an adhesive layer, as the adhesive layer adhesive used in the adhesive layer, the adhesive used in the previously known such purpose can be used without particular restriction, and acrylic resin, fluorine resin (such as PVdF), rubber resin (such as styrene butadiene rubber (SBR)), polyurethane resin, silicone resin, epoxy resin, etc. can be listed. These can be used alone or in combination of two or more. In addition, when the adhesive layer includes inorganic particles, the ratio of the inorganic particles to the total mass of the adhesive layer is preferably about 5 to 20% by mass, and more preferably about 10 to 15% by mass.

[0057] In the case where the separator 26 has a heat-resistant layer, the ratio of the inorganic particles to the total mass of the heat-resistant layer is preferably 85% by mass or more, more preferably 90% by mass or more, and further preferably 95% by mass or more. As the heat-resistant layer adhesive used in the heat-resistant layer, the adhesive used in the previously known such purpose can be used without particular restriction, for example, acrylic resin, fluorine resin, epoxy resin, polyurethane resin, ethylene vinyl acetate resin, etc. can be listed. These can be used alone or in combination of two or more. In addition, the type of the heat-resistant layer adhesive and the adhesive layer adhesive can be the same or different.

[0058] As the inorganic particles used in the heat-resistant layer and the adhesive layer of the separator 26, any inorganic particles used in such applications known in the past can be used without particular limitation, and for example, insulating ceramic particles are preferably included. Among them, from the viewpoint of heat resistance, inorganic oxides such as alumina, zirconia, silica, and titanium dioxide, metal hydroxides such as aluminum hydroxide, and clay minerals such as boehmite are preferred, and alumina and boehmite are more preferred. In addition, from the viewpoint of suppressing thermal shrinkage of the separator 26, compounds containing aluminum are particularly preferred.

[0059] The positive electrode current collecting portion 50 is as follows Figure 3 As shown, a conduction path is formed to electrically connect the positive electrode sheet group 23 composed of a plurality of positive electrode sheets 22t to the positive terminal 30. The positive electrode collector 50 includes a first positive electrode collector 51 and a second positive electrode collector 52. The first positive electrode collector 51 is mounted on the inner surface of the sealing plate 14. The second positive electrode collector 52 extends along the second side wall 12c of the outer body 12. Figure 3 to Figure 5 As shown, the positive electrode second current collecting portion 52 is attached to the wound electrode body 20 .

[0060] The negative electrode current collecting portion 60 is as follows Figure 3 As shown, a conduction path is formed to electrically connect the negative electrode sheet group 25 composed of a plurality of negative electrode sheets 24t to the negative electrode terminal 40. The negative electrode collector 60 includes a negative electrode first collector 61 and a negative electrode second collector 62. The configuration of the negative electrode first collector 61 and the negative electrode second collector 62 may be the same as the positive electrode first collector 51 and the positive electrode second collector 52 of the positive electrode collector 50.

[0061] <Method of Manufacturing Battery Stack 500>

[0062] Figure 7 1 is a flowchart showing a manufacturing method of a battery stack 500 according to an embodiment. The battery stack 500 disclosed herein can be manufactured by a manufacturing method including a preparation step S10 and a stacking step S20, and is characterized in that the preparation step S10 is performed. In addition, in the manufacturing method of the battery stack 500 disclosed herein, in addition to the above-mentioned steps, other steps may be included at any stage, and the manufacturing process other than the steps may be the same as before.

[0063] (Preparation Step S10)

[0064] In the preparation step S10, the electricity storage cell 100 including the wound electrode body 20, the nonaqueous electrolyte, and the case 10 is prepared. In the preparation step S10, the electricity storage cell 100 may be purchased and prepared, or the electricity storage cell 100 may be manufactured and prepared.

[0065] Here, it is characterized in that, for the storage battery cell 100 prepared in the preparation step S10, the storage battery cell 100 is provided with a plurality of holes in the thickness direction ( Figure 1 A load is applied at a speed of 0.1 mm / min to 0.1 MPa in the X direction) and the load is reduced at a speed of 0.1 mm / min to 0.01 MPa after the application as one cycle. When this treatment is performed for 5 cycles, the relationship between the thickness X1 of the storage cell relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the first cycle and the thickness X5 of the storage cell relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the fifth cycle satisfies the following formula: (X1-X5) / X1×100≥0.3. Hereinafter in this specification, (X1-X5) / X1×100 is also referred to as "cell thickness change". It should be noted that the "cell thickness change" in this specification is obtained by measurement using Autograph (precision universal testing machine).

[0066] Figure 8 This is an example of an Fs curve obtained in the preparation step S10 in one embodiment. Here, the Fs curve of the first cycle is equivalent to the Fs curve of the storage cell at the time of shipment (i.e., before use as a battery stack). On the other hand, the Fs curve of the fifth cycle is equivalent to the Fs curve of the storage cell from which the non-aqueous electrolyte retained inside the wound electrode body is removed. Therefore, the difference between X1 and X5 (X1-X5) is equivalent to the thickness of the non-aqueous electrolyte retained inside the wound electrode body at the time of shipment. Moreover, the "cell thickness change" involved in this embodiment is the reduction rate of the cell thickness under a surface pressure of 0.04 MPa, which becomes an indicator of the retention amount of the non-aqueous electrolyte in the wound electrode body.

[0067] Fig. 9 This is a schematic diagram for explaining the change in thickness of the wound electrode body 20 according to one embodiment. Fig.13 It is a schematic diagram for explaining the change in thickness of the wound electrode body 20 according to the conventional example. Fig. 9 and Fig.13 In each of the figures, (a) shows the wound electrode body 20 before the battery stack is constrained, (b) shows the wound electrode body 20 when the battery stack is constrained, and (c) shows the wound electrode body 20 when the nonaqueous electrolyte returns to the wound electrode body 20 . Fig.14This is an example of an Fs curve according to a conventional example. Fig.14 To correspond to Figure 8 . Fig. 9 and Fig.13 In FIG. 1 , a portion of the wound electrode body 20 is partially enlarged.

[0068] In the case where the nonaqueous electrolyte exists inside the wound electrode body 20, for example, the nonaqueous electrolyte exists inside the gaps 26s of the separator 26 of the wound electrode body 20. Fig.13 The state shown in (a) is a state where the nonaqueous electrolyte is retained in the gap 26s of the wound electrode body 20 in the storage cell 100 before being constrained. When constraining the storage cell 100 during battery stack manufacturing, a load is applied to the storage cell 100 in the thickness direction X. Fig.13 As shown in (b), the gaps 26s of the wound electrode body 20 are squeezed, and the non-aqueous electrolyte retained inside the gaps 26s is squeezed out to the outside of the wound electrode body 20. On the other hand, when the battery stack 500 is in use, for example, during initial charging, in a low temperature environment, and under low SOC conditions, the thickness of the wound electrode body 20 is reduced. In particular, when the conditions of low temperature environment, low SOC conditions, and initial charging are met, the reduction in the thickness of the wound electrode body 20 becomes significant. As a result, the restraint load on the storage unit 100 generated by the restraint mechanism 300 becomes smaller. Thus, as Fig.13 As shown in (c), the non-aqueous electrolyte outside the wound electrode body 20 returns to the inside of the wound electrode body 20 at the portion where the restraining load becomes smaller. Here, the amount of non-aqueous electrolyte that returns to the inside of the wound electrode body 20 is affected by the amount of voids 26s in the wound electrode body 20. In other words, when the amount of voids 26s in the wound electrode body 20 of the storage cell 100 is small, the amount of non-aqueous electrolyte that returns to the inside of the wound electrode body 20 becomes smaller. Fig.14 As shown, in the conventional storage cell 100, the difference between X1 and X5 is small. In other words, the gap 26s for the non-aqueous electrolyte present outside the wound electrode body 20 to return to the inside of the wound electrode body 20 is small. In this way, when the gap 26s of the wound electrode body 20 of the storage cell 100 is small, the amount of non-aqueous electrolyte returning to the wound electrode body 20 is small, so the thickness of the wound electrode body 20 is not well increased, and the thickness of the storage cell 100 is still thin. Therefore, the load applied to the storage cell 100 is reduced, and it is no longer possible to restrain with a sufficient load.

[0069] Here, in the battery stack 500 according to the present embodiment, it is characterized in that in the preparation step S10, a storage cell having a cell thickness variation (%) of 0.3% or more (≥0.3) is prepared. The storage cell 100 is made to have a sufficient difference between X1 and X5. In other words, Fig. 9As shown in (a), the wound electrode body 20 is made thick enough to retain the non-aqueous electrolyte component inside the wound electrode body during shipment. Fig. 9 As shown in (c), there is a sufficient gap 26s for the non-aqueous electrolyte existing outside the wound electrode body 20 to return to the inside of the wound electrode body 20. Therefore, by re-entering the non-aqueous electrolyte, the thickness of the wound electrode body 20 increases, and the thickness of the storage cell 100 increases. Therefore, the reduction of the load applied to the storage cell 100 is suppressed, and in the battery stack 500, a sufficient load is maintained on the storage cell 100.

[0070] Fig.10 Schematic diagram for explaining the measurement of the cell thickness variation in the preparation step S10. Fig.10 In FIG. 1 , the direction in which the load is applied by the Autograph 600 in the thickness direction of the power storage unit 100 is indicated by a white arrow. Fig.10 As shown in FIG. 1 , first, the power storage cell 100 is placed on the Autograph 600 in such a manner that a load is applied in the thickness direction (the direction of the white arrow). Fig.10 As shown in FIG. 1 , the pair of first side walls 12 b of the storage cell 100 are arranged in contact with the Autograph 600. When the storage cell 100 is viewed in the horizontal direction, the load generated by the Autograph 600 is applied to the flat portion 20 f of the wound electrode body 20. Figure 3 The storage cell 100 is set in Autograph 600 in such a manner that a load is applied to the portion indicated by the imaginary line. There is no particular limitation on the means for measuring the thickness displacement of the storage cell 100, and for example, a laser displacement meter (for example, manufactured by KEYENCE Co., Ltd., product name: LK-G157, etc.) can be used. In addition, the thickness of the storage cell 100 may be measured at one location or at multiple locations (more than two locations). Then, a load is applied to the storage cell 100 at a speed of 0.1 mm / min in the thickness direction of the storage cell 100 (illustrated by a white arrow). When the load reaches 0.1 MPa, the load is reduced to 0.01 MPa at a speed of 0.1 mm / min. The above-mentioned cycle is regarded as one cycle, and this process is performed for 5 cycles. At this time, the Fs curve (load-displacement curve) of the pressurized side of the 1st cycle and the 5th cycle is obtained (refer to Figure 8 ).

[0071] Based on the obtained Fs curve, the thickness of the storage cell at 0.04 MPa in the first cycle was plotted and set as X1. On the other hand, based on the obtained Fs curve, the thickness of the storage cell at 0.04 MPa in the fifth cycle was plotted and set as X5. Then, the cell thickness change (%) was calculated according to the following formula (i).

[0072] (X1-X5) / X1×100···Formula (i)

[0073] The method of controlling the numerical range of the cell thickness variation of the storage cell 100 is not particularly limited, and various methods can be used. For example, the cell thickness variation of the storage cell 100 can be controlled by adjusting the gap 26s of the separator 26, the size of the wound electrode body 20, and the like.

[0074] The method for controlling the numerical range of the cell thickness variation of the storage cell 100 is not limited to this, and for example, it can be controlled by adjusting the length Ln of the negative electrode active material layer 24a in the width direction Y of the wound electrode body 20. At this time, the length Ln of the negative electrode active material layer 24a in the width direction Y is preferably 20 cm or more. According to this structure, the entry and exit of the non-aqueous electrolyte into the wound electrode body 20 can be appropriately controlled. That is, the numerical range of the cell thickness variation of the storage cell 100 can be controlled. Similarly, the numerical range of the cell thickness variation of the storage cell 100 can be controlled by adjusting the ratio (Ln / T) of the length Ln of the negative electrode active material layer 24a in the width direction to the height T of the wound electrode body 20 (electrode body aspect ratio). In this case, the above-mentioned electrode body aspect ratio is preferably 2.8 to 3.2. With this structure, the entry and exit of the non-aqueous electrolyte into the wound electrode body 20 can also be appropriately controlled.

[0075] The method for controlling the numerical range of the cell thickness variation of the storage cell 100 is not limited to this. For example, when the separator 26 has an adhesive layer on its surface, it can be controlled by adjusting the ratio of the area where the adhesive layer is formed (area of ​​the adhesive layer forming region / area of ​​the separator×100). In this case, the ratio of the area where the adhesive layer is formed is preferably about 3 to 30%, and more preferably about 5 to 15%. In addition, it is preferred that the adhesive layer on the surface of the separator 26 is applied in a dotted shape. Thus, the gap 26s of the separator 26 can be appropriately increased, and the amount of non-aqueous electrolyte retained can be increased. In addition, the ratio (Vol%) of the volume of the adhesive layer to the volume between the electrode (positive electrode or negative electrode) and the substrate portion of the separator (volume of the adhesive layer of the separator / volume between the electrode and the separator substrate×100) is preferably 50 to 97 Vol%, and more preferably 85 to 95 Vol%. By using a wound electrode body having this numerical range, the numerical range of the cell thickness variation of the storage cell 100 can also be controlled to a preferred numerical range.

[0076] The method for controlling the numerical range of the cell thickness variation of the storage cell 100 is not limited to the above, and can also be controlled by adjusting the particle size (D50) of the inorganic particles contained in the adhesive layer and the heat-resistant layer. In this case, the particle size (D50) of the inorganic particles contained in the adhesive layer and the heat-resistant layer is preferably about 0.1 to 0.6 μm. It should be noted that in the specification, the particle size (D50) of the inorganic particles represents the average particle diameter of the weight accumulation of 50 wt% calculated from the smallest particle size in the particle size distribution measured by the laser diffraction method.

[0077] In the preparation step S10, a storage cell 100 having a cell thickness variation value in the range of 0.3% or more (≥0.3) can be prepared. The cell thickness variation value can be measured by the above-mentioned method in the preparation step S10, thereby confirming that the cell thickness variation value range of the storage cell 100 is in the range of 0.3% or more (≥0.3).

[0078] There is no particular upper limit on the cell thickness variation. The greater the cell thickness variation, the greater the thickness of the storage cell 100 before the constraint (before the battery stack is installed). Therefore, from the perspective of miniaturization of the installation device in the stacking step S20 and labor saving in the stacking step S20, the cell thickness variation is preferably 2.0% or less.

[0079] (Lamination Step S20)

[0080] In the stacking step S20, a plurality of power storage cells 100 are stacked along the thickness direction X of the power storage cells 100. The stacking step S20 may be the same as a conventionally known method for manufacturing a battery stack. Here, a plurality of power storage cells 100 are clamped in the arrangement direction X by a pair of end plates 310 and constrained by side plates 320 and a plurality of screws 330. At this time, a constraint load is applied in the stacking direction of the power storage cells 100 by a constraint mechanism 300. In this way, the battery stack 500 involved in this embodiment is manufactured. The constraint load when the cells are stacked in the stacking step S20 may be, for example, 2 to 30 kN, preferably 3 to 20 kN.

[0081] <Method of Manufacturing Power Storage Cell 100>

[0082] Although not particularly limited, the electric storage cell 100 in the preparation step S10 can be prepared by, for example, the manufacturing method described below. It should be noted that the manufacturing method of the electric storage cell 100 described below is an example of the preparation step S10 in this specification. Fig.11 FIG. 1 is a flowchart showing a method for manufacturing the power storage unit 100 according to one embodiment. Fig.11As shown, although not particularly limited, the storage cell 100 can be manufactured by a manufacturing method that typically includes, in sequence, an assembly step S101, a drying step S102, a liquid injection step S103, an exhaust charging step S104, a decompression step S105, a liquid injection hole sealing step S106, an activation step S107, and an aging step S108. In addition, in the manufacturing method of the storage cell 100 disclosed herein, in addition to the above-mentioned steps, other steps may be included at any stage, and the manufacturing process other than the above steps may be the same as in the past.

[0083] (Assembly process S101)

[0084] In the assembly step S101, the wound electrode body 20 is placed in the case 10 (external body 12) to prepare an assembly. In this specification, the term "assembly" refers to the power storage unit in a state before the injection hole sealing step described later is performed.

[0085] In the assembly process S101, the positive electrode second collector 52 is installed on the positive electrode sheet group 23 of the wound electrode body 20, and the negative electrode second collector 62 of the negative electrode collector 60 is installed on the negative electrode sheet group 25. Next, the positive terminal 30 and the negative terminal 40 are installed on the sealing plate 14. Next, the positive terminal 30 is joined to the positive electrode first collector 51 and the negative terminal 40 is joined to the negative electrode first collector 61 by a conventionally known method (e.g., ultrasonic bonding, resistance welding, laser welding, etc.). Next, the wound electrode body 20 is accommodated in an insulating sheet. The insulating sheet can be prepared, for example, by bending an insulating resin sheet made of a resin material such as polyethylene (PE) into a bag or box shape. Then, the wound electrode body 20 covered with an insulating sheet is preferably accommodated (inserted) into the internal space of the outer body 12. Then, the outer body 12 of the shell 10 is joined to the sealing plate 14 to make an assembly. The joining can be performed by welding such as laser welding, for example. In the assembly step S101 , the liquid injection hole 15 is not sealed.

[0086] In the assembly step S101, the wound electrode body 20 is preferably arranged in the thickness direction of the storage battery cell 100 (in other words, the direction substantially perpendicular to the first side wall 12b of the case 10) in a direction (short side direction X) that coincides with the thickness direction of the wound electrode body 20. In other words, the wound electrode body 20 is preferably arranged inside the outer casing 12 so that the winding axis WL is parallel to the bottom 12a of the outer casing 12.

[0087] (Drying process S102)

[0088] In the drying step S102, the assembly is dried to remove moisture contained in the assembly (e.g., the interior of the wound electrode body 20). The drying method can be performed by a known method. For example, the drying step S102 can be performed by conveying the assembly (the case 10 that accommodates the wound electrode body 20) to a drying furnace (not shown) and heating it.

[0089] The drying temperature and drying time in the drying step S102 can be appropriately adjusted according to the amount of water contained in the wound electrode body 20, etc. The drying temperature is not particularly limited as long as it is within the range that can remove the water, and it is preferably dried at a temperature at which the separator 26 of the wound electrode body 20 is not damaged. In addition, the drying step S102 is preferably carried out in a reduced pressure atmosphere. Thereby, the drying time in the drying step S102 can be shortened. However, it is not limited to this, and the drying step S102 can be carried out in an atmospheric pressure atmosphere. It should be noted that in the technology disclosed herein, the drying step S102 is not a necessary step. In some preferred embodiments, the drying step S102 can also be omitted.

[0090] (Liquid injection step S103)

[0091] In the injection process S103, a non-aqueous electrolyte is injected into the shell 10 that accommodates the wound electrode body 20 from the injection hole 15 provided in the sealing plate 14. The injection process S103 can be implemented in an atmospheric pressure atmosphere or in a reduced pressure atmosphere. Preferably, it can be implemented in a reduced pressure atmosphere. As a result, the impregnation of the non-aqueous electrolyte into the wound electrode body 20 is improved, and the injection process S103 can be performed in a shorter time. In the injection process S103, the non-aqueous electrolyte is injected in a manner that the non-aqueous electrolyte becomes the entire weight of the wound electrode body 20. The injection process S103 can appropriately utilize a non-aqueous electrolyte injection device that is previously known. It should be noted that at this time, as a pressurized gas that can be used to pressurize the non-aqueous electrolyte, as in the past, inert gases such as nitrogen (N2), dry air, etc. can be listed. After the injection process S103 is completed, it is preferably appropriately pressurized and depressurized in the shell 10.

[0092] (Exhaust Charging Step S104)

[0093] In the exhaust charging step S104, the assembly is charged. As a result, a film can be formed on the surface of the negative electrode active material layer 24a. Furthermore, by discharging the gas generated during charging and discharging to the outside of the shell 10, the amount of gas generated inside the shell 10 is reduced after the injection hole 15 is sealed, and the gas can be suppressed from remaining in the wound electrode body 20 after the injection hole 15 is sealed. There is no particular limitation on the charging conditions in this step, and it can be the same as the previous manufacturing method. Although there is no particular limitation, for example, the exhaust charging step S104 can be implemented by charging at a current of about 0.05C to 10C at a normal temperature environment (for example, 25°C) until the SOC (State of Charge) becomes about 20% to 90%.

[0094] In the exhaust charging step S104, it is preferred to perform the process while the shell 10 is constrained and a load is applied to the shell 10. As a result, since the gas in the shell 10 is easily squeezed out, it is possible to suppress the mixing of gas in the electrode body. In the case where the shell 10 is constrained in the exhaust charging step S104, it is preferred to apply a load to the first side wall 12b of the shell 10. In addition, in the constraint, when viewed from the front of the first side wall 12b of the shell 10, it is preferred to use the center CP (refer to Figure 3 ) is constrained in a manner that is substantially consistent with the center of the constrained area. In addition, there is no particular limitation on the constrained area, and it is preferred that the first side wall 12b of the shell 10 constrain an area centered on the center CP of the wound electrode body 20, with a length of 280 to 295 mm in the long side direction Y and a length of 85 to 95 mm in the up and down direction Z. There is no particular limitation on the load applied to the shell 10, and it is preferably 0.25 to 0.80 MPa. It should be noted that in this specification, the so-called "center CP of the wound electrode body 20" is, for example, Figure 3 As shown, it refers to the point where the center MY in the longitudinal direction Y and the center MZ in the vertical direction Z are orthogonal to each other on the surface having the flat portion 20 f in the wound electrode body 20 (the surface facing the first side wall 12 b of the case 10 ).

[0095] (Decompression Step S105)

[0096] In the decompression step S105, the gas existing inside the shell 10 (such as air, gas generated in the exhaust charging step S104, etc.) is further discharged to the outside of the shell 10 by decompressing the inside of the shell 10. The decompression step S105 can be the same as the means used in the decompression step in the previous manufacturing method of this type, and in particular, it does not add features to the technology disclosed herein, so a more detailed description is omitted. It should be noted that in the technology disclosed herein, the decompression step S105 is not a necessary step. In some preferred embodiments, the decompression step S105 can also be omitted.

[0097] (Liquid injection hole sealing step S106)

[0098] In the injection hole sealing step S106, the injection hole 15 of the assembly is sealed. The injection hole sealing step S106 can be the same as the manufacturing method of the previously known storage battery unit 100, and is not particularly limited. Here, the injection hole 15 is sealed by using a metal sealing member 16, and the metal part of the sealing member 16 is welded to the sealing plate 14 (the peripheral portion of the injection hole 15) to seal it. However, the sealing method of the injection hole 15 is not limited to this. Although the illustration is omitted, the injection hole 15 can be sealed with rivets such as blind rivets, for example.

[0099] (Activation Step S107)

[0100] In the activation step S107, the storage cell 100 whose injection hole 15 is sealed in the injection hole sealing step S106 is charged while applying a load in the thickness direction of the storage cell 100. Thus, a film is formed on the surface of the negative electrode active material layer 24a. It should be noted that the activation step S107 is included as an example of the "preparation step S10" in this specification.

[0101] The charging conditions in the activation step S107 are not particularly limited and can be the same as those in the conventional manufacturing method. Although not particularly limited, for example, the activation step S107 can be performed by charging at a current of about 0.05C to 10C at a normal temperature environment (e.g., 25°C) until the SOC (State of Charge) reaches about 20% to 90%.

[0102] In the activation step S107, the load applied to the storage cell 100 is preferably 0.5 to 0.7 MPa. According to this configuration, the cell thickness variation can be further kept within a preferred range. The method of applying the load to the storage cell 100 is not particularly limited, and general means that can be used in the conventional method of manufacturing the storage cell can be used. For example, the load can be applied to the storage cell 100 by clamping a pair of first side walls 12b of the storage cell 100 with a restraining plate and connecting the restraining plate with a bridging member.

[0103] (Aging process S108)

[0104] In the aging step S108, the storage cell 100 that has passed the activation step S107 is stored for a predetermined time in a predetermined temperature environment while maintaining the charged state. As a result, a film can be more preferably formed on the surface of the negative electrode active material layer 24a. It should be noted that the aging step S108 is not an essential step in the technology disclosed herein. In some preferred embodiments, the aging step S108 can also be omitted.

[0105] It should be noted that the conditions of the aging process S108 can be appropriately adjusted according to the desired method of film formation, and are not particularly limited. For example, the unit temperature (aging temperature) in the aging process S108 can be set to be above 30°C, preferably above 40°C, for example, above 50°C, and further above 60°C. There is no particular restriction on the upper limit of the aging temperature, for example, about 70°C or less can be used as an indicator. The temperature management in the aging process S108 can use a thermostatic bath, for example. The implementation time (aging time) of the aging process S108 can be appropriately changed according to the aging temperature, for example, and is not particularly limited. For example, when the aging temperature is about 45 to 65°C, it is preferred that the aging time is about 3 to 30 hours.

[0106] In the aging step S108, it is preferred to perform aging while applying a load in the thickness direction X of the power storage cell 100. The amount of load applied to the power storage cell in the aging step S108 is not particularly limited, but is preferably 0.5 to 0.7 MPa. Alternatively, the aging step S108 may be performed while maintaining the load applied in the activation step S107.

[0107] The battery stack 500 can be used for various purposes, for example, it can be suitably used as a power source (driving power source) for a motor mounted on a car, truck, etc. The type of vehicle is not particularly limited, and examples thereof include a plug-in hybrid electric vehicle (PHEV), a hybrid electric vehicle (HEV), and a battery electric vehicle (BEV).

[0108] The following describes embodiments of the technology disclosed herein, but the embodiments are not intended to limit the technology disclosed herein.

[0109] <Preparation of power storage unit>

[0110] First, three storage cells for constructing the battery stack according to Example 1 were prepared. The wound electrode assembly housed in the storage cell according to Example 1 was Figure 5The wound electrode body shown has a pair of curved portions, a strip-shaped positive electrode and a strip-shaped negative electrode stacked via a strip-shaped separator and wound in the length direction. It should be noted that as the separator of Example 1, a separator having an adhesive layer and a heat-resistant layer, a ratio of the forming area of ​​the adhesive layer of 30%, and a particle size of the inorganic particles contained in the heat-resistant layer of 0.5 μm is used. In addition, the length in the width direction of the negative electrode active material layer forming area of ​​the storage unit involved in the embodiment is set to 29 cm, and the aspect ratio of the electrode body (the ratio of the length Ln in the width direction of the negative electrode active material layer to the height T of the wound electrode body (Ln / T)) is set to 3.0. In addition, the number of stacked layers of the positive electrode involved in the wound electrode body is 33.

[0111] Next, as Example 2, three storage cells according to Example 2 were prepared which were the same as those according to Example 1 except that a separator in which the ratio of the adhesive layer formed area was 7% and the particle size of inorganic particles in the adhesive layer was 0.3 μm was used.

[0112] As Comparative Example 1, three storage cells involved in Comparative Example 1 were prepared, which were the same as the storage cells involved in Example 1, except that a separator in which the ratio of the formation area of ​​the adhesive layer was 100% and the particle size of the inorganic particles of the adhesive layer was 1.0 μm was used. Similarly, as Comparative Example 2, three storage cells involved in Comparative Example 2 were prepared, which were the same as the storage cells involved in Example 1, except that the separator in Comparative Example 1 was used and charging and discharging were performed while applying a load of 0.4 MPa in the thickness direction of the storage cells in the activation process. In addition, as Comparative Example 3, in addition to using a so-called stacked structure electrode body (i.e., an electrode body that is not a wound electrode body) in which a roughly rectangular positive electrode and a roughly rectangular negative electrode are stacked in the thickness direction X of the storage cell via a roughly rectangular separator, the aspect ratio of the above-mentioned electrode body is 1.6, the shape of the shell is changed together with the change of the above-mentioned electrode body (however, the plate thickness and material are not changed), and charging and discharging are performed while applying a load of 0.18 MPa in the thickness direction of the storage cell during the activation process, three storage cells involved in Comparative Example 3 that are the same as the storage cells involved in Example 1 are prepared.

[0113] <Evaluation of cell thickness variation>

[0114] The above-mentioned method was used to evaluate the change in cell thickness for the storage cells involved in Examples 1 to 2 and Comparative Examples 1 to 3. It should be noted that Autograph used a precision universal testing machine (Autograph AGX-V) manufactured by Shimadzu Corporation. In addition, as for the cell thickness, LK-G157 manufactured by KEYENCE Corporation was used as a laser displacement meter for measurement. First, as Fig.10As shown, the storage cell is set in Autograph. Then, a load is applied in the thickness direction of the storage cell (illustrated by a white arrow) at a speed of 0.1 mm / min. After the load applied to the storage cell reaches 0.1 MPa, the load is reduced to 0.01 MPa at a speed of 0.1 mm / min. These treatments are regarded as one cycle, and the treatment is performed for 5 cycles. In this way, the Fs curves (load-displacement curves) involved in the first cycle and the fifth cycle are obtained respectively. Then, from the obtained Fs curves, the thickness X1 of the storage cell relative to the surface pressure of 0.04 MPa in the first cycle and the thickness X5 of the storage cell relative to the surface pressure of 0.04 MPa in the fifth cycle are obtained, and the cell thickness change (%) is calculated using X1 and X5 using formula (i). The results are shown in Table 1.

[0115] Unit thickness change (%) = (X1-X5) / X1×100···Formula (i)

[0116] [Table 1]

[0117] Table 1

[0118]

[0119] <0.3~3kN spring constant>

[0120] For the storage cells involved in Examples 1 to 2 and Comparative Examples 1 to 3, a "0.3 to 3 kN spring constant" is calculated. It should be noted that in this specification, the so-called "0.3 to 3 kN spring constant" is an indicator that represents the degree of detachment of the battery stack restraint load when the cell thickness is reduced. Specifically, based on the Fs curve obtained above, a coordinate graph is prepared in which the change in cell thickness between the 1st cycle and the 5th cycle at the same load is set as Δ cell thickness (mm) as the horizontal axis and the applied load (kN) as the vertical axis. Then, the spring constant when the load range is 0.3 to 3 kN is calculated as "0.3 to 3 kN spring constant (kN / mm)". It should be noted that the "0.3 to 3 kN spring constant" is calculated according to the following formula (ii). The results are shown in Table 1.

[0121] 0.3 to 3 kN spring constant (kN / mm) = -((3-0.3)(kN) / (Δ unit thickness at 3 kN - Δ unit thickness at 0.3 kN))(mm) ···Formula (ii)

[0122] In addition, for Examples 1 and 2 and Comparative Example 2, a coordinate diagram is shown in which the change in cell thickness under the same load between the 1st cycle and the 5th cycle is plotted as Δ cell thickness (mm) on the horizontal axis and the applied load (kN) on the vertical axis. Fig.12 . Fig.12In the coordinate diagram, the area between 0.3 and 3 kN of load is represented by a thick line.

[0123] <Results>

[0124] As can be seen from Table 1, Examples 1 and 2, in which the cell thickness variation is 0.3% or more (≥0.3), have a lower "0.3 to 3 kN spring constant" than Comparative Examples 1 to 3. This means that even when the cell thickness is reduced due to low temperature conditions, low SOC conditions, etc., the thickness of the storage cell is appropriately controlled (the thickness of the storage cell increases again), so that the degree of dropout of the battery stack restraint load is small. Therefore, in a battery stack manufactured using a storage cell with a cell thickness variation of 0.3% or more (≥0.3), even when the thickness of the storage cell is reduced, the thickness of the storage cell is appropriately controlled, so that the reduction of the restraint load of the battery stack can be suppressed (the dropout of the restraint load is small).

[0125] The preferred embodiment of the present disclosure is described above, and the above embodiment is only an example. The present disclosure can be implemented in various other ways. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in this field. The technology described in the claims includes the technology of variously deforming and changing the above-mentioned exemplified embodiments. For example, part of the above-mentioned embodiment can be replaced by other variations, and other variations can be added to the above-mentioned embodiment. In addition, as long as the features of the technology are not described as necessary features, they can be deleted as appropriate.

[0126] As described above, specific aspects of the technology disclosed herein include aspects described in the following items.

[0127] Item 1: A method for manufacturing a battery stack, which is a method for manufacturing a battery stack including a plurality of square storage cells, comprising: a preparation step of preparing the storage cells, wherein the storage cells include a flat-shaped wound electrode body in which a positive electrode and a negative electrode are stacked and wound via a separator, a non-aqueous electrolyte, and a shell for accommodating the wound electrode body and the non-aqueous electrolyte; and a stacking step of stacking a plurality of the storage cells along the thickness direction of the storage cells; stacking the storage cells prepared in the preparation step in the thickness direction of the storage cells A load is applied at a speed of 0.1 mm / min until it reaches 0.1 MPa, and then the load is reduced at a speed of 0.1 mm / min to 0.01 MPa as one cycle. When this treatment is performed for 5 cycles, the relationship between the thickness X1 of the storage cell relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the first cycle and the thickness X5 of the storage cell relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the fifth cycle satisfies the following formula: (X1-X5) / X1×100≥0.3.

[0128] Item 2: A method for manufacturing a battery stack according to Item 1, wherein the negative electrode includes a negative electrode core and a negative electrode active material layer formed on the negative electrode core, and the length Ln of the negative electrode active material layer in the width direction orthogonal to the length direction of the wound electrode body is greater than 20 cm.

[0129] Item 3: A method for manufacturing a battery stack according to Item 2, wherein, when the length of the wound electrode body in a direction perpendicular to the winding axis direction and perpendicular to the thickness direction of the wound electrode body is set as the height T of the wound electrode body, the ratio of the length Ln in the width direction of the negative electrode active material layer to the height T of the wound electrode body (Ln / T) is 2.8 to 3.2.

[0130] Item 4: A method for manufacturing a battery stack according to any one of Items 1 to 3, wherein the preparation step includes an activation step of charging the power storage unit while applying a load in the thickness direction of the power storage unit, and in the activation step, the load applied to the power storage unit is 0.5 to 0.7 MPa.

[0131] Item 5: The method for manufacturing a battery stack according to any one of Items 1 to 4, wherein the number of stacked layers of the positive electrode is 30 or more.

[0132] Item 6: A method for manufacturing a battery stack according to any one of Items 1 to 5, wherein the relationship between the thickness X1 of the battery cell relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the first cycle and the thickness X5 of the battery cell relative to the surface pressure of 0.04 MPa in the pressurized side Fs curve of the fifth cycle also satisfies the following formula: (X1-X5) / X1×100≤2.0.

Claims

1. A method for manufacturing a battery stack, which is a method for manufacturing a battery stack including a plurality of square power storage cells, comprising: a step of preparing the electricity storage unit, the electricity storage unit including a flat wound electrode body in which a positive electrode and a negative electrode are stacked and wound via a separator, a nonaqueous electrolyte, and a case accommodating the wound electrode body and the nonaqueous electrolyte; and a stacking step of stacking a plurality of the power storage cells in a thickness direction of the power storage cells; When a load of 0.1 MPa is applied to the storage battery cell prepared in the preparation step in the thickness direction of the storage battery cell at a speed of 0.1 mm / min and then reduced at a speed of 0.1 mm / min to 0.01 MPa, one cycle is defined as five cycles of the load. The relationship between the thickness X1 of the electric storage cell at a surface pressure of 0.04 MPa in the pressurized side Fs curve of the first cycle and the thickness X5 of the electric storage cell at a surface pressure of 0.04 MPa in the pressurized side Fs curve of the fifth cycle satisfies the following equation: (X1-X5) / X1×100≥0.

3.

2. The method for manufacturing a battery stack according to claim 1, wherein: The negative electrode includes a negative electrode core and a negative electrode active material layer formed on the negative electrode core. A length Ln of the negative electrode active material layer in a width direction perpendicular to the longitudinal direction of the wound electrode body is 20 cm or more.

3. The method for manufacturing a battery stack according to claim 2, wherein: When the length of the wound electrode body in a direction perpendicular to the winding axis direction and perpendicular to the thickness direction of the wound electrode body is defined as the height T of the wound electrode body, A ratio (Ln / T) of a length Ln in a width direction of the negative electrode active material layer to a height T of the wound electrode body is 2.8 to 3.

2.

4. The method for manufacturing a battery stack according to claim 1 or 2, wherein: The preparation step includes an activation step of charging the power storage cell while applying a load in the thickness direction of the power storage cell. In the activation step, a load applied to the power storage cell is 0.5 to 0.7 MPa.

5. The method for manufacturing a battery stack according to claim 1 or 2, wherein: The positive electrode has 30 or more layers stacked.

6. The method for manufacturing a battery stack according to claim 1 or 2, wherein: The relationship between the thickness X1 of the electric storage cell at the pressurized side Fs curve of the first cycle and the thickness X5 of the electric storage cell at the pressurized side Fs curve of the fifth cycle and the surface pressure of 0.04 MPa also satisfies the following equation: (X1-X5) / X1×100≤2.0.