Fluorocarbon electrolyte additive, preparation method thereof, infiltrating type electrolyte and lithium ion battery

Through the synergistic effect of the fluorocarbon chain, carbonate/carboxylate and functional groups of the fluorocarbon electrolyte additive, the difficulty in wetting and safety issues of lithium-ion battery cells is solved, the wetting characteristics and electrochemical performance of the battery are improved, and the High energy density and improved safety.

CN118738560APending Publication Date: 2024-10-01LIONGO (CHANGZHOU) NEW ENERGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411070915.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

After increasing the compaction density of the positive and negative electrode materials of lithium-ion batteries, the cell infiltration is difficult and the liquid absorption consistency is poor, resulting in extended production cycles, performance deterioration and safety issues, especially the lithium precipitation in the negative electrode, which causes safety hazards.

Method used

Using fluorocarbon electrolyte additives, through the synergistic effect of fluorocarbon chains, carbonate/carboxylate groups and functional groups, the surface tension of the cell is reduced, the wetting characteristics are improved, and a tough film is formed on the electrode surface to protect the electrode sheet. , improve electrochemical performance.

Benefits of technology

Significantly improves the infiltration characteristics and cycle performance of lithium-ion batteries, reduces side reactions, enhances the stability and high ion conductivity of the electrode sheets, and matches the highly compacted positive electrode sheets to improve the energy density and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981663630000011
    Figure BDA0004981663630000011
  • Figure BDA0004981663630000022
    Figure BDA0004981663630000022
  • Figure BDA0004981663630000031
    Figure BDA0004981663630000031
Patent Text Reader

Abstract

The invention provides a fluorocarbon electrolyte additive, a preparation method thereof, an infiltrating electrolyte and a lithium ion battery. The fluorocarbon electrolyte additive has a structure as shown in a formula I, the additive comprises three characteristic groups, one is a fluorocarbon chain, the second is an electrolyte-philic carbonic ester and carboxylic ester group (R1), and the third is a functional group (R2). The synergistic effect of the three groups can obviously reduce the surface tension of the battery cell and improve the infiltration characteristic of the battery cell, so that a high-compaction positive pole piece can be matched, and a necessary condition is provided for obtaining a high-energy-density lithium ion battery. The fluorocarbon chain can form a film rich in fluorine on the surface of the battery cell, and the film is tough and high in strength, can inhibit harmful reaction between an electrode plate and an electrolyte in the circulation process, has relatively high ionic conductivity, does not hinder conduction of lithium ions, and remarkably improves the first effect and the circulation performance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a fluorocarbon electrolyte additive, a preparation method thereof, an immersion-type electrolyte and a lithium ion battery. Background Art

[0002] With the increasing popularity of electronic products such as electric vehicles and portable devices, the demand for high-energy-density lithium-ion batteries is becoming more and more urgent. This type of battery has broad application prospects in the fields of energy storage, aerospace, etc. How to improve the energy density of lithium batteries has become the focus of scholars' research.

[0003] The use of positive and negative electrode materials with higher compaction density can maximize the space utilization of the battery. However, as the compaction density of the positive and negative electrode materials increases, the problem of difficulty in cell wetting arises. The use of conventional electrolytes will make it difficult for the electrodes to absorb liquid and increase the wetting aging time, thereby lengthening the battery production cycle and reducing production efficiency. Poor consistency in electrode absorption will lead to deterioration of the performance of the problem battery cell and even cause safety problems due to lithium plating at the negative electrode. Summary of the invention

[0004] The object of the present invention is to provide a fluorocarbon electrolyte additive, a preparation method thereof, an infiltration-type electrolyte and a lithium-ion battery. The fluorocarbon electrolyte additive of the present invention improves the wettability while improving the cycle performance of the battery cell, avoiding the problem of high impedance of general surfactants.

[0005] The present invention provides a fluorocarbon electrolyte additive having a structure shown in Formula I:

[0006]

[0007] In formula I, 5≤n1≤10, 1≤n2≤3, R1 is R2 is an electron withdrawing group.

[0008] Preferably, R2 is sulfonic acid, cyano, nitro, amino, ethylene oxide, trifluoromethyl, trifluoroethyl, maleimide, vinyl or ethynyl.

[0009] The present invention provides a method for preparing the fluorocarbon electrolyte additive as described above, comprising the following steps:

[0010] In the presence of a protective atmosphere and a catalyst, reacting the compound represented by formula II, the compound represented by formula III and phosgene, or mixing the compound represented by formula IV and the compound represented by formula III to react, to obtain the compound represented by formula I;

[0011]

[0012] Preferably, the catalyst is pyridine and its derivatives.

[0013] Preferably, the reaction temperature is -5 to 0°C; and the reaction time is 4 to 8 hours.

[0014] The present invention provides an immersion-type electrolyte, comprising a lithium salt, an organic solvent and an additive;

[0015] The additive is the fluorocarbon electrolyte additive described above or the fluorocarbon electrolyte additive prepared by the preparation method described above.

[0016] Preferably, the organic solvent includes one or more of carbonate solvents, carboxylate solvents, amine solvents, sulfone solvents and nitrile solvents.

[0017] Preferably, the lithium salt is one or more of lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoromethylsulfonate, lithium difluorooxalatoborate and lithium bis(oxalatoborate);

[0018] The concentration of the lithium salt in the immersion electrolyte is 0.5-2 mol / L.

[0019] Preferably, the mass concentration of the additive in the immersion electrolyte is 0.005-0.5%.

[0020] The present invention provides a lithium ion battery, comprising the above-mentioned immersion electrolyte.

[0021] The present invention provides a fluorocarbon electrolyte additive having a structure shown in Formula I. The additive in the present invention comprises three characteristic groups, one of which is a fluorocarbon bond. The high bond energy and low polarity of the fluorocarbon bond (FC) result in a weak interaction force between the fluorocarbon functional groups, making it easier to directional aggregate and arrange into a molecular membrane at the liquid / gas interface, and compared with other groups, the surfactant molecules containing fluorocarbon bonds have a stronger hydrophobic effect; the second is a carbonate and carboxylate group (R1) of a pro-electrolyte, which acts together with a fluorocarbon chain to form a hydrophilic-hydrophobic structure to achieve the effect of improving the wetting; the third functional group (R2) can further improve the electrochemical performance of the battery cell according to the electrolyte system. The synergistic effect of the three groups can significantly reduce the surface tension of the battery cell, improve the wetting characteristics of the battery cell, and then match the high-density positive electrode sheet, which provides a necessary condition for obtaining a lithium-ion battery with a high energy density. The fluorocarbon chain in the present invention can form a fluorine-rich film on the surface of the battery cell. The film is tough and has high strength. It can inhibit harmful reactions between the electrode sheet and the electrolyte during the cycle. At the same time, it has a high ion conductivity and will not hinder the conduction of lithium ions, thereby significantly improving the initial efficiency and cycle performance of the battery cell.

[0022] In the present invention, the non-aqueous electrolyte containing a small amount of the additive of the present invention can significantly improve the wetting characteristics of the battery cell, and at the same time can form a tough film on the electrode surface to protect the electrode sheet and reduce side reactions. DETAILED DESCRIPTION

[0023] The present invention provides a fluorocarbon electrolyte additive having a structure shown in Formula I:

[0024]

[0025] In formula I, 5≤n1≤10, 1≤n2≤3, R1 is R2 is an electron withdrawing group.

[0026] In the present invention, 5≤n1≤10, preferably, 6≤n1≤9, such as n1 is 5, 6, 7, 8, 9, 10, preferably a range value with any of the above values ​​as the upper or lower limit. When n1 is less than 5, the fluorocarbon chain is too short to exert the hydrophobic properties of the fluorocarbon group, and the improvement of the surface tension is limited; when n1 is greater than 10, the fluorocarbon chain is too long to make the preparation process difficult.

[0027] In the present invention, 1≤n2≤3, such as n2 is 1, 2 or 3, preferably a range value with any of the above values ​​as the upper or lower limit. When n2 is greater than 3, the longer carbon chain will cause the electron-withdrawing properties of the R2 group to fail to act on the carboxylate group or carbonate group (R1), making it difficult to optimize the electron cloud distribution of the R1 group, and unable to further enhance the additive's ability to improve wetting.

[0028] In the present invention, R1 is preferably a carboxylate (-OCO-) or a carbonate (-CH2OCOO-), R1 is a hydrophilic group in the fluorocarbon wetting improvement additive, and forms a hydrophilic-hydrophobic surfactant molecular structure with the hydrophobic fluorocarbon chain. At the same time, the carboxylate and carbonate groups of the R1 group are similar to the electrolyte solvent groups, which can improve the solubility of the fluorocarbon wetting additive.

[0029] In the present invention, the R2 group is preferably a functional group with electron-withdrawing ability, and R2 is preferably a sulfonic acid group, a cyano group, a nitro group, an amino group, an ethylene oxide group, a trifluoromethyl group, a trifluoroethyl group, a maleimide group, a vinyl group or an ethynyl group. The R2 group in the present invention can optimize the electron cloud distribution of the R1 group, increase the hydrophilicity without affecting the hydrophobicity of the fluorocarbon chain, and further increase the improvement of the surface tension of the additive; at the same time, it can give the wetting improver a more excellent film-forming stability.

[0030] The present invention also provides a method for preparing a fluorocarbon electrolyte additive, comprising the following steps:

[0031] In the presence of a protective atmosphere and a catalyst, reacting the compound represented by formula II, the compound represented by formula III and phosgene, or mixing the compound represented by formula IV and the compound represented by formula III to react, to obtain the compound represented by formula I;

[0032]

[0033] In the present invention, due to the different types of R1 groups, the raw materials used in the preparation of the structural compound shown in formula I are also different. When R1 is a carbonate, the raw materials for preparation are the compound shown in formula II, the compound shown in formula III and phosgene. When R1 is a carboxylate, the raw materials for preparation are the compound shown in formula IV and the compound shown in formula III.

[0034] Specifically, when R1 is a carbonate, the preparation process is as shown in Formula 1:

[0035] Under the conditions of a protective atmosphere and a catalyst, reacting the compound represented by formula II, the compound represented by formula III and phosgene to obtain the compound represented by formula I;

[0036]

[0037] In the present invention, the compound represented by formula II and the acyl chloride are preferably mixed and reacted for 2 to 4 hours in a protective atmosphere and in the presence of a catalyst, and then the compound represented by formula III is added and the reaction is continued for 2 to 4 hours to obtain the compound represented by formula I.

[0038] In the present invention, n1, n2, R1 and R2 in Formula II and Formula III are consistent with n1, n2, R1 and R2 described above, and the present invention will not be repeated here.

[0039] In the present invention, the usage ratio of the compound represented by Formula II, the compound represented by Formula III and the acyl chloride is 1:1:1 according to the theoretical molar ratio of Formula 1. According to the characteristics of the reaction, such as errors in the operating process, to ensure the complete reaction of a certain reactant or to increase the reaction rate, etc., those skilled in the art can make adaptive adjustments based on the theoretical molar ratio. This is achievable by those skilled in the art, and the present invention is not particularly limited herein.

[0040] In the present invention, the protective atmosphere is preferably nitrogen and / or argon, and the catalyst is preferably pyridine and its derivatives, such as one or more of pyridine, 4-methylpyridine, 4-ethylpyridine and 2,5-lutidine.

[0041] In the present invention, the reaction temperature is preferably -5 to 0°C, more preferably -4 to -1°C, such as -5°C, -4°C, -3°C, -2°C, -1°C, preferably a range value with any of the above values ​​as the upper or lower limit; the reaction time is preferably 4 to 8 hours, more preferably 5 to 6 hours.

[0042] When R1 is carboxylate, the preparation process is shown in Formula 2:

[0043] In the presence of a protective atmosphere and a catalyst, the compound represented by formula IV and the compound represented by formula III are mixed and reacted to obtain a compound represented by formula I;

[0044]

[0045] In the present invention, n1, n2, R1 and R2 in Formula IV and Formula III are consistent with n1, n2, R1 and R2 described above, and the present invention will not be repeated here.

[0046] In the present invention, the usage ratio of the compound represented by Formula IV and the compound represented by Formula III is 1:1 according to the theoretical molar ratio of Formula 2. According to the characteristics of the reaction, such as errors in the operating process, to ensure the complete reaction of a certain reactant or to increase the reaction rate, etc., those skilled in the art can make adaptive adjustments based on the theoretical molar ratio. This is achievable by those skilled in the art, and the present invention is not particularly limited here.

[0047] In the present invention, the protective atmosphere is preferably nitrogen and / or argon, and the catalyst is preferably pyridine and its derivatives, such as one or more of pyridine, 4-methylpyridine, 4-ethylpyridine and 2,6-lutidine.

[0048] In the present invention, the reaction temperature is preferably -5 to 0°C, more preferably -4 to -1°C, such as -5°C, -4°C, -3°C, -2°C, -1°C, preferably a range value with any of the above values ​​as the upper or lower limit; the reaction time is preferably 4 to 8 hours, more preferably 5 to 6 hours.

[0049] The present invention also provides an immersion-type electrolyte, comprising a lithium salt, an organic solvent and the fluorocarbon electrolyte additive described above.

[0050] In the present invention, the mass concentration of the fluorocarbon electrolyte additive in the immersion electrolyte is preferably 0.005-0.5%, more preferably 0.01-0.45%, such as 0.005%, 0.01%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, preferably a range value with any of the above values ​​as the upper or lower limit.

[0051] In the present invention, the lithium salt is preferably one or more of lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoromethylsulfonate, lithium difluorooxalatoborate and lithium bis(oxalatoborate); the concentration of the lithium salt in the wetting electrolyte is preferably 0.5 to 2 mol / L, more preferably 1 to 1.5 mol / L.

[0052] In the present invention, the organic solvent is preferably one or more of a carbonate solvent, a carboxylate solvent, an amine solvent, a sulfone solvent and a nitrile solvent.

[0053] The carbonate solvent preferably includes one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, methyl propyl carbonate, butylene carbonate, methyl butyl carbonate and dibutyl carbonate.

[0054] The carboxylate solvent preferably includes one or more of methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate and methyl propionate.

[0055] The amine solvent preferably includes one or more of N-methylacetamide, N-methylformamide, dimethylformamide and diethylformamide.

[0056] The sulfone solvents preferably include dimethyl sulfide, dimethyl sulfoxide, cyclopentane, diphenyl sulfoxide, thionyl chloride, dipropyl sulfone, dimethyl sulfite, diethyl sulfite, and tetramethyl sulfoxide; the nitrile solvents mainly include one or more of acetonitrile, succinonitrile, adiponitrile, 3-methoxypropionitrile, 3-ethoxypropionitrile, and 1,3,6-hexanetrinitrile.

[0057] The fluorocarbon electrolyte additive in the present invention can significantly reduce the infiltration time of the electrolyte and has a certain improvement effect on the electrochemical performance of the battery cell.

[0058] The present invention also provides a lithium ion battery, comprising the above-mentioned immersion electrolyte.

[0059] In the present invention, the positive electrode in the lithium-ion battery includes a positive electrode current collector and a positive electrode material layer arranged on the surface of the positive electrode current collector. The material of the positive electrode current collector can be selected from aluminum, titanium or stainless steel. The positive electrode material layer includes a positive electrode active material, a conductive agent and a binder. The positive electrode active material can be lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP), medium-high nickel ternary materials and their composite positive electrode materials. The conductive agent can be a carbon material, such as one or more of carbon black, conductive polymers, acetylene black, carbon fiber, carbon nanotubes and graphite. The binder can be one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride, carboxymethyl cellulose (CMC), polytetrafluoroethylene (PTFE), fluorine-based rubber, ethylene propylene diene monomer rubber and styrene butadiene rubber (SBR).

[0060] In the present invention, the negative electrode in the lithium-ion battery preferably includes a negative electrode current collector and a negative electrode material layer on the surface of the negative electrode current collector. The material of the negative electrode current collector can be selected from copper, nickel or stainless steel. The negative electrode material layer includes a negative electrode active material, a conductive agent and a binder. The negative electrode active material can be metallic lithium, a lithium-embedded carbon material or a lithium alloy. The conductive agent can be a carbon material, such as one or more of carbon black, conductive polymers, acetylene black, carbon fibers, carbon nanotubes and graphite. The binder can be one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride, carboxymethyl cellulose (CMC), polytetrafluoroethylene (PTFE), fluorine-based rubber, ethylene propylene diene monomer rubber and styrene butadiene rubber (SBR).

[0061] In the present invention, the isolation membrane can be polypropylene (PP), polyethylene (PE), a composite material of polypropylene (PP), polyethylene (PE), glass fiber felt, or a composite membrane formed by welding or bonding with a wettable polyolefin microporous membrane.

[0062] The present invention provides a fluorocarbon electrolyte additive having a structure shown in Formula I. The additive in the present invention comprises three characteristic groups, one of which is a fluorocarbon chain. The high bond energy and low polarity of the fluorocarbon bond (FC) result in a weak interaction force between the fluorocarbon chains. The fluorocarbon surfactant molecules have a stronger hydrophobicity than other surfactant molecules in aqueous solution, and are more likely to be oriented and aggregated into molecular membranes at the liquid / gas interface, which is beneficial to improving the wetting characteristics; the second is a carbonate and carboxylate group (R1) of a pro-electrolyte, which works together with the fluorocarbon chain to form a hydrophilic-hydrophobic structure to achieve the effect of improving the wetting; the third functional group (R2) can further improve the electrochemical performance of the battery cell according to the electrolyte system. The synergistic effect of the three groups can significantly reduce the surface tension of the battery cell, improve the wetting characteristics of the battery cell, and then match the high-density positive electrode sheet, which provides a necessary condition for obtaining a lithium-ion battery with a high energy density. The fluorocarbon chain in the present invention can form a fluorine-rich film on the surface of the battery cell. The film is tough and has high strength. It can inhibit harmful reactions between the electrode sheet and the electrolyte during the cycle. At the same time, it has a high ion conductivity and will not hinder the conduction of lithium ions, thereby significantly improving the initial efficiency and cycle performance of the battery cell.

[0063] In the present invention, the non-aqueous electrolyte containing a small amount of the additive of the present invention can significantly improve the wetting characteristics of the battery cell, and at the same time can form a tough film on the electrode surface to protect the electrode sheet and reduce side reactions.

[0064] In order to further illustrate the present invention, a fluorocarbon electrolyte additive, a preparation method thereof, an immersion-type electrolyte and a lithium-ion battery provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0065] Example 1

[0066] 0.1 mol of 1H,1H-perfluoro-1-nonanol was added to 1 mol of pyridine, and the round-bottom flask containing the above substances was placed in an ice-water bath. Phosgene was introduced under stirring. After reacting for 4 hours, 0.1 mol of 3-hydroxypropanesulfonic acid was added to the above system. The reaction was continued for 4 hours under the same conditions. The mixture was added with sodium bicarbonate aqueous solution for washing and drying, and extracted by flash column chromatography to obtain compound A. GC-MS (m / z): calcd. for C 13 H9F 17 O6S[M+1] + , 615.98, found 616.24.

[0067]

[0068] In a glove box, 30wt% EC, 30.99wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.01wt% of compound A was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0069] Example 2

[0070] Take 0.1 mol of perfluoro-1-nonanoyl chloride into 1 mol of pyridine, put the round-bottom flask containing the above substances into an ice-water bath, add 0.1 mol of 3-hydroxypropanesulfonic acid into the above system under stirring, react for 4 hours, add sodium bicarbonate aqueous solution to the mixture for washing and drying, and extract it by flash column chromatography to obtain compound B, GC-MS (m / z): calcd.for C 12 H7F 17 O6S[M+1] + , 585.97, found 586.22.

[0071]

[0072] In a glove box, 30wt% EC, 30.99wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.01wt% of compound B was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0073] Embodiment 3:

[0074] Take 0.1 mol of 1H,1H-perfluoro-1-hexanol and add it to 1 mol of 4-methylpyridine. Put the round-bottom flask containing the above substances into an ice-water bath, and introduce phosgene under stirring. After reacting for 4 hours, add 0.1 mol of ethanolamine to the above system, and keep the same conditions to continue the reaction for 4 hours. Add sodium bicarbonate aqueous solution to the mixture for washing and drying, and use flash column chromatography to extract it to obtain compound C. GC-MS (m / z): calcd. for C9H8F 11 NO3[M+1] + , 387.15, found 387.03.

[0075]

[0076] In a glove box, 30wt% EC, 30.995wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.005wt% of compound C was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0077] Example 4

[0078] Take 0.1 mol of perfluoro-1-nonanoyl chloride into 1 mol of 4-ethylpyridine, put the round-bottom flask containing the above substances into an ice-water bath, add 0.1 mol of 2,2,2-trifluoroethanol into the above system under stirring, react for 8 hours, add sodium bicarbonate aqueous solution to the mixture for washing and drying, and extract it by flash column chromatography to obtain compound D, GC-MS (m / z): calcd.for C 11 H2F 20 O2[M+1] + , 546.10, found 545.97.

[0079]

[0080] In a glove box, 30wt% EC, 30.9wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.1wt% of compound D was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0081] Embodiment 5:

[0082] 0.1 mol of 1H,1H-perfluoro-1-nonanol was added to 1 mol of 2,6-dimethylpyridine, and the round-bottom flask containing the above substances was placed in an ice-water bath. Phosgene was introduced under stirring. After reacting for 4 hours, 0.1 mol of 4-butene-1-ol was added to the above system. The reaction was continued for 8 hours under the same conditions. The mixture was added with sodium bicarbonate aqueous solution for washing and drying, and extracted by flash column chromatography to obtain compound E. GC-MS (m / z): calcd. for C 14 H9F 17 O3[M+1] + , 548.03, found 548.20.

[0083]

[0084] In a glove box, 30wt% EC, 30.98wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.02wt% of compound E was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0085] Example 6

[0086] 0.1 mol of 1H,1H-perfluoro-1-nonanol was added to 1 mol of pyridine, and the round-bottom flask containing the above substances was placed in an ice-water bath. Phosgene was introduced under stirring. After reacting for 4 hours, 0.1 mol of 4-butyn-1-ol was added to the above system. The reaction was continued for 7 hours under the same conditions. The mixture was washed and dried with sodium bicarbonate aqueous solution, and extracted using flash column chromatography to obtain compound F. GC-MS (m / z): calcd. for C 14 H7F 17 O3[M+1] + , 546.02, found 546.18.

[0087]

[0088] In a glove box, 30wt% EC, 30.8wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.2wt% of compound F was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0089] Example 7

[0090] Take 0.1 mol of 1H,1H-perfluoro-1-nonanol and add it to 1 mol of pyridine. Put the round-bottom flask containing the above substances into an ice-water bath, and introduce phosgene under stirring. After reacting for 4 hours, add 0.1 mol of cyanomethyl alcohol to the above system, and keep the same conditions to continue the reaction for 4 hours. Add sodium bicarbonate aqueous solution to the mixture for washing and drying, and extract it by flash column chromatography to obtain compound G. GC-MS (m / z): calcd.for C 12 H4F 17 NO3[M+1] + ,532.99,found533.17.

[0091]

[0092] In a glove box, 30wt% EC, 30.9wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.05wt% of compound G and 0.05wt% of compound B were added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0093] Example 8

[0094] 0.1 mol of 1H,1H-perfluoro-1-undecanol was added to 1 mol of pyridine, and the round-bottom flask containing the above substances was placed in an ice-water bath. Phosgene was introduced under stirring. After reacting for 5 hours, 0.1 mol of 2-(ethylene oxide)ethanol was added to the above system. The reaction was continued for 7 hours under the same conditions. The mixture was added with sodium bicarbonate aqueous solution for washing and drying, and extracted by flash column chromatography to obtain compound H. GC-MS (m / z): calcd. for C 16 H9F 21 O4[M+1] + , 664.02, found 664.21.

[0095]

[0096] In a glove box, 30wt% EC, 30.85wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.05wt% of compound H and 0.01wt% of compound A were added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0097] Comparative Example 1

[0098] In a glove box, 30wt% EC, 30wt% DMC, and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; 1wt% fluorobenzene was further added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte. The obtained electrolyte was subjected to a wetting test.

[0099] Comparative Example 2

[0100] In a glove box, 30wt% EC, 31wt% DMC, and 26wt% EMC were mixed evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; the obtained mixed solution was used as an electrolyte.

[0101] Comparative Example 3

[0102] 0.1 mol of 1H,1H-perfluoro-1-nonanol was added to 1 mol of pyridine, and the round-bottom flask containing the above substances was placed in an ice-water bath. Phosgene was introduced under stirring. After reacting for 4 hours, 0.1 mol of propanol was added to the above system. The reaction was continued for 4 hours under the same conditions. The mixture was added with sodium bicarbonate aqueous solution for washing and drying, and extracted by flash column chromatography to obtain compound I. GC-MS (m / z): calcd. for C 13 H9F 17 O3[M+1] + ,536.03,found536.18.

[0103]

[0104] In a glove box, 30wt% EC, 30.99wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.01wt% of compound I was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0105] Comparative Example 4

[0106] In a glove box, 30wt% EC, 30.99wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.01wt% perfluorononane was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0107] Comparative Example 5

[0108] In a glove box, 30wt% EC, 30.99wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; 0.01wt% hydroxypropanesulfonic acid was further added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0109] Comparative Example 6

[0110] 0.1 mol of perfluoro-1-nonanoyl chloride was added to 1 mol of pyridine, and the round-bottom flask containing the above substances was placed in an ice-water bath. 0.1 mol of 3-hydroxypentanesulfonic acid was added to the above system under stirring. After reacting for 4 hours, the mixture was added with sodium bicarbonate aqueous solution for washing and drying. The compound J was extracted by flash column chromatography. GC-MS (m / z): calcd.for C 14 H 11 F17 O5S[M+1] + , 614.01, found 614.36.

[0111]

[0112] In a glove box, 30wt% EC, 30.99wt% DMC and 26wt% EMC were stirred evenly to form a mixed solution; 13wt% LiPF6 was added to the mixed solution and stirred to fully dissolve to obtain a mixed salt solution; further 0.01wt% of compound J was added to the mixed salt solution, and the obtained mixed solution was used as an electrolyte.

[0113] Application Examples

[0114] Take 95.5wt% LiFePO4, 2wt% PVDF and 2.5wt% conductive carbon black, mix and disperse them evenly in NN dimethyl pyrrolidone to make a slurry, evenly coat it on aluminum foil, and roll it (surface density is 2.6g / cm 3 ) cutting the sheet to obtain the positive electrode sheet;

[0115] 96.3w% artificial graphite, 1.7w% CMC, 1w% SBR and 1wt% conductive carbon black were mixed and dispersed evenly in pure water to form a slurry, which was evenly coated on the copper foil and rolled (surface density was 1.6g / cm 3 ) cut into pieces to obtain the negative electrode sheet.

[0116] A 2032 button cell was assembled in the order of negative electrode shell - negative electrode sheet - polypropylene separator - positive electrode sheet - gasket - spring sheet - positive electrode shell, and then the electrolytes in Examples 1 to 8 and Comparative Examples 1 to 6 were injected.

[0117] The button battery cycle test is 0.2C constant current and constant voltage to 3.75V, and 0.2C constant current discharge to 2.5V.

[0118] The wetting balance method was used to test the amount of washing liquid per unit area of ​​the positive electrode within a certain period of time to characterize the improvement effect of electrolyte additives on the wetting of the LFP positive electrode.

[0119] The above test results are shown in Table 1.

[0120] Table 1 Battery performance test results in the embodiments and comparative examples

[0121]

[0122] It can be found from Examples 1-8 and Comparative Examples 1 and 2 that a small amount of wetting additives can achieve a wetting improvement effect that is better than that of 1% fluorobenzene, which is far better than the commonly used measures in the market, indicating that the structure described in this article can significantly reduce the surface tension of the electrolyte and is an excellent wetting improvement additive; at the same time, due to the improvement effect of the fluorocarbon chain and the functional group, the first effect, cycle stability and rate performance of the battery cell are improved to a certain extent; while improving the wetting ability of the electrolyte, the electrochemical performance of the battery cell is improved.

[0123] By comparing Examples 1-8 with Comparative Examples 2 and 3, it can be found that a single fluorocarbon compound has little improvement on the battery cell, and the introduction of functional groups can further improve the wetting ability and electrochemical performance of the fluorocarbon compound.

[0124] By comparing Examples 1-8 with Comparative Example 4 and Example 5, it can be found that a single fluorocarbon chain and a functional group cannot effectively improve the wetting properties and electrochemical properties of the electrolyte, which further confirms that the fluorocarbon wetting additives mentioned in this article achieve the improvement of the wetting effect and the electrochemical performance through the synergistic effect of fluorocarbon chains, carboxylates / carbonates, and functional groups.

[0125] By comparing Example 2 with Comparative Example 6, it can be found that when the carbon chain of n2 is longer, the functional group will not further optimize the wetting properties of the fluorocarbon compound.

[0126] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A fluorocarbon electrolyte additive having a structure shown in Formula I: In formula I, 5≤n1≤10, 1≤n2≤3, R1 is R2 is an electron withdrawing group.

2. The fluorocarbon electrolyte additive according to claim 1, characterized in that: The R2 is sulfonic acid, cyano, nitro, amino, ethylene oxide, trifluoromethyl, trifluoroethyl, maleimide, vinyl or ethynyl.

3. A method for preparing the fluorocarbon electrolyte additive as claimed in claim 1, comprising the following steps: In the presence of a protective atmosphere and a catalyst, reacting the compound represented by formula II, the compound represented by formula III and phosgene, or mixing the compound represented by formula IV and the compound represented by formula III to react, to obtain the compound represented by formula I; 4. The preparation method according to claim 3, characterized in that: The catalyst is pyridine and its derivatives.

5. The preparation method according to claim 3, characterized in that: The protective atmosphere is argon; the reaction temperature is -5 to 0°C; and the reaction time is 4 to 8 hours.

6. An immersion electrolyte comprising a lithium salt, an organic solvent and an additive; The additive is the fluorocarbon electrolyte additive according to claim 1 or 2 or the fluorocarbon electrolyte additive prepared by the preparation method according to any one of claims 3 to 5.

7. The immersion electrolyte according to claim 6, characterized in that: The organic solvent includes one or more of carbonate solvents, carboxylate solvents, amine solvents, sulfone solvents and nitrile solvents.

8. The immersion electrolyte according to claim 6, characterized in that: The lithium salt is one or more of lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoromethylsulfonate, lithium difluorooxalatoborate and lithium bis(oxalatoborate); The concentration of the lithium salt in the immersion electrolyte is 0.5-2 mol / L.

9. The immersion electrolyte according to claim 6, characterized in that: The mass concentration of the additive in the immersion electrolyte is 0.005-0.5%.

10. A lithium ion battery, characterized in that: The invention comprises the immersion-type electrolyte as described in any one of claims 6 to 9.

Citation Information

Cited By

  • Functionally modified high-nickel positive electrode composite material and method for preparing the same

    CN119812283B