Surface difunctional modified inorganic solid electrolyte and preparation method and application thereof
By modifying the inorganic solid electrolyte and introducing ionic liquids with titanate coupling agents, the safety hazards of liquid electrolytes in lithium batteries and the problem of high interfacial impedance of composite electrolytes are solved, and the migration rate and electrochemical performance of lithium ions are improved to achieve Efficient electrochemical performance improvement and process simplification are achieved.
Patent Information
- Application Number
- CN202410677243.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-01
AI Technical Summary
Liquid electrolytes in traditional lithium batteries have irreversible side reactions, volatilization and leakage problems, leading to safety hazards. The composite solid electrolyte has high interfacial impedance and low ionic conductivity, which affects electrochemical performance.
Titanate coupling agent is used to surface modify the inorganic solid electrolyte to reduce the surface energy, optimize the compatibility of the organic-inorganic interface, and introduce ionic liquid to broaden the migration channel of lithium ions. The composite solid electrolyte is prepared by solution casting method.
It improves the dispersion of the inorganic solid electrolyte and the migration rate of lithium ions, improves the ionic conductivity and electrochemical performance, simplifies the process, reduces the cost, and is suitable for large-scale production.
Smart Images

Figure CN118738523A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a surface dual-functional modified inorganic solid electrolyte and a preparation method and application thereof. Background Art
[0002] With the rapid development of electric vehicles and other energy storage industries, the energy density of traditional lithium battery systems is gradually approaching its theoretical limit and cannot meet the growing energy density requirements in practical applications. Lithium metal has an ultra-high theoretical specific capacity (~3860mAh·g -1 ), low redox potential (-3.04 V vs standard hydrogen electrode) and light bulk density (0.534 g cm -3 ), so lithium metal batteries with lithium metal as the negative electrode are widely considered to be one of the most promising next-generation energy storage devices. However, the use of traditional liquid electrolytes usually has some problems, such as irreversible side reactions leading to dendrite growth, and volatilization or leakage of electrolytes during battery service causing safety accidents. Using safer solid electrolytes to replace liquid electrolytes is a feasible solution to optimize the electrochemical performance and safety of lithium metal batteries.
[0003] Solid electrolytes can be mainly divided into three categories: inorganic solid electrolytes, solid polymer electrolytes and composite solid electrolytes. Inorganic solid electrolytes have advantages such as high room temperature conductivity, high mechanical properties, and wide electrochemical window, but they still have some defects, such as poor chemical stability, high processing cost, and large solid-solid interface impedance. Solid polymer electrolytes have advantages such as good flexibility and good processability, but they also have disadvantages such as low ionic conductivity and poor mechanical properties. Composite polymer electrolytes formed by using polymers as the matrix and adding inorganic fillers combine the advantages of the above two, such as high ionic conductivity, high mechanical strength, good flexibility, and close contact with electrodes, and are considered to be the most promising candidates for solid electrolytes. However, problems such as the agglomeration of inorganic fillers in composite solid electrolytes and poor inorganic-organic interface contact limit the uniformity of the internal components of the composite solid electrolyte and the lithium ion transport at the interface, resulting in high interface impedance, low ionic conductivity, and poor electrochemical performance of solid-state batteries. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a surface bifunctional modified inorganic solid electrolyte and its preparation method and application.
[0005] The above object of the present invention is achieved through the following technical solutions:
[0006] The first aspect of the present invention provides a method for preparing a surface dual-functional modified inorganic solid electrolyte, comprising the following steps:
[0007] (1) adjusting the pH value of the aqueous solution of the organic solvent to 4 to 6 to obtain an acidic organic solution;
[0008] (2) adding a titanate coupling agent to the acidic organic solution obtained in step (1), and stirring at 20 to 50° C. to obtain a mixed solution;
[0009] (3) adding an inorganic solid electrolyte to the mixed solution obtained in step (2), stirring at 40 to 80° C. to obtain a suspension, centrifuging and drying to obtain an intermediate product;
[0010] (4) dissolving the intermediate product obtained in step (3) and the ionic liquid in an organic solvent, stirring at 40 to 90° C., centrifuging and drying to obtain a surface bifunctional modified inorganic solid electrolyte.
[0011] The surface modification of the inorganic solid electrolyte by the titanate coupling agent in the present invention reduces the surface energy of the inorganic solid electrolyte, promotes the dispersion of the inorganic solid electrolyte, and optimizes the organic-inorganic interface compatibility between the inorganic solid electrolyte and the polymer matrix. At the same time, the introduced ionic liquid broadens the migration channel of lithium ions at the interface, promotes the rapid migration of lithium ions at the organic-inorganic interface, and improves the ionic conductivity.
[0012] Furthermore, in step (1), an acidic regulator is used to adjust the pH value of the aqueous solution of the organic solvent to provide an acidic environment for the hydrolysis of the titanate coupling agent, wherein the acidic regulator is selected from one or more of formic acid, glacial acetic acid and acetic acid, and the organic solvent is selected from one or more of methanol, anhydrous ethanol, isopropanol and acetone.
[0013] Furthermore, in step (1), the volume ratio of the organic solvent to water in the aqueous solution of the organic solvent is (5-20):1.
[0014] Further, in step (2), the titanate coupling agent is selected from one or more of isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl tri (dioctyl phosphate) titanate, isopropyl trioleyl titanate, isopropyl tri (dioctyl pyrophosphate) titanate, isopropyl tri (isostearoyl) titanate, isopropyl tri (dodecylbenzenesulfonyl) titanate, isopropyl triisostearyl titanate, bis (dioctyl pyrophosphate) ethylene titanate, trihydroxy acyl titanate isopropyl, di (dioctyl pyrophosphate) ethylene glycol titanate, dihydroxy acyl ethylene diethylene titanate, bistriethanolamine diisopropyl titanate and tetraisopropyl di (dioctyl phosphite) titanate.
[0015] Furthermore, in step (2), the stirring time is 1 to 10 hours.
[0016] Furthermore, the mass ratio of the titanate coupling agent in step (2) to the inorganic solid electrolyte in step (3) is (0.2-2):1.
[0017] Furthermore, in step (3), the inorganic solid electrolyte is selected from one or more of a NASICON solid electrolyte, a garnet solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a perovskite solid electrolyte and an antiperovskite solid electrolyte.
[0018] Furthermore, the NASICON type solid electrolyte includes Li 1+x Al x Ti 2-X (PO 4)3 (LATP), the garnet-type solid electrolyte includes Li7La3Zr2O 12 (LLZO).
[0019] Furthermore, in step (3), the stirring time is 1 to 24 hours.
[0020] Furthermore, in step (3), unreacted titanate coupling agent is removed by centrifugal drying.
[0021] Furthermore, in step (3), the centrifugal speed is 1000-10000 rpm, the drying temperature is 60-200° C., and the drying time is 1-24 h.
[0022] Further, in step (4), the ionic liquid is selected from 1-methylimidazole bis(trifluoromethanesulfonyl imide), 1-ethylimidazole bis(trifluoromethanesulfonyl imide), 1-propylimidazole bis(trifluoromethanesulfonyl imide), 1-butylimidazole bis(trifluoromethanesulfonyl imide), 1-pentylimidazole bis(trifluoromethanesulfonyl imide), 1-hexylimidazole bis(trifluoromethanesulfonyl imide), 1-octylimidazole bis(trifluoromethanesulfonyl imide), 1-decylimidazole bis(trifluoromethanesulfonyl imide), 1-dodecylimidazole bis(trifluoromethanesulfonyl imide), 1-tetradecylimidazole bis(trifluoromethanesulfonyl imide), 1-hexadecylimidazole bis(trifluoromethanesulfonyl imide), imide salts, 1-octadecyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-methyl-3-imidazole bis trifluoromethanesulfonyl imide salts, 1-ethyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-propyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-butyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-pentyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-hexyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-octyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-decyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salts, 1-benzyl-3-methyl 1-methyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-dodecyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-tetradecyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-hexadecyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-octadecyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-methyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-ethyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-propyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-butyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1- 2,3-pentyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-hexyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-octyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-decyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-benzyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-dodecyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-tetradecyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-hexadecyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-octadecyl imidazolium bis trifluoromethanesulfonyl imide salt,3-Dimethylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-ethylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-propylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-butylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-benzylimidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl Propyl-3-ethyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-propyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-butyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-hexyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-octylimidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-2,3-dimethyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-vinyl imidazole bis trifluoromethanesulfonyl imide salt Imidium salts, 1-ethylpyridine bis trifluoromethanesulfonyl imide salts, 1-propylpyridine bis trifluoromethanesulfonyl imide salts, 1-butylpyridine bis trifluoromethanesulfonyl imide salts, 1-hexylpyridine bis trifluoromethanesulfonyl imide salts, 1-octylpyridine bis trifluoromethanesulfonyl imide salts, 1-ethyl-4-methylpyridine bis trifluoromethanesulfonyl imide salts, 1-propyl-4-methylpyridine bis trifluoromethanesulfonyl imide salts, 1-butyl-4-methylpyridine bis trifluoromethanesulfonyl imide salts, 1-hexylpyridine bis trifluoromethanesulfonyl imide salts One or more of 1-methyl-4-pyridine bis-trifluoromethanesulfonyl imide salt, 1-octyl-4-methylpyridine bis-trifluoromethanesulfonyl imide salt, 1-ethyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, 1-propyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, 1-butyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, 1-hexyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, and 1-octyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt. ,
[0023] Furthermore, the mass ratio of the titanate coupling agent in step (2) to the ionic liquid in step (4) is (1-10):1.
[0024] Furthermore, the temperature is controlled in step (2) to ensure complete hydrolysis of the titanate coupling agent; the temperature is controlled in step (3) to ensure that the titanate coupling agent is fully grafted onto the surface of the inorganic solid electrolyte; and the temperature is controlled in step (4) to ensure complete surface modification of the ionic liquid.
[0025] Furthermore, in step (4), the stirring time is 1 to 24 hours.
[0026] The second aspect of the present invention provides a surface bifunctional modified inorganic solid electrolyte prepared by the method described in the first aspect.
[0027] The third aspect of the present invention provides a composite solid electrolyte, which is prepared from the surface dual-functional modified inorganic solid electrolyte described in the second aspect, a polymer matrix and a lithium salt.
[0028] Specifically, the surface dual-functional modified inorganic solid electrolyte, polymer matrix and lithium salt are mixed, an organic solvent is added and stirred evenly, and then poured on a flat mold surface, and the composite solid electrolyte is obtained after removing the organic solvent.
[0029] The present invention adopts the solution casting method to prepare the composite solid electrolyte, which has a simple process flow, low cost and is conducive to large-scale production.
[0030] Furthermore, the polymer matrix is one of polyethylene oxide (PEO), polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polymethyl methacrylate, polycaprolactone, polyvinyl alcohol, and polyvinyl pyrrolidone.
[0031] Furthermore, the lithium salt is one of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(difluoromethanesulfonylimide), and lithium bis(trifluoromethanesulfonylimide).
[0032] Furthermore, the mass percentage of the surface bifunctional modified inorganic solid electrolyte to the polymer matrix is 10% to 50%, and the mass ratio of the polymer matrix to the lithium salt is (2 to 10):1.
[0033] Furthermore, the organic solvent is selected from one or more of anhydrous acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone (NMP), acetone, tetrahydrofuran, dimethyl sulfoxide, chloroform, carbon tetrachloride and toluene.
[0034] Furthermore, the material of the mold is one of glass, polyethylene terephthalate, and polytetrafluoroethylene.
[0035] The fourth aspect of the present invention provides an application of the composite solid electrolyte described in the third aspect in the preparation of a solid-state battery, wherein the solid-state battery includes an all-solid-state lithium metal battery.
[0036] Beneficial effects of the present invention:
[0037] 1. The surface modification of the inorganic solid electrolyte by the titanate coupling agent in the present invention reduces the surface energy of the inorganic solid electrolyte, promotes the dispersion of the inorganic solid electrolyte, and optimizes the organic-inorganic interface compatibility between the inorganic solid electrolyte and the polymer matrix. At the same time, the introduced ionic liquid broadens the migration channel of lithium ions at the interface, promotes the rapid migration of lithium ions at the organic-inorganic interface, and improves the ionic conductivity.
[0038] 2. The present invention adopts the solution casting method to prepare the composite solid electrolyte, which has a simple process flow, low cost and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a cycle performance diagram of the button-type all-solid-state lithium metal battery prepared by the composite solid electrolyte of Application Example 1 and Comparative Examples 1-2.
[0040] Figure 2 This is a cycle performance diagram of the button-type all-solid-state lithium metal battery prepared using the button-type all-solid-state lithium metal battery of Application Example 2 and the composite solid electrolyte of Comparative Examples 1 to 2.
[0041] Figure 3 It is a cycle performance diagram of the button-type all-solid-state lithium metal battery prepared by the button-type all-solid-state lithium metal battery of Application Example 3 and the composite solid electrolyte of Comparative Examples 1 to 2. DETAILED DESCRIPTION
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0043] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0044] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0045] Example 1
[0046] A composite solid electrolyte is prepared by the following method:
[0047] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0048] The preparation method of the surface bifunctional modified LATP comprises the following steps:
[0049] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0050] (2) adding 0.5 g of isopropyl dioleyl (dioctyl phosphate) titanate to the acidic organic solution, stirring at 30° C. for 4 h to obtain a mixed solution;
[0051] (3) adding 1 g of LATP to the mixed solution, stirring at 60° C. for 12 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 80° C. for 12 h to obtain an intermediate product;
[0052] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.25 g of 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 80° C. for 12 h, centrifuged, washed, and dried at 80° C. for 12 h to obtain the surface bifunctional modified LATP.
[0053] Example 2
[0054] A composite solid electrolyte is prepared by the following method:
[0055] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0056] The preparation method of the surface bifunctional modified LATP comprises the following steps:
[0057] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0058] (2) adding 0.5 g of isopropyl tri(dioctylphosphoyl) titanate to the acidic organic solution, stirring at 30° C. for 4 h to obtain a mixed solution;
[0059] (3) adding 1 g of LATP to the mixed solution, stirring at 60° C. for 12 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 80° C. for 12 h to obtain an intermediate product;
[0060] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.25 g of 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 80° C. for 12 h, centrifuged, washed, and dried at 80° C. for 12 h to obtain the surface bifunctional modified LATP.
[0061] Example 3
[0062] A composite solid electrolyte is prepared by the following method:
[0063] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0064] The preparation method of the surface bifunctional modified LATP comprises the following steps:
[0065] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0066] (2) adding 0.5 g of isopropyl tri(dioctyl pyrophosphate) titanate to the acidic organic solution, stirring at 30° C. for 4 h to obtain a mixed solution;
[0067] (3) adding 1 g of LATP to the mixed solution, stirring at 60° C. for 12 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 80° C. for 12 h to obtain an intermediate product;
[0068] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.25 g of 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 80° C. for 12 h, centrifuged, washed, and dried at 80° C. for 12 h to obtain the surface bifunctional modified LATP.
[0069] Example 4
[0070] A composite solid electrolyte is prepared by the following method:
[0071] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified Li6PS5Cl were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60 °C in vacuum for 24 h to obtain a composite solid electrolyte.
[0072] Among them, the preparation method of surface bifunctional modified Li6PS5Cl includes the following steps:
[0073] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0074] (2) adding 1 g of isopropyl tri(dodecylbenzenesulfonyl) titanate to the acidic organic solution and stirring at 25° C. for 6 h to obtain a mixed solution;
[0075] (3) Add 1 g of Li6PS5Cl to the mixed solution, stir at 70°C for 18 h to obtain a suspension, centrifuge at 8000 rpm, wash, and dry at 60°C for 24 h to obtain an intermediate product;
[0076] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.5 g of 1-methyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 60° C. for 16 h, centrifuged, washed, and dried at 60° C. for 24 h to obtain surface bifunctional modified Li6PS5Cl.
[0077] Example 5
[0078] A composite solid electrolyte is prepared by the following method:
[0079] 1g PEO, 0.4077g lithium bis(trifluoromethanesulfonyl)imide and 0.1g surface bifunctional modified Li3InCl6 were dissolved in 10g anhydrous acetonitrile and stirred continuously at room temperature for 24h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried in vacuum at 60°C for 24h to obtain a composite solid electrolyte.
[0080] The preparation method of surface bifunctional modified Li3InCl6 comprises the following steps:
[0081] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0082] (2) adding 1 g of isopropyl tri(dodecylbenzenesulfonyl) titanate to the acidic organic solution and stirring at 25° C. for 6 h to obtain a mixed solution;
[0083] (3) Add 1 g of Li3InCl6 to the mixed solution, stir at 70°C for 18 h to obtain a suspension, centrifuge at 8000 rpm, wash, and dry at 60°C for 24 h to obtain an intermediate product;
[0084] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.5 g of 1-methyl-2,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 60°C for 16 h, centrifuged, washed, and dried at 60°C for 24 h to obtain surface bifunctional modified Li3InCl6.
[0085] Example 6
[0086] A composite solid electrolyte is prepared by the following method:
[0087] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LLZO were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0088] The preparation method of the surface dual-functional modified LLZO comprises the following steps:
[0089] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0090] (2) adding 1 g of isopropyl tri(dodecylbenzenesulfonyl) titanate to the acidic organic solution and stirring at 25° C. for 6 h to obtain a mixed solution;
[0091] (3) adding 1 g of LLZO to the mixed solution, stirring at 70°C for 18 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 60°C for 24 h to obtain an intermediate product;
[0092] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.5 g of 1-methyl-2,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 60° C. for 16 h, centrifuged, washed, and dried at 60° C. for 24 h to obtain a surface bifunctional modified LLZO.
[0093] Example 7
[0094] A composite solid electrolyte is prepared by the following method:
[0095] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0096] The preparation method of the surface bifunctional modified LATP comprises the following steps:
[0097] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0098] (2) adding 1 g of bis(dioctyloxypyrophosphate)ethylene titanate to the acidic organic solution, stirring at 40° C. for 3 h to obtain a mixed solution;
[0099] (3) adding 1 g of LATP to the mixed solution, stirring at 50° C. for 20 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 60° C. for 24 h to obtain an intermediate product;
[0100] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.6 g of 1-ethylpyridine bistrifluoromethanesulfonyl imide salt was slowly added, stirred at 50° C. for 20 h, centrifuged, washed, and dried at 60° C. for 24 h to obtain the surface bifunctional modified LATP.
[0101] Example 8
[0102] A composite solid electrolyte is prepared by the following method:
[0103] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0104] The preparation method of the surface bifunctional modified LATP comprises the following steps:
[0105] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0106] (2) adding 1 g of bis(dioctyloxypyrophosphate)ethylene titanate to the acidic organic solution, stirring at 40° C. for 3 h to obtain a mixed solution;
[0107] (3) adding 1 g of LATP to the mixed solution, stirring at 50° C. for 20 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 60° C. for 24 h to obtain an intermediate product;
[0108] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.6 g of 1-ethyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 50° C. for 20 h, centrifuged, washed, and dried at 60° C. for 24 h to obtain the surface bifunctional modified LATP.
[0109] Example 9
[0110] A composite solid electrolyte is prepared by the following method:
[0111] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g surface bifunctional modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred continuously at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60°C in vacuum for 24 h to obtain a composite solid electrolyte.
[0112] The preparation method of the surface bifunctional modified LATP comprises the following steps:
[0113] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0114] (2) adding 1 g of bis(dioctyloxypyrophosphate)ethylene titanate to the acidic organic solution, stirring at 40° C. for 3 h to obtain a mixed solution;
[0115] (3) adding 1 g of LATP to the mixed solution, stirring at 50° C. for 20 h to obtain a suspension, centrifuging at 8000 rpm, washing, and drying at 60° C. for 24 h to obtain an intermediate product;
[0116] (4) The intermediate product was added to anhydrous ethanol and stirred continuously to form a stable suspension, and 0.6 g of 1-octyl-4-methylpyridine bis(trifluoromethanesulfonyl)imide salt was slowly added, stirred at 50° C. for 20 h, centrifuged, washed, and dried at 60° C. for 24 h to obtain the surface bifunctional modified LATP.
[0117] Comparative Example 1
[0118] A composite solid electrolyte is prepared by the following method:
[0119] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g LATP were dissolved in 10 g anhydrous acetonitrile and stirred at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60° C. in a vacuum oven for 24 h to obtain a composite solid electrolyte.
[0120] Comparative Example 2
[0121] A composite solid electrolyte is prepared by the following method:
[0122] 1 g PEO, 0.4077 g lithium bis(trifluoromethanesulfonyl)imide and 0.1 g modified LATP were dissolved in 10 g anhydrous acetonitrile and stirred at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate and dried at 60° C. in a vacuum oven for 24 h to obtain a composite solid electrolyte.
[0123] The preparation method of modified LATP comprises the following steps:
[0124] (1) Mix 50 mL of anhydrous ethanol and 5 mL of deionized water, add glacial acetic acid to adjust the pH value to 4-6, and continue stirring to obtain an acidic organic solution;
[0125] (2) adding 0.5 g of isopropyl dioleyl (dioctyl phosphate) titanate to the acidic organic solution, stirring at 30° C. for 4 h to obtain a mixed solution;
[0126] (3) 1 g of LATP was added to the mixed solution, and the mixture was stirred at 60° C. for 12 h to obtain a suspension. The suspension was centrifuged at 8000 rpm, washed, and dried at 80° C. for 12 h to obtain the modified LATP.
[0127] Comparative Example 3
[0128] A composite solid electrolyte is prepared by the following method:
[0129] (1) LATP was added to anhydrous ethanol and stirred continuously to form a stable suspension, 0.25 g of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt was slowly added, and the mixture was stirred at 80° C. for 12 h. The mixture was centrifuged, washed, and dried at 80° C. for 12 h to obtain the product.
[0130] (2) 1 g of PEO, 0.4077 g of lithium bis(trifluoromethanesulfonyl)imide and 0.1 g of the above product were dissolved in 10 g of anhydrous acetonitrile, and the mixture was stirred at room temperature for 24 h to obtain a composite slurry. The composite slurry was evenly poured on a smooth glass plate, and vacuum dried at 60° C. for 24 h to obtain a composite solid electrolyte.
[0131] After the composite solid electrolyte in Comparative Example 3 was centrifugally dried, it was found that there was no ionic liquid in the composite electrolyte, that is, in the absence of a titanate coupling agent, the ionic liquid could not be combined with the surface of the solid electrolyte LATP alone.
[0132] Test Case
[0133] The composite solid electrolytes of Examples 1 to 9 and Comparative Examples 1 to 2 are used to prepare button-type all-solid-state lithium metal batteries (Examples 1 to 9 correspond to Application Examples 1 to 9). The preparation method is: in a glove box filled with high-purity argon, the button-type all-solid-state lithium metal battery is assembled in the order of positive electrode shell-positive electrode sheet-composite solid electrolyte membrane-lithium sheet-gasket-spring-negative electrode shell.
[0134] Among them, the composite solid electrolyte membrane is prepared by punching a composite polymer electrolyte into discs; the preparation method of the positive electrode sheet is: lithium iron phosphate (LFP), carbon black (Super P) and polyvinylidene fluoride (PVDF) are uniformly mixed in NMP at a mass ratio of 8:1:1 to obtain a slurry, the slurry is uniformly coated on an aluminum foil, and placed in a vacuum drying oven at 80°C for drying for 24 hours to obtain a positive electrode sheet.
[0135] The electrochemical performance tests (cycle stability and capacity retention rate) of the button-type all-solid-state lithium metal batteries prepared by the button-type all-solid-state lithium metal batteries of the test application examples 1 to 9 and the composite solid electrolytes of the comparative examples 1 to 3 were conducted.
[0136] The test method is: using the LAND CT2001A battery test system, at 60°C, the button-type all-solid-state lithium metal battery is charged and discharged at a rate of 0.2C, with a voltage range of 2.9 to 3.8V.
[0137] Test results such as Figure 1 to Figure 3 As shown in Table 1:
[0138] Table 1
[0139]
[0140]
[0141] Figure 1 The cycle performance diagram of the button-type all-solid-state lithium metal battery prepared by the button-type all-solid-state lithium metal battery of Application Example 1 and the composite solid electrolyte of Comparative Examples 1-2; Figure 2 The cycle performance diagram of the button-type all-solid-state lithium metal battery prepared by the composite solid electrolyte of Application Example 2 and Comparative Examples 1-2; Figure 3 It is a cycle performance diagram of the button-type all-solid-state lithium metal battery prepared by the button-type all-solid-state lithium metal battery of Application Example 3 and the composite solid electrolyte of Comparative Examples 1 to 2.
[0142] from Figure 1 to Figure 3 As can be seen from Table 1, the initial discharge specific capacity of the button-type all-solid-state lithium metal batteries of Application Examples 1 to 9 is between 165.6 and 169.2 mAh·g -1 , the discharge capacity after 100 cycles is between 156.5 and 160.5 mAh g -1 The average coulombic efficiency is between 99.61% and 99.82%. The initial discharge capacity of the button-type all-solid-state lithium metal battery prepared by the composite solid electrolyte of Comparative Example 1 is only 139.3 mAh·g -1 , and the discharge capacity decays to ~0 after 60 cycles of unstable cycling. Although the initial capacity of comparative example 2 is increased to 154.8 mAh g -1 However, after 100 cycles, the capacity decayed to 118.3 mAh g -1, the capacity retention rate is only 76.42%. The initial discharge specific capacity and capacity retention rate of Comparative Examples 1 to 2 are lower than those of Application Examples 1 to 9, indicating that the use of titanate coupling agent as a surface modifier optimizes the compatibility of the organic-inorganic interface. At the same time, the introduced ionic liquid broadens the migration channel of lithium ions, promotes the rapid migration of lithium ions at the organic-inorganic interface, and improves the cycle stability of the all-solid-state lithium metal battery. In addition, since titanate coupling agent is not used in Comparative Example 3, the ionic liquid cannot be well retained on the surface of the inorganic solid electrolyte during the preparation process, and its application effect is similar to that of Comparative Example 1.
[0143] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a surface dual-functional modified inorganic solid electrolyte, characterized in that: The following steps are involved: (1) adjusting the pH value of the aqueous solution of the organic solvent to 4 to 6 to obtain an acidic organic solution; (2) adding a titanate coupling agent to the acidic organic solution obtained in step (1), and stirring at 20 to 50° C. to obtain a mixed solution; (3) adding an inorganic solid electrolyte to the mixed solution obtained in step (2), stirring at 40 to 80° C. to obtain a suspension, centrifuging and drying to obtain an intermediate product; (4) dissolving the intermediate product obtained in step (3) and the ionic liquid in an organic solvent, stirring at 40 to 90° C., centrifuging and drying to obtain a surface bifunctional modified inorganic solid electrolyte.
2. The preparation method according to claim 1, characterized in that: In step (1), an acidic regulator is used to adjust the pH value of the aqueous solution of the organic solvent, wherein the acidic regulator is selected from one or more of formic acid, glacial acetic acid and acetic acid, and the organic solvent is selected from one or more of methanol, anhydrous ethanol, isopropanol and acetone.
3. The preparation method according to claim 1, characterized in that: In step (2), the titanate coupling agent is selected from one or more of isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl tri (dioctyl phosphate) titanate, isopropyl trioleyl titanate, isopropyl tri (dioctyl pyrophosphate) titanate, isopropyl tri (isostearoyl) titanate, isopropyl tri (dodecylbenzenesulfonyl) titanate, isopropyl triisostearyl titanate, bis (dioctyl pyrophosphate) ethylene titanate, trihydroxy acyl titanate isopropyl, di (dioctyl pyrophosphate) ethylene glycol titanate, dihydroxy acyl ethylene diethylene titanate, bistriethanolamine diisopropyl titanate and tetraisopropyl di (dioctyl phosphite) titanate.
4. The preparation method according to claim 1 or 3, characterized in that: The mass ratio of the titanate coupling agent in step (2) to the inorganic solid electrolyte in step (3) is (0.2-2):
1.
5. The preparation method according to claim 1, characterized in that: In step (3), the inorganic solid electrolyte is selected from one or more of a NASICON solid electrolyte, a LISICON solid electrolyte, a LiPON solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a perovskite solid electrolyte and an antiperovskite solid electrolyte.
6. The preparation method according to claim 1, characterized in that: In step (4), the ionic liquid is selected from 1-methylimidazole bis trifluoromethanesulfonyl imide salt, 1-ethylimidazole bis trifluoromethanesulfonyl imide salt, 1-propylimidazole bis trifluoromethanesulfonyl imide salt, 1-butylimidazole bis trifluoromethanesulfonyl imide salt, 1-pentylimidazole bis trifluoromethanesulfonyl imide salt, 1-hexylimidazole bis trifluoromethanesulfonyl imide salt, 1-octylimidazole bis trifluoromethanesulfonyl imide salt, 1-decylimidazole bis trifluoromethanesulfonyl imide salt, 1-dodecylimidazole bis trifluoromethanesulfonyl imide salt, 1-tetradecylimidazole bis trifluoromethanesulfonyl imide salt, 1-hexadecylimidazole bis trifluoromethanesulfonyl imide salt , 1-octadecyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-methyl-3-imidazole bis trifluoromethanesulfonyl imide salt, 1-ethyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-propyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-butyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-pentyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-hexyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-octyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-decyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt, 1-benzyl-3-methyl imidazolium bis trifluoromethanesulfonyl imide salt 1-methyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-ethyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-propyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-butyl-2,3-dimethylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-pentyl ... bis(trifluoromethanesulfonyl)imide salt of 1-hexyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-octyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-decyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-benzyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-dodecyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-tetradecyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-hexadecyl-2,3-dimethylimidazolium, bis(trifluoromethanesulfonyl)imide salt of 1-octadecyl-2,3-Dimethylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-ethylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-propylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-butylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl-3-benzylimidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-methylimidazole bis trifluoromethanesulfonyl imide salt, 1-vinyl Propyl-3-ethyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-propyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-butyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-hexyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-octylimidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-2,3-dimethyl imidazole bis trifluoromethanesulfonyl imide salt, 1-allyl-3-vinyl imidazole bis trifluoromethanesulfonyl imide salt Imidium salts, 1-ethylpyridine bis trifluoromethanesulfonyl imide salts, 1-propylpyridine bis trifluoromethanesulfonyl imide salts, 1-butylpyridine bis trifluoromethanesulfonyl imide salts, 1-hexylpyridine bis trifluoromethanesulfonyl imide salts, 1-octylpyridine bis trifluoromethanesulfonyl imide salts, 1-ethyl-4-methylpyridine bis trifluoromethanesulfonyl imide salts, 1-propyl-4-methylpyridine bis trifluoromethanesulfonyl imide salts, 1-butyl-4-methylpyridine bis trifluoromethanesulfonyl imide salts, 1-hexylpyridine bis trifluoromethanesulfonyl imide salts One or more of 1-methyl-4-pyridine bis-trifluoromethanesulfonyl imide salt, 1-octyl-4-methylpyridine bis-trifluoromethanesulfonyl imide salt, 1-ethyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, 1-propyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, 1-butyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, 1-hexyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt, and 1-octyl-1-methylpiperidine bis-trifluoromethanesulfonyl imide salt. , 7. The preparation method according to claim 1 or 6, characterized in that: The mass ratio of the titanate coupling agent in step (2) to the ionic liquid in step (4) is (1-10):
1.
8. A surface bifunctional modified inorganic solid electrolyte prepared by the method according to any one of claims 1 to 7.
9. A composite solid electrolyte, characterized in that: The invention is prepared from the surface dual-functional modified inorganic solid electrolyte as claimed in claim 8, a polymer matrix and a lithium salt.
10. Use of the composite solid electrolyte according to claim 9 in preparing a solid-state battery.